A method for batch preparation of transmission electron microscope grid array

The transmission electron microscope grid array is constructed by sputtering metal thin film deposition and photolithography plating technology, which solves the efficiency and quality problems of batch preparation of graphene grids in the existing technology, and achieves high-quality, uniform and regular grid arrays. Array preparation is suitable for the preparation of graphene and ordinary electron microscope grids.

CN118064856BActive Publication Date: 2024-10-25PEKING UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410168665.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2024-10-25
Estimated Expiration
2044-02-06

AI Technical Summary

Technical Problem

It is difficult to realize the batch preparation of high-quality graphene transmission electron microscope grids with existing technology, especially due to the poor anisotropy of the growth substrate caused by the wet etching process and the low efficiency and high cost caused by the reliance on imported grids.

Method used

A metal film substrate is deposited by sputtering, photolithography is used to construct a periodic photoresist soft template array, and a transmission electron microscope grid grid array is constructed through electroplating, and then the template is removed to obtain a uniform and regular transmission electron microscope grid grid. array.

Benefits of technology

It achieves the batch preparation of high-quality transmission electron microscope grids, improves the yield rate, is suitable for the characterization of different sample types, and meets the mass production needs of graphene transmission electron microscope grids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064856B_ABST
    Figure CN118064856B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for batch preparation of transmission electron microscope grid arrays, belonging to the field of materials. The method of the present invention comprises the following steps: after sputtering a layer of metal film substrate on the surface of a hard substrate, using photolithography to construct a periodic photoresist soft template array as a mask, then constructing a transmission electron microscope grid grid array structure by electroplating, and finally removing the periodic photoresist soft template array and the metal film substrate to obtain the transmission electron microscope grid array. The method of the present invention solves the technical problem of batch preparation of transmission electron microscope grids in China. The method is simple and easy to implement, and has universal applicability. The prepared transmission electron microscope grid structure has excellent quality and can be directly used for the preparation of ordinary electron microscope grids and graphene electron microscope grids that meet the requirements of transmission electron microscope sample preparation. The latter can be used for single particle structure analysis of cryo-electron microscopy and high-resolution imaging of nanoparticles and single atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of materials, and in particular to a method for batch preparing a transmission electron microscope grid array. Background Art

[0002] Graphene is an ideal transmission electron microscope grid material. During the electron microscope characterization process, graphene with a single layer of carbon atoms will hardly bring background interference. Its excellent mechanical and electrical properties can effectively realize sample loading and significantly reduce the sample displacement caused by high-energy electron beam irradiation, making it possible to characterize the sample with high resolution. Therefore, graphene transmission electron microscope grids have good application prospects in the fields of support membranes and so on.

[0003] In order to realize the widespread application of graphene transmission electron microscope grids, the preparation method of high-quality graphene transmission electron microscope grids is indispensable. At present, the process route of preparing graphene transmission electron microscope grids by directly etching the growth substrate (patent number ZL201811381142.1) can effectively avoid graphene damage caused by transfer; the use of isopropyl alcohol-assisted glue-free transfer method can realize the clean transfer of foil graphene (patent number CN201611019356.5) and wafer graphene (patent number CN202110333466.3), and realize the preparation of high-quality, ultra-clean graphene transmission electron microscope support film. However, these preparation processes are difficult to achieve in the batch preparation of high-quality graphene transmission electron microscope grids: the former uses a wet etching process, and the anisotropy of the etching of the graphene growth substrate is poor, making it difficult to achieve high-yield batch preparation of graphene transmission electron microscope grids; the latter is heavily dependent on imported grids, and requires manpower to operate each grid one by one, which is time-consuming and labor-intensive, and does not meet the requirements of batch production of graphene transmission electron microscope grids. Therefore, in order to truly achieve the batch preparation of high-quality graphene transmission electron microscope grids, it is crucial to achieve batch preparation of transmission electron microscope grid arrays.

[0004] In addition, the preparation technology of high-quality TEM grids is not mature in China, and most commercial TEM grids are still imported. And when using commercial TEM grids on the market to prepare graphene TEM grids, it is necessary to operate the scattered grids one by one, which is not conducive to the realization of batch preparation of graphene TEM grids. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for batch preparation of transmission electron microscope grid arrays. The method of the present invention effectively realizes the batch preparation of high-quality transmission electron microscope grid arrays with uniform and regular grids.

[0006] The present invention first provides a method for preparing a transmission electron microscope grid array, comprising the following steps:

[0007] (1) Using a sputtering method, a metal film substrate is deposited on the surface of a hard substrate as an electroplating conductive layer and a separation sacrificial layer;

[0008] (2) constructing a periodic photoresist soft template array on the surface of the metal film substrate of the hard substrate by using a photolithography method;

[0009] (3) using the periodic photoresist soft template array as a mask, and constructing a transmission electron microscope grid grid array structure on the surface of the metal film substrate exposed outside the pattern by electroplating;

[0010] (4) removing the periodic photoresist soft template array and the metal film substrate, peeling off the grid grid structure from the surface of the hard substrate, and obtaining the transmission electron microscope grid array.

[0011] In the above-mentioned preparation method, in step (1), the hard substrate may be an industrial substrate such as quartz, sapphire, silicon wafer or mica;

[0012] The size of the hard substrate is 1 to 12 inches, and specifically may be 4 inches.

[0013] In the above-mentioned preparation method, in step (1), the metal film substrate is a non-inert metal substrate, specifically a copper or nickel substrate;

[0014] The sputtering parameters are: the sputtering temperature is room temperature (generally 15-35° C.), the sputtering power is 50-200 W, the sputtering time is 480 s-960 s, the sputtering atmosphere is Ar, and the sputtering pressure is 0.01-1 Pa;

[0015] The thickness of the obtained metal film substrate is 50-200 nm, specifically 100 nm.

[0016] In the above-mentioned preparation method, in step (2), the periodic photoresist soft template array is a square periodic pattern;

[0017] The steps of the photolithography are as follows:

[0018] (a) spin coating a negative photoresist on the surface of the metal film substrate at a spin coating rate of 2000 to 6000 r / min;

[0019] (b) baking the negative photoresist at 80 to 120° C. for 2 to 5 minutes;

[0020] (c) exposing the plate to a UV lithography machine for 4 to 10 seconds to copy the grid pattern on the lithography plate onto the negative photoresist on the surface of the metal film substrate;

[0021] (d) baking the patterned negative photoresist at 80 to 120° C. for 2 to 5 minutes;

[0022] (e) After soaking in a developer for 5 to 15 minutes, washing in a fixer for 30 to 120 seconds to obtain a periodic pattern on the negative photoresist.

[0023] In the above-mentioned preparation method, the square periodic pattern is micrometer-level, and the side length of the square can be 30 to 420 μm, specifically 80 μm;

[0024] The period of the square periodic pattern is 40 to 500 μm, and may be specifically 100 μm;

[0025] The size of the square periodic pattern array is 3 mm, preferably circular, to meet the grid size requirements of a transmission electron microscope.

[0026] In the above-mentioned preparation method, in step (3), the material of the transmission electron microscope grid grid array structure is a metal commonly used for electroplating, such as gold, copper or nickel;

[0027] The electroplating parameters are: average current density is 0.5A / dm 2 ~2A / dm 2 , the temperature is 20℃~30℃, and the electroplating time is 20min~50min.

[0028] In the above-mentioned preparation method, in step (4), the reagent for removing the periodic photoresist soft template array can be at least one of N-methyl-2-pyrrolidone, nitrogen ethyl pyrrolidone and acetone; the reagent for removing the metal film substrate can be selected from one or more of hydrochloric acid, ammonium persulfate solution or ferric chloride solution according to the type of metal.

[0029] In the above-mentioned preparation method, in step (4), the grid structure is peeled off from the surface of the hard substrate with the aid of tweezers.

[0030] In the above-mentioned preparation method, in step (4), optionally, the process of peeling the grid grid structure from the surface of the hard substrate can be achieved with the aid of a thermal release tape.

[0031] In the above-mentioned preparation method, in step (4), optionally, after the transmission electron microscope grid array structure is separated from the hard substrate, it is immersed in a passivation solution of the corresponding metal, and the immersion time can be 2 to 5 minutes.

[0032] In the above-mentioned preparation method, in step (3), optionally, after the electroplating process is completed, the obtained transmission electron microscope grid grid array structure is immersed in a passivation solution of the corresponding metal, and the immersion time can be 2 to 5 minutes.

[0033] The present invention also provides a transmission electron microscope grid array prepared by the above preparation method.

[0034] In the above-mentioned transmission electron microscope grid array, the height of the transmission electron microscope grid array is 5-15 μm, and specifically can be 8 μm.

[0035] The application of the above-mentioned transmission electron microscope grid array in the preparation of transmission electron microscope grids also falls within the protection scope of the present invention.

[0036] The present invention has the following advantages:

[0037] (1) The process of the present invention is simple, wherein the hard substrate can be reused and only needs to be ultrasonically cleaned before use; the material and shape structure of the grid can be adjusted according to the sample type, and is suitable for transmission electron microscopy characterization of different samples;

[0038] (2) The electron microscope grid obtained by the present invention has a high yield rate, the grid area and spacing in the grid are controllable, and large-scale wafer-level preparation and large-scale batch preparation can be achieved;

[0039] (4) The transmission electron microscope grid structure prepared by the present invention can be directly used for the preparation of ordinary electron microscope grids and graphene electron microscope grids that meet the requirements of transmission electron microscope sample preparation. The latter can be used for single particle structure analysis of cryo-electron microscopy and high-resolution imaging of nanoparticles and single atoms.

[0040] (3) The transmission electron microscope grid prepared by the present invention meets commercial standards and can realize batch preparation of transmission electron microscope grids. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a schematic flow diagram of the preparation process of the present invention;

[0042] Figure 2 A photo of a photolithography mask used in Example 1 and a schematic diagram of a single grid structure;

[0043] Figure 3 Optical characterization of the periodic photoresist soft template array prepared in Example 1; Figure 3 A is a real picture of a 4-inch periodic photoresist soft template array; B is a low-resolution optical microscope image; C is a high-resolution optical microscope image;

[0044] Figure 4 is a scanning electron microscope image of the periodic photoresist soft template array prepared in Example 1; Figure 4A is a low-resolution scanning electron microscope image of the periodic photoresist soft template array when the tilt angle is 0°; B is a high-resolution scanning electron microscope image of the periodic photoresist soft template array when the tilt angle is 0°; C is a low-resolution scanning electron microscope image of the periodic photoresist soft template array when the tilt angle is 45°; D is a high-resolution scanning electron microscope image of the periodic photoresist soft template array when the tilt angle is 45°;

[0045] Figure 5 This is a physical photograph of the transmission electron microscope grid array prepared in Example 1; Figure 5 A is a photo of the object before peeling off from the hard substrate surface; B is a photo of the object after peeling off from the hard substrate surface;

[0046] Figure 6 is a scanning electron microscope image of the transmission electron microscope grid array prepared in Example 1; Figure 6 A is a low-resolution scanning electron microscope image when the tilt angle of the transmission electron microscope grid array is 0°; B is a high-resolution scanning electron microscope image when the tilt angle of the transmission electron microscope grid array is 0°; C is a low-resolution scanning electron microscope image when the tilt angle of the transmission electron microscope grid array is 45°; D is a high-resolution scanning electron microscope image when the tilt angle of the transmission electron microscope grid array is 45°. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.

[0048] The experimental methods in the following examples are all conventional methods unless otherwise specified.

[0049] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0050] In the following embodiments, the photoresist pattern layer is produced by a UV exposure machine, the exposure wavelength is 365nm, and the exposure time is 4 to 10 seconds; the negative photoresist model is AR-N 4400-25; the developer model is AR 300-56, and the developer formula is (AR300-46): water = 5:1 (volume ratio); the fixing solution is pure water.

[0051] In the following embodiments, the electroplating solution is a bright acid copper electroplating solution (Beichen Hardware Technology Co., Ltd., item number BC-121), and the electroplating anode is a phosphor copper plate.

[0052] In the following examples, the copper film removing solution is a 0.5 mol / L ammonium persulfate aqueous solution.

[0053] The fabricated transmission electron microscope grid arrays were characterized, including the photoresist soft template arrays obtained by photolithography and the transmission electron microscope grid arrays obtained by electroplating. The measurement methods are as follows:

[0054] Use a Nikon upright metallographic microscope, model LV100ND, or a scanning electron microscope (Tachi S-4800). Optical microscopy or scanning electron microscopy can clearly characterize the structure and morphology of the photoresist soft template array and the transmission electron microscope grid array.

[0055] Example 1: Batch preparation of copper transmission electron microscope grid arrays

[0056] The specific implementation process is as follows:

[0057] (1) Preparation of metal film substrate: A layer of copper film was sputtered on the surface of a quartz wafer (4 inches) using a magnetron sputtering apparatus. The sputtering temperature was room temperature, the sputtering power was 150 W, the sputtering time was 720 s, the sputtering atmosphere was Ar, and the sputtering pressure was 0.68 Pa to obtain a copper film with a thickness of 100 nm.

[0058] (2) Preparation of periodic photoresist soft template array: Using photolithography, a periodic pattern similar to the transmission grid is produced on the surface of the copper film on the surface of the quartz wafer.

[0059] The specific method is:

[0060] (a) Spin-coat positive photoresist AR-N 4400-25 on the back of the copper foil substrate at a spin-coating rate of 3000 r / min;

[0061] (b) baking the photoresist at 90°C for 2 min;

[0062] (c) Covering the photoresist surface with a photomask, and exposing it in a UV lithography machine (manufacturer: Institute of Optoelectronics Technology, Chinese Academy of Sciences, model URE-2000 / 35) for 5 s;

[0063] (d) baking the exposed sample (photoresist / copper film / quartz wafer) at 100°C for 2 min;

[0064] (e) The baked sample was immersed in a developer for 7 minutes, then immersed in a fixer for 40 seconds, and dried with nitrogen.

[0065] (3) Preparation of transmission electron microscope grid array structure: Add 500 mL of bright acid copper electroplating solution to the electroplating tank, connect the sample obtained in (2) to the negative electrode of the electroplating electrode as the electroplating cathode; connect the phosphor copper plate to the positive electrode of the electroplating electrode as the electroplating anode. The average current density is 1.2 A / dm 2, temperature is 25℃, and electroplating time is 40min.

[0066] (4) Separation of transmission electron microscope grid array: Soak the sample obtained in (3) in N-methyl-2-pyrrolidone liquid for 5 minutes, then take it out and wash it with deionized water. Then soak the above sample in 0.5 mol / L ammonium persulfate aqueous solution for 3 minutes, then take it out and wash it with deionized water. After the sample is dried, use tweezers to gently lift the copper plating on the edge of the above sample, and the transmission electron microscope grid array can be completely separated from the hard substrate surface.

[0067] Figure 1 It is a schematic diagram of the process of the preparation process of the present invention, which can be specifically divided into six steps: sputtering metal film, spin coating photoresist, photolithography / development, electroplating, debonding / cleaning, and etching / separation.

[0068] Figure 2 The actual photo of the photolithography mask used in this embodiment and the schematic diagram of a single grid structure, wherein the single grid structure is a circle with a diameter of 3 mm, the side length of the grid pattern in the single grid structure is 80 μm, and the period of the grid pattern is 100 μm.

[0069] Figure 3 This is an optical photograph of the periodic photoresist soft template array prepared in this embodiment. The dark semicircular ring area and the square area in the figure are the parts where the photoresist soft template exists. It can be seen that the edges of the photoresist soft template array are clear and neat, and the copper film substrate not covered by the photoresist is completely exposed. In the photoresist soft template array, the side length of the square is 80μm, and the period of the square pattern is 100μm.

[0070] Figure 4 This is a scanning electron microscope image of the periodic photoresist soft template array prepared in this embodiment. To ensure the imaging quality of the periodic photoresist soft template array sample, the sample was gold-sprayed with a thickness of about 10 nm. To further reflect the thickness of the periodic photoresist soft template array, the sample was tilted with an angle of 45°. It can be seen that the surface of the photoresist soft template array is flat and the height is consistent, about 10 μm.

[0071] Figure 5 This is a photo of the transmission electron microscope grid array prepared in this example.

[0072] Figure 6 The scanning electron microscope image of the transmission electron microscope grid array prepared in this embodiment shows that the structure surface of the grid array is flat, the grains are fine, and the grid height is about 8 μm.

Claims

1. A method for preparing a transmission electron microscope grid array, comprising the following steps: (1) Using the sputtering method, a metal film substrate is deposited on the surface of a hard substrate as an electroplating conductive layer and a separation sacrificial layer; The sputtering parameters are as follows: the sputtering temperature is room temperature, the sputtering power is 50-200 W, the sputtering time is 480 s-960 s, the sputtering atmosphere is Ar, and the sputtering pressure is 0.01-1 Pa; (2) constructing a periodic photoresist soft template array on the surface of the metal film substrate of the hard substrate by using a photolithography method; The steps of the photolithography are as follows: (a) spin coating a negative photoresist on the surface of the metal film substrate at a spin coating rate of 2000-6000 r / min; (b) baking the negative photoresist at 80 to 120° C. for 2 to 5 min; (c) exposing the plate to a UV lithography machine for 4 to 10 seconds to copy the grid pattern on the lithography plate onto the negative photoresist on the surface of the metal film substrate; (d) baking the patterned negative photoresist at 80-120° C. for 2-5 min; (e) after soaking in a developer for 5 to 15 minutes, washing in a fixer for 30 to 120 seconds to obtain a periodic pattern on the negative photoresist; (3) Using the periodic photoresist soft template array as a mask, constructing a transmission electron microscope grid grid array structure on the surface of the metal film substrate exposed outside the pattern by electroplating; The parameters of the electroplating are: average current density of 0.5 A / dm 2 ~2 A / dm 2 , the temperature is 20℃~30℃, and the electroplating time is 20 min~50 min; (4) Removing the periodic photoresist soft template array and the metal film substrate, peeling off the grid grid structure from the surface of the hard substrate, and obtaining the transmission electron microscope grid array.

2. The preparation method according to claim 1, Features: In step (1), the hard substrate is quartz, sapphire, silicon wafer or mica; The hard substrate has a size of 1 to 12 inches.

3. The preparation method according to claim 1 or 2, Features: In step (1), the metal film substrate is a non-inert metal substrate; The obtained metal film substrate has a thickness of 50-200 nm.

4. The preparation method according to claim 3, Features: In step (1), the metal film substrate is a copper or nickel substrate.

5. The preparation method according to claim 1 or 2, Features: In step (2), the periodic photoresist soft template array is a square periodic pattern.

6. The preparation method according to claim 5, Features: The square periodic pattern is at the micrometer level, and the square side length is 30-420 μm; The period of the square periodic pattern is 40-500 μm.

7. The preparation method according to claim 1 or 2, Features: In step (3), the material of the transmission electron microscope grid array structure is gold, copper or nickel.

8. The preparation method according to claim 1 or 2, Features: In step (4), the reagent for removing the periodic photoresist soft template array is at least one of N-methyl-2-pyrrolidone, nitrogen ethyl pyrrolidone and acetone; The reagent for removing the metal film substrate is selected from hydrochloric acid, ammonium persulfate solution or ferric chloride solution according to the type of metal; In step (4), the grid structure is peeled off from the surface of the hard substrate with the aid of tweezers or thermal release tape.

9. A transmission electron microscope grid array prepared by the preparation method according to any one of claims 1 to 8.

10. The transmission electron microscope grid array according to claim 9, Features: The height of the transmission electron microscope grid array is 5-15 μm.

11. Use of the transmission electron microscope grid array according to claim 9 or 10 in the preparation of transmission electron microscope grids.

Citation Information

Cited By

  • Preparation method and application of hexagonal boron nitride / graphene suspended composite support membrane with strength and toughness