Method for preparing high-temperature and high-viscosity metal film using metal film as substrate

By preparing a high-viscosity slurry on the metal film and performing microwave roller coating and ultraviolet irradiation treatment, the problem of reduced peeling force of functional metal film materials under high temperature conditions was solved, high peeling force and cohesion were achieved, and thermal conductivity and thermal conductivity were improved. Shielding properties for high temperature applications.

CN118085682BActive Publication Date: 2024-10-18HANPIN (KUNSHAN) ELECTRONIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410323828.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2024-10-18
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

The peeling force of existing functional metal film materials drops significantly under high temperature conditions, and the cohesive force and peeling force show opposite behavior, which cannot meet the bonding needs of high-temperature applications.

Method used

Using a metal film as the base material, a high-viscosity slurry is prepared and subjected to microwave roller coating and ultraviolet irradiation treatment to form a high-temperature and high-viscosity metal film, improve its peeling force and cohesion, and enhance thermal conductivity and shielding properties.

Benefits of technology

Achieving high peeling force and high cohesion, the normal temperature peeling force can reach more than 4000gf/inch, the high temperature peeling force can reach more than 2000gf/inch, the cohesive retention force can meet the high temperature of 85 degrees/1000g>24H, and the overall thermal conductivity is>100W/mk. The shielding efficiency is >80dB at 10M~5GHz, the Vickers hardness is as high as 100HV, and the elastic modulus is as high as 50,000MPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118085682B_ABST
    Figure CN118085682B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-temperature and high-viscosity metal film with a metal film as a substrate, comprising the following steps: S1. preparing a high-viscosity slurry; S2. coating the high-viscosity slurry with a microwave roller; S3. ultraviolet light irradiation treatment; the method for preparing a high-temperature and high-viscosity metal film provided by the invention uses a metal film as a substrate, and single-sidedly coats the formulated slurry to achieve high peeling force and high cohesion; the thickness is 10U-200U, and the peeling force is based on the 50U finished product thickness index as an example. The normal temperature peeling force can reach more than 4000gf / inch, and the high temperature peeling force can reach more than 2000gf / inch, and the cohesion retention force can meet the high temperature of 85 degrees / 1000g>24H. It has a good heat dissipation effect, and the overall thermal conductivity is greater than 100W / mk; it has excellent shielding effectiveness, and the shielding effectiveness is greater than 80dB at 10M-5GHz, and it has excellent supporting performance, and the substrate has high stiffness, and its Vickers hardness is as high as 100HV, and its elastic modulus is as high as 50000MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional metal film materials, and in particular to a method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate. Background Art

[0002] Functional metal film materials are new materials developed on the basis of traditional pressure-sensitive tape products. They are new material products developed from traditional pressure-sensitive tape products (i.e. traditional adhesive products). Traditional adhesive products mainly provide single purposes such as packaging, sealing, protection, labeling, splicing, etc., while functional metal film tape materials can achieve multiple functions such as protection, adhesion, buffering, conductivity, insulation, shielding, support, heat conduction and heat dissipation, and light transmission on the same material by developing adhesives with different functions, different coating materials, and specific formulas combined with a variety of substrates. They have important uses in electronics, communications, new energy, precision machinery, intelligent instruments and other industries.

[0003] With the advancement of science and technology, the application of bonding effects is constantly improving, from the early flat attachment to the later curved surface attachment, and the application of curved surfaces from 2.5D to 3D, the requirements for the bonding effect of tapes are getting higher and higher. However, the existing functional metal film materials still have the following obvious defects: Affected by the inherent properties of acrylic acid at high temperature, its general high-temperature online peeling force will drop significantly, and may be less than 1 / 3 of the normal temperature peeling force. Among them, the peeling force and cohesive force are inversely expressed under a certain formulation system.

[0004] Therefore, providing a method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate to solve the above-mentioned defects is a major problem that needs to be solved at present. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a high-temperature and high-viscosity metal film with a metal film as a substrate. The high-temperature and high-viscosity metal film developed according to the technical solution provided by the present invention achieves high peeling force and high cohesion; the thickness is 10U~200U, and the peeling force is taken as an example of the 50U finished product thickness index. The normal temperature peeling force can reach more than 4000gf / inch, and the high temperature peeling force can reach more than 2000gf / inch, and the cohesion retention force can meet the high temperature of 85 degrees / 1000g>24H. It has good heat dissipation effect, and the overall thermal conductivity is greater than 100W / mk; it has excellent shielding effectiveness, and the shielding effectiveness is greater than 80dB at 10M~5GHz, and it has excellent supporting performance. The substrate has high stiffness, and its Vickers hardness is as high as 100HV, and its elastic modulus is as high as 50000MPa.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate comprises the following steps:

[0008] S1. Preparation of high viscosity slurry:

[0009] S101. Preparation of primary slurry: 40-60 parts of epoxy resin by mass are taken and stirred at a temperature of 40-50°C, 4-5 parts of chromium oxide, sodium sulfite, a mixture of diphenyl ether tetracarboxylic dianhydride in a mass ratio of 3:2:1, and 5-7 parts of dispersant are added in sequence, and stirred for 0.5-1h; then 1-2 parts of coupling agent are added, and the temperature is quickly raised to 130-160°C, stirred for 1-2h, and cooled to room temperature to obtain primary slurry;

[0010] S102. Preparation of high-viscosity slurry: 2-3 parts of a mixture of 2-hydroxy-2-methyl-1-phenylacetone and 1-hydroxycycloethylphenyl ketone in a mass ratio of 1:1 and 20-30 parts of filler are added to the primary slurry prepared in S101, and then the temperature is raised to 90-110° C., stirred for 1-2 hours, and cooled to room temperature to obtain a high-viscosity slurry;

[0011] S2. Microwave roller coating of high viscosity slurry: The metal film substrate is subjected to microwave treatment for 5-10 minutes, and then the high viscosity slurry is evenly roller-coated on the surface of the metal film substrate under the microwave treatment condition, and the roller coating thickness is 10-200U;

[0012] S3. Ultraviolet light irradiation treatment: After the metal film substrate after step S2 is subjected to ultraviolet light radiation irradiation treatment, a high-temperature and high-viscosity metal film is obtained.

[0013] Preferably, in S101, the dispersant is selected from one of polyethylene glycol and stearamide;

[0014] Preferably, in S101, the coupling agent is selected from one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and isobutyltriethoxysilane;

[0015] Preferably, in S102, the filler is selected from one or more of talc powder, mica powder, titanium dioxide, and silicon nitride.

[0016] Preferably, in S2, the process parameters of the microwave treatment are: 20-25 W / cm2.

[0017] Preferably, in S3, the process parameters of the ultraviolet radiation are temperature 60-70°C, energy UVA600, and curing time 3-5s.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The high-temperature and high-viscosity metal film material prepared by the method provided by the present invention achieves high peeling force and high cohesion; the peeling force is taken as an example of the thickness index of the 50U finished product, the normal temperature peeling force can reach more than 4000gf / inch, the high temperature peeling force can reach more than 2000gf / inch, and the cohesion retention force can meet the high temperature of 85 degrees / 1000g>24H; the overall thermal conductivity is greater than 100W / mk; it has excellent shielding effectiveness, and the shielding effectiveness is greater than 80dB at 10M~5GHz;

[0020] 2. The high-temperature and high-viscosity metal film material prepared by the method provided by the present invention has excellent supporting performance and high stiffness of the substrate. Its Vickers hardness is as high as 100 HV and its elastic modulus is as high as 50,000 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a process flow chart for preparing the high temperature and high viscosity metal thin film material of the present invention;

[0022] Figure 2 The present invention is a flow chart of the preparation process of the high viscosity slurry. DETAILED DESCRIPTION

[0023] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] See also Figure 1-2 , the present invention provides a technical solution:

[0025] Example 1

[0026] S1. Preparation of high viscosity slurry:

[0027] S101. Preparation of primary slurry: 40 parts of epoxy resin are taken by mass and stirred at a temperature of 40°C, 4 parts of chromium oxide, sodium sulfite, a mixture of diphenyl ether tetracarboxylic anhydride in a mass ratio of 3:2:1, 5 parts of polyethylene glycol are added in sequence, and stirred for 0.5h, followed by adding 1 part of γ-aminopropyltriethoxysilane, and the temperature is quickly raised to 130°C, stirred for 1h, and cooled to room temperature to obtain a primary slurry;

[0028] S102. Preparation of high-viscosity slurry: Add 2 parts of a mixture of 2-hydroxy-2-methyl-1-phenylacetone and 1-hydroxycycloethyl phenyl ketone in a mass ratio of 1:1, and 20 parts of a mixture of titanium dioxide and talc in a mass ratio of 1:4 to the primary slurry prepared in S101, then heat to 90° C., stir for 2 hours, and cool to room temperature to obtain a high-viscosity slurry;

[0029] S2. Microwave roller coating of high viscosity slurry: Control the microwave process parameters to 20W / cm2, microwave the metal film substrate for 5 minutes, and then evenly roll the high viscosity slurry on the surface of the metal film substrate under microwave treatment conditions, with a roller coating thickness of 50U;

[0030] S3. Ultraviolet irradiation treatment: The ultraviolet irradiation process parameters are controlled to be a temperature of 60°C and an energy of UVA600. After being subjected to ultraviolet radiation treatment for 4 seconds, a high-temperature and high-viscosity metal film is obtained.

[0031] Example 2

[0032] S1. Preparation of high viscosity slurry:

[0033] S101. Preparation of primary slurry: 60 parts of epoxy resin were taken by mass and stirred at a temperature of 40°C, 5 parts of chromium oxide, sodium sulfite, a mixture of diphenyl ether tetracarboxylic anhydride in a mass ratio of 3:2:1, and 7 parts of stearamide were added in sequence and stirred for 1 hour, followed by adding 2 parts of γ-aminopropyltrimethoxysilane, and the temperature was quickly raised to 160°C, stirred for 2 hours, and cooled to room temperature to obtain a primary slurry;

[0034] S102. Preparation of high-viscosity slurry: 3 parts of a mixture of 2-hydroxy-2-methyl-1-phenylacetone and 1-hydroxycycloethylphenyl ketone in a mass ratio of 1:1 and 30 parts of a mixture of silicon nitride and mica powder in a mass ratio of 2:3 were added to the primary slurry prepared in S101, followed by heating to 110° C., stirring for 2 h, and cooling to room temperature to obtain a high-viscosity slurry;

[0035] S2. Microwave roller coating of high viscosity slurry: Control the microwave process parameters to 25W / cm2, microwave the metal film substrate for 8 minutes, and then evenly roll the high viscosity slurry on the surface of the metal film substrate under the microwave treatment condition, with a roller coating thickness of 100U;

[0036] S3. Ultraviolet irradiation treatment: Control the ultraviolet irradiation process parameters to be a temperature of 60-70°C and an energy of UVA600. After subjecting it to ultraviolet radiation treatment for 5 seconds, a high-temperature and high-viscosity metal film is obtained.

[0037] In order to improve the technical effect of the high-temperature and high-viscosity metal film, this embodiment intends to further process step S101, including the following steps:

[0038] Add 6 parts of a mixture of sodium carbonate and sodium bicarbonate in a mass ratio of 1:1 and 8-10 parts of a mixture of zinc phosphate and aluminum chromate in a mass ratio of 1:1 to the primary slurry prepared in S101, and stir for 20 minutes;

[0039] The high-viscosity slurry obtained in step S102 is further processed, including the following steps:

[0040] The pH value of the obtained high-viscosity slurry was adjusted to 5, the temperature was raised to 60°C, and stirred for 30 minutes.

[0041] Example 3

[0042] S1. Preparation of high viscosity slurry:

[0043] S101. Preparation of primary slurry: 50 parts of epoxy resin were taken by mass and stirred at a temperature of 45°C, and 5 parts of chromium oxide, sodium sulfite, a mixture of diphenyl ether tetracarboxylic anhydride in a mass ratio of 3:2:1 and 6 parts of stearamide were added in sequence, and stirred for 1 hour, followed by adding 1 part of isobutyl triethoxysilane, and the temperature was quickly raised to 150°C, stirred for 1.5 hours, and cooled to room temperature to obtain a primary slurry;

[0044] S102. Preparation of high-viscosity slurry: Add 2 parts of a mixture of 2-hydroxy-2-methyl-1-phenylacetone and 1-hydroxycycloethylphenyl ketone in a mass ratio of 1:1, 25 parts of silicon nitride, and a mixture of talc powder and mica powder in a mass ratio of 2:2:3 to the primary slurry prepared in S101, then heat to 100° C., stir for 1.5 hours, and cool to room temperature to obtain a high-viscosity slurry;

[0045] S2. Microwave roller coating of high viscosity slurry: Control the microwave process parameters to 22W / cm2, microwave the metal film substrate for 10 minutes, and then evenly roll the high viscosity slurry on the surface of the metal film substrate under microwave treatment conditions, with a roller coating thickness of 80U;

[0046] S3. Ultraviolet irradiation treatment: The ultraviolet irradiation process parameters are controlled to be a temperature of 65°C and an energy of UVA600. After being subjected to ultraviolet radiation treatment for 3 seconds, a high-temperature and high-viscosity metal film is obtained.

[0047] Comparative Example

[0048] Comparative Example 1:

[0049] Comparative Example 1 is different from Example 1 in that the S1 step originally existing in Example 1 is partially omitted in Comparative Example 1, thereby canceling the step of adding "a mixture of γ-aminopropyltriethoxysilane, 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycycloethylphenylketone in a mass ratio of 1:1", and the remaining steps are exactly the same in Comparative Example 1 and Example 1.

[0050] Comparative Example 2:

[0051] Comparative Example 2 is different from Example 1 in that the S1 step originally existing in Example 1 is partially omitted in Comparative Example 2, thereby canceling the step of adding "a mixture of chromium oxide, sodium sulfite, diphenyl ether tetracarboxylic dianhydride in a mass ratio of 3:2:1, and polyethylene glycol", and the remaining steps are exactly the same in Comparative Example 2 and Example 1.

[0052] Comparative Example 3:

[0053] Comparative Example 3 is different from Comparative Example 2 in that the S1 step originally existing in Comparative Example 2 is partially omitted in Comparative Example 3, thereby canceling the step of adding "a mixture of γ-aminopropyltriethoxysilane, 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycycloethylphenylketone in a mass ratio of 1:1", and the remaining steps are exactly the same in Comparative Example 3 and Comparative Example 2.

[0054] Comparative Example 4:

[0055] There are the following differences between Comparative Example 4 and Example 1. The only difference is that in Comparative Example 4, steps S2 and S3 originally existing in Example 1 are omitted, thereby canceling the steps of "microwave treatment of the metal film substrate" and "ultraviolet light irradiation treatment", and the remaining steps in Comparative Example 4 are exactly the same as those in Example 1.

[0056] The peeling force of Examples 1-3 and Comparative Examples 1-4 at room temperature and the peeling force, cohesion, thermal conductivity, Vickers hardness, and elastic modulus at high temperature (85° C.) were measured; the shielding coefficients of Examples 1-3 and Comparative Examples 1-4 were measured at 10M to 5GHz, and the results are shown in Table 1 below:

[0057] Table 1

[0058]

[0059]

[0060] The test results in Table 1 show that the parameters such as the peeling force at room temperature / high temperature, the cohesive force at high temperature, the thermal conductivity, the shielding effectiveness, the Vickers hardness, and the elastic modulus of Examples 1-3 are significantly better than those of Comparative Examples 1-4. Therefore, the high-temperature and high-viscosity metal film prepared by the technical solution provided by the present invention is reliable. At the same time, the parameters such as the peeling force at room temperature / high temperature, the cohesive force at high temperature, the thermal conductivity, the shielding effectiveness, the Vickers hardness, and the elastic modulus of Example 1 are significantly better than those of Comparative Examples 1-4. In particular, the huge difference in parameters between Example 1 and Comparative Example 3 proves that the technical solution provided by the present invention can significantly improve the metal film on the basis of using a brand-new coating material. The peeling force, cohesive force, thermal conductivity and shielding effectiveness of the material. The high-temperature and high-viscosity metal film material with a thickness of 50U prepared by the technical solution of the present invention has a room temperature peeling force of more than 4000gf / inch, a high temperature peeling force of more than 2000gf / inch, and a cohesive retention force that can meet the high temperature of 85 degrees / 1000g>24H, an overall thermal conductivity of more than 100W / mk, and a shielding effectiveness of more than 80dB at 10M~5GHz; Vickers hardness of more than 100HV, and an elastic modulus of more than 50000MPa, which effectively solves the defect that the high-temperature online peeling force of the metal film material will be greatly reduced, and has broad application prospects.

[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate, It is characterized in that The following steps are involved: S1. Preparation of high viscosity slurry: S101. Preparation of primary slurry: 40-60 parts of epoxy resin by mass are taken and stirred at a temperature of 40-50°C, 4-5 parts of chromium oxide, sodium sulfite, a mixture of diphenyl ether tetracarboxylic dianhydride in a mass ratio of 3:2:1, and 5-7 parts of dispersant are added in sequence, and stirred for 0.5-1h; then 1-2 parts of coupling agent are added, and the temperature is quickly raised to 130-160°C, stirred for 1-2h, and cooled to room temperature to obtain primary slurry; S102. Preparation of high-viscosity slurry: 2-3 parts of a mixture of 2-hydroxy-2-methyl-1-phenylacetone and 1-hydroxycycloethylphenyl ketone in a mass ratio of 1:1 and 20-30 parts of filler are added to the primary slurry prepared in S101, and then the temperature is raised to 90-110° C., stirred for 1-2 hours, and cooled to room temperature to obtain a high-viscosity slurry; S2. Microwave roller coating of high viscosity slurry: The metal film substrate is subjected to microwave treatment for 5-10 minutes, and then the high viscosity slurry is evenly roller-coated on the surface of the metal film substrate under the microwave treatment condition, and the roller coating thickness is 10-200U; S3. UV irradiation treatment: After the metal film substrate after step S2 is subjected to UV radiation irradiation treatment, a high-temperature and high-viscosity metal film is obtained; In S101, the dispersant is selected from one of polyethylene glycol and stearamide; In S101, the coupling agent is selected from one or more of γ-aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, and isobutyltriethoxysilane.

2. A method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate according to claim 1, It is characterized in that In S102, the filler is selected from one or more of talc powder, mica powder, titanium dioxide, and silicon nitride.

3. The method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate according to claim 1, It is characterized in that In S2, the process parameters of the microwave treatment are: 20-25W / cm 2 .

4. The method for preparing a high-temperature and high-viscosity metal film using a metal film as a substrate according to claim 1, It is characterized in that In S3, the process parameters of the ultraviolet radiation are temperature 60-70°C, energy UVA600, and curing time 3-5s.

Citation Information

Patent Citations

  • Preparation method of high-temperature-resistant heat-conduction single-sided adhesive tape

    CN109880545A

  • High-flexibility, high-hardness and low-warpage hardening glue, hardening protective film and preparation method

    CN110484180A

  • High-temperature-resistant epoxy resin adhesive and preparation method thereof

    CN113403010A