A composite friction material

By using a composite friction material and modified polyester fiber woven with a mixture of cotton and polyester fiber, the problem of test result deviation in the alcohol friction resistance test is solved, the water absorption and air permeability are improved, and the water absorption and breathability are improved, meeting various industry standards, and reducing the Trial costs.

CN118087146BActive Publication Date: 2024-10-29FOSHAN JINLEI TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410198574.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-22
Publication Date
2024-10-29
Estimated Expiration
2044-02-22

AI Technical Summary

Technical Problem

There is a deviation in the test results in the alcohol friction resistance test, which mainly comes from the inconsistent standards of weight weight, friction cloth material, friction speed and alcohol purity, resulting in inaccurate test results.

Method used

Composite friction material woven with a mixture of cotton and polyester fiber, 40%-60% cotton, 60%-40% polyester fiber, and ≥95% edible alcohol and hydrophilic modified polyester fiber. Ester fiber improves hydrophilicity and breathability, reducing alcohol volatilization and frictional heat generation.

Benefits of technology

It reduces the deviation of test results in the alcohol friction resistance test, improves the water absorption and breathability of the friction cloth, avoids alcohol flashover caused by friction heat, meets the usage standards of various industries, and reduces test costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a composite friction material, and relates to the field of friction materials. A composite friction material comprises a friction cloth, wherein the friction cloth is made of cotton and polyester fibers mixed and woven, and the mass percentages of the cotton and the polyester fibers in the friction cloth are respectively: 40%-60% cotton and 60%-40% polyester fibers. The application has the effect of providing a friction cloth suitable for all industries and reducing the deviation of test results.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of friction materials, in particular to a composite friction material. Background Art

[0002] Alcohol friction resistance test is widely used in alcohol resistance and friction resistance test of surface materials. It can be used to test the wear resistance of spray paint, silk screen and other printed bodies on the surface of various electronic products such as plastics, mobile phone shells, battery silk screen, leather, etc., and evaluate the wear resistance of surface materials. Alcohol friction resistance test requires the use of a multifunctional alcohol friction resistance tester.

[0003] During the test, fix the material sample to be tested on the clamping device of the test machine, wrap the friction part of the friction rod with friction cloth and fix the position, pour alcohol into the hollow position of the upper part of the friction rod, wet the friction cloth with alcohol, place weights, set the friction speed and friction times. Turn on the instrument, rub the material sample with friction cloth, observe the surface loss of the material sample, and evaluate the wear resistance.

[0004] The experimental deviation of alcohol friction resistance test mainly comes from four aspects: weight of weight, friction cloth material, friction speed and alcohol purity. At present, the testing standards only make specific data standards for weight of weight and friction speed. There is no unified standard for friction cloth material and alcohol purity, which leads to deviation in test results. Summary of the invention

[0005] In order to provide a friction cloth suitable for all industries and reduce the deviation of test results, the present application provides a composite friction material.

[0006] The composite friction material provided in this application adopts the following technical solution:

[0007] A composite friction material comprises a friction cloth, wherein the friction cloth is made of cotton and polyester fibers mixed and woven together, and the mass percentages of the cotton and the polyester fibers in the friction cloth are respectively: 40%-60% cotton and 60%-40% polyester fibers.

[0008] By adopting the above technical scheme, cotton has good air permeability and strong water absorption, polyester fiber has good air permeability, friction resistance and strong structural stability, and the friction cloth woven by mixing cotton and polyester fibers has good water absorption, thereby retaining alcohol and reducing the volatilization of alcohol during work; it has good air permeability, thereby avoiding alcohol flash fire caused by frictional heat; after a long period of friction, there will be no structural fracture, and the friction degree will not be affected, which meets the use standards of various industries for alcohol friction resistance testing.

[0009] Optionally, alcohol is also included, and the alcohol is used to wet the friction cloth. The alcohol is selected from edible alcohol with a volume concentration of ≥95%.

[0010] By adopting the above technical solution, edible alcohol ≥95% is suitable for most alcohol resistance test standards. There is no significant difference in test results compared with anhydrous ethanol, and edible alcohol has a higher cost-effectiveness.

[0011] Optionally, the polyester fiber is a hydrophilically modified polyester fiber.

[0012] By adopting the above technical solution, the hydrophilicity of the polyester fiber is improved, thereby increasing the absorption of alcohol by the friction cloth and reducing the evaporation of alcohol due to frictional heat, meeting the test requirements of highly wear-resistant products. There is no need to add additional alcohol in an experiment, thereby avoiding increasing test variability.

[0013] Optionally, the hydrophilic modified polyester fiber is made of the following raw materials in parts by weight:

[0014] 160-170 parts of purified terephthalic acid;

[0015] 65-75 parts of ethylene glycol;

[0016] 2-5 parts of polyol monomer;

[0017] Catalyst 0.5-1 part;

[0018] 1-3 parts of additives.

[0019] By adopting the above technical scheme, the polyester fiber is modified using a polyol monomer, the original molecular chain structure of the polyester fiber is destroyed, and hydrophilic hydroxyl groups are introduced into the molecular chain of the hydrophilic modified polyester fiber to improve the hydrophilicity of the polyester fiber.

[0020] Optionally, the polyol monomer is selected from one or more of sorbitol, polyethylene glycol, tetramethyldisiloxanediol, 1,4-butanediol, and dimethyldiphenyldisiloxanediol.

[0021] By adopting the above technical solution, a polyol having multiple hydroxyl groups is selected.

[0022] Optionally, the polyol monomer is a mixture of 1,4-butanediol and tetramethyldisiloxanediol, and the mass ratio of the 1,4-butanediol to the tetramethyldisiloxanediol is (1.2-1.5):(1.0-1.1).

[0023] By adopting the above technical solution, polyols and polyols containing silicon in the main chain are selected and mixed as modified monomers, which improves the hydrophilicity and makes it easier for small dye molecules to penetrate, thereby improving the dyeing performance of the hydrophilic modified polyester fiber.

[0024] Optionally, the catalyst is selected from one or more of antimony trioxide, antimony acetate, and ethylene glycol antimony.

[0025] By adopting the above technical solution, the rate of the esterification reaction of purified terephthalic acid and ethylene glycol can be increased by adding an antimony-based catalyst.

[0026] Optionally, the auxiliary agent is selected from one or more of trimethyl phosphate, triethyl phosphate, tripropyl phosphate, and triphenyl phosphate.

[0027] By adopting the above technical solution, the addition of the auxiliary agent can serve as a stabilizer and reduce the viscosity of the hydrophilic modified polyester fiber at the same time.

[0028] Optionally, the preparation of the rubbing cloth comprises the following steps:

[0029] Wash the cotton and polyester fibers separately to remove impurities and dirt, and then dry the cotton and polyester fibers;

[0030] Using a carding machine, cotton and polyester fibers are mixed according to a mass ratio to form a uniform fiber mixture;

[0031] The fiber mixture is spun through a spinning frame to obtain yarn;

[0032] The yarn is subjected to subsequent treatments such as finishing and dyeing to obtain the friction cloth.

[0033] By adopting the above technical scheme, the cotton and polyester fibers are mixed by silk thread mixing, and then the cotton and polyester fibers are mixed and spun to form a tightly interwoven friction cloth.

[0034] Optionally, the preparation of the hydrophilic modified polyester fiber comprises the following steps:

[0035] Purified terephthalic acid, ethylene glycol, a catalyst and an auxiliary agent are added together to an esterification reaction kettle for esterification, and then a polyol monomer is added to continue esterification for 40-60 minutes. After the esterification is completed, vacuum is drawn to carry out polycondensation reaction. After the reaction is completed, stirring is stopped, and nitrogen is used to break the vacuum and discharge the material to obtain a hydrophilic modified polyester chip;

[0036] The hydrophilic modified polyester chips are made into hydrophilic modified polyester fibers by adopting the HOY process: metering, spinneret extrusion, cooling, oiling and high-speed winding.

[0037] By adopting the above technical solution, the polyol monomer is added in the second stage of esterification, which reduces the esterification reaction time of the polyol monomer, and effectively avoids branching and crosslinking while ensuring the introduction of hydroxyl groups into the hydrophilic modified polyester fiber.

[0038] In summary, this application has the following beneficial effects:

[0039] 1. Cotton has good air permeability and strong water absorption, while polyester fiber has good air permeability, is resistant to friction, and has strong structural stability. The friction cloth woven by a mixture of cotton and polyester fibers has good water absorption, which can retain alcohol and reduce the volatilization of alcohol during work; it has good air permeability, thus avoiding alcohol flash fire caused by heat generated by friction; after a long period of friction, there will be no structural fractures, which will not affect the degree of friction, and it meets the use standards of various industries for alcohol friction resistance testing.

[0040] 2. Edible alcohol ≥95% is suitable for most alcohol resistance test standards. There is no significant difference in test results compared with anhydrous ethanol, and edible alcohol has a higher cost-effectiveness.

[0041] 3. The hydrophilic modified polyester fiber improves the hydrophilicity of the polyester fiber, thereby increasing the absorption of alcohol by the friction cloth and reducing the evaporation of alcohol due to frictional heat, meeting the test of high wear-resistant products. There is no need to add additional alcohol in an experiment to avoid increasing test variability. DETAILED DESCRIPTION

[0042] The present application is further described in detail below in conjunction with Examples 1-9 and Comparative Examples 1-3.

[0043] Preparation Example

[0044] Preparation Example 1

[0045] Preparation of hydrophilic modified polyester fiber

[0046] 160 parts by mass of purified terephthalic acid, 65 parts by mass of ethylene glycol, 0.5 parts by mass of ethylene glycol antimony and 1 part by mass of trimethyl phosphate were mixed, stirred evenly and added into an esterification reaction kettle for esterification reaction. The reaction temperature was controlled to be 230° C. and the reaction pressure was 0.2 MPa. When the esterification water output reached 87%, 2 parts by mass of sorbitol were added into the esterification reaction kettle. The esterification reaction was continued at normal pressure for 40 minutes. When the esterification water output reached 95%, the esterification was terminated.

[0047] After the esterification reaction is completed, the low vacuum stage condensation reaction begins under negative pressure conditions. The pressure in this stage is steadily pumped from normal pressure to an absolute pressure of 490 Pa within 30 minutes, the reaction temperature is 250°C, and the reaction time is 35 minutes. Then the vacuum is continued to be pumped to carry out the high vacuum stage condensation reaction, so that the reaction pressure is further reduced to an absolute pressure of 100 Pa, the reaction temperature is 270°C, and the reaction time is 50 minutes to obtain hydrophilic modified polyester chips.

[0048] The hydrophilic modified polyester chips were made into hydrophilic modified polyester fibers by adopting the HOY process: metering, spinneret extrusion, cooling, oiling and high-speed winding. The spinneret aspect ratio of melt spinning was 2.5, the spinning temperature was 275°C, the side blowing speed was 0.50 m / s, and the oiling rate was 1.0%.

[0049] Preparation Example 2

[0050] Preparation of hydrophilic modified polyester fiber

[0051] 170 parts by mass of purified terephthalic acid, 75 parts by mass of ethylene glycol, 1 part by mass of antimony trioxide and 3 parts by mass of triphenyl phosphate were mixed, stirred evenly and added into an esterification reaction kettle for esterification reaction. The reaction temperature was controlled to be 250° C. and the reaction pressure was 0.4 MPa. When the esterification water output reached 90%, 5 parts by mass of 1,4-butanediol were added into the esterification reaction kettle. The esterification reaction was continued for 60 minutes under normal pressure. When the esterification water output reached 97%, the esterification was terminated.

[0052] After the esterification reaction is completed, the low vacuum stage condensation reaction begins under negative pressure conditions. The pressure in this stage is steadily pumped from normal pressure to an absolute pressure of 420 Pa within 35 minutes, the reaction temperature is 265°C, and the reaction time is 40 minutes. Then the vacuum is continued to be pumped to carry out the high vacuum stage condensation reaction, so that the reaction pressure is further reduced to an absolute pressure of 90 Pa, the reaction temperature is 280°C, and the reaction time is 55 minutes, thereby obtaining hydrophilic modified polyester chips.

[0053] The hydrophilic modified polyester chips were made into hydrophilic modified polyester fibers by adopting the HOY process: metering, spinneret extrusion, cooling, oiling and high-speed winding. The spinneret aspect ratio of melt spinning was 3, the spinning temperature was 290°C, the side blowing speed was 0.40m / s, and the oiling rate was 1.2%.

[0054] Preparation Example 3

[0055] Preparation of hydrophilic modified polyester fiber

[0056] 165 parts by mass of purified terephthalic acid, 70 parts by mass of ethylene glycol, 0.8 parts by mass of antimony acetate and 2 parts by mass of triethyl phosphate were mixed, stirred evenly and added into an esterification reaction kettle for esterification reaction. The reaction temperature was controlled to be 240° C. and the reaction pressure was 0.3 MPa. When the esterification water output reached 88%, 3 parts by mass of dimethyldiphenyldisiloxanediol were added into the esterification reaction kettle. The esterification reaction was continued under normal pressure for 50 minutes. When the esterification water output reached 96%, the esterification was terminated.

[0057] After the esterification reaction is completed, the low vacuum stage condensation reaction begins under negative pressure conditions. The pressure in this stage is steadily pumped from normal pressure to an absolute pressure of 450 Pa within 30 minutes, the reaction temperature is 260°C, and the reaction time is 40 minutes. Then the vacuum is continued to be pumped to carry out the high vacuum stage condensation reaction, so that the reaction pressure is further reduced to an absolute pressure of 95 Pa, the reaction temperature is 275°C, and the reaction time is 50 minutes to obtain hydrophilic modified polyester chips.

[0058] The hydrophilic modified polyester chips were made into hydrophilic modified polyester fibers by adopting the HOY process: metering, spinneret extrusion, cooling, oiling and high-speed winding. The spinneret aspect ratio of melt spinning was 2.8, the spinning temperature was 280°C, the side blowing speed was 0.45m / s, and the oiling rate was 1.1%.

[0059] Preparation Example 4

[0060] Preparation of hydrophilic modified polyester fiber

[0061] The difference between this preparation example and preparation example 1 is that the polyol monomer in this preparation example is a mixture of 1,4-butanediol and tetramethyldisiloxanediol, specifically 1.2 parts by mass of 1,4-butanediol and 0.8 parts by mass of tetramethyldisiloxanediol.

[0062] The preparation method of the hydrophilic modified polyester fiber is the same as that in Preparation Example 1.

[0063] Preparation Example 5

[0064] Preparation of hydrophilic modified polyester fiber

[0065] The difference between this preparation example and preparation example 1 is that the polyol monomer in this preparation example is a mixture of 1,4-butanediol and tetramethyldisiloxanediol, specifically 1.04 parts by mass of 1,4-butanediol and 0.96 parts by mass of tetramethyldisiloxanediol.

[0066] The preparation method of the hydrophilic modified polyester fiber is the same as that in Preparation Example 1.

[0067] Example

[0068] Example 1

[0069] Preparation of a friction cloth

[0070] Wash the cotton and polyester fibers separately to remove impurities and dirt, and then dry the cotton and polyester fibers;

[0071] Using a carding machine to mix cotton and polyester fibers in a mass ratio of 60%:40% to form a uniform fiber mixture; spinning the fiber mixture and spinning it through a spinning machine to obtain yarn;

[0072] The yarn is subjected to subsequent treatments such as finishing and dyeing to obtain the friction cloth.

[0073] The cotton was purchased from Shandong Xuzheng Textile Co., Ltd., and the polyester fiber was purchased from Zhejiang Euro Knitting Co., Ltd.

[0074] Example 2

[0075] Preparation of a friction cloth

[0076] The difference between this embodiment and embodiment 1 is that the cotton fiber and the polyester fiber are mixed in a mass ratio of 50%:50%.

[0077] The preparation method of the rubbing cloth is the same as that of Example 1.

[0078] The cotton was purchased from Shandong Xuzheng Textile Co., Ltd., and the polyester fiber was purchased from Zhejiang Euro Knitting Co., Ltd.

[0079] Example 3

[0080] Preparation of a friction cloth

[0081] The difference between this embodiment and embodiment 1 is that the cotton fiber and the polyester fiber are mixed in a mass ratio of 40%:60%.

[0082] The preparation method of the rubbing cloth is the same as that of Example 1.

[0083] The cotton was purchased from Shandong Xuzheng Textile Co., Ltd., and the polyester fiber was purchased from Zhejiang Euro Knitting Co., Ltd.

[0084] Example 4

[0085] Preparation of a friction cloth

[0086] The difference between this embodiment and embodiment 1 is that the polyester fiber is hydrophilic modified polyester fiber, and the mass ratio of cotton to hydrophilic modified polyester fiber is 60%:40%.

[0087] The preparation method of the rubbing cloth is the same as that of Example 1.

[0088] The cotton was purchased from Shandong Xuzheng Textile Co., Ltd., and the hydrophilic modified polyester fiber was purchased from Zhejiang Euro Knitting Co., Ltd.

[0089] Example 5

[0090] Preparation of a friction cloth

[0091] The difference between this embodiment and embodiment 1 is that the polyester fiber is the hydrophilic modified polyester fiber prepared in embodiment 1, and the mass ratio of cotton to the hydrophilic modified polyester fiber is 60%:40%.

[0092] The preparation method of the rubbing cloth is the same as that of Example 1.

[0093] Example 6

[0094] Preparation of a friction cloth

[0095] The difference between this embodiment and embodiment 1 is that the polyester fiber is the hydrophilic modified polyester fiber prepared in preparation example 2, and the mass ratio of cotton to the hydrophilic modified polyester fiber is 50%:50%.

[0096] The preparation method of the rubbing cloth is the same as that of Example 1.

[0097] Example 7

[0098] Preparation of a friction cloth

[0099] The difference between this embodiment and embodiment 1 is that the polyester fiber is the hydrophilic modified polyester fiber prepared in preparation example 3, and the mass ratio of cotton to the hydrophilic modified polyester fiber is 40%:60%.

[0100] The preparation method of the rubbing cloth is the same as that of Example 1.

[0101] Example 8

[0102] Preparation of a friction cloth

[0103] The difference between this embodiment and embodiment 1 is that the polyester fiber is the hydrophilic modified polyester fiber prepared in embodiment 4, and the mass ratio of cotton to the hydrophilic modified polyester fiber is 60%:40%.

[0104] The preparation method of the rubbing cloth is the same as that of Example 1.

[0105] Example 9

[0106] Preparation of a friction cloth

[0107] The difference between this embodiment and embodiment 1 is that the polyester fiber is the hydrophilic modified polyester fiber prepared in embodiment 5, and the mass ratio of cotton to the hydrophilic modified polyester fiber is 60%:40%.

[0108] The preparation method of the rubbing cloth is the same as that of Example 1.

[0109] Comparative Example

[0110] Comparative Example 1

[0111] Preparation of a friction cloth

[0112] The difference between this comparative example and Example 1 is that the friction cloth is woven from 100% by mass of cotton.

[0113] Comparative Example 2

[0114] Preparation of a friction cloth

[0115] The difference between this comparative example and Example 1 is that the friction cloth is woven from 100% by mass of polyester fibers.

[0116] Comparative Example 3

[0117] Preparation of a friction cloth

[0118] The difference between this comparative example and Example 1 is that the friction cloth is made of 80% by mass of cotton and 20% by mass of polyester fiber mixed and woven.

[0119] The preparation method of the rubbing cloth is the same as that of Example 1.

[0120] Performance Testing

[0121] 1. Appearance observation

[0122] The friction cloths prepared in Examples 1-9 and Comparative Examples 1-3 were observed to see whether the surfaces of the friction cloths were smooth and whether there was a drop-line phenomenon, and the results were recorded in Table 1.

[0123] 2. Texture Detection

[0124] The friction cloths prepared in Examples 1-9 and Comparative Examples 1-3 were respectively moistened with edible alcohol having a volume concentration of ≥95%, and subjected to 600 abrasion tests on high-permeability glass. The friction cloths were observed using a 100X electronic magnifying glass to see if their texture had structural fractures, and the results were recorded in Table 1.

[0125] 3. Water absorption

[0126] The capillary effect of the friction cloths prepared in Examples 1-9 and Comparative Examples 1-3 was measured using a capillary effect tester in accordance with FZ / T 01071-1999 “Test Method for Capillary Effect of Textiles”, and the results are recorded in Table 1.

[0127] 4. Breathability

[0128] The air permeability of the friction cloths prepared in Examples 1-9 and Comparative Examples 1-3 was measured using a digital air permeability meter in accordance with GB / T 5453-1997 "Determination of Air Permeability of Textile Fabrics", and the results are recorded in Table 1.

[0129] Table 1

[0130]

[0131] Result analysis:

[0132] Comparative Example 1 uses pure cotton as the friction cloth. The prepared friction cloth has good hydrophilicity and good air permeability, but poor wear resistance. After the wear resistance test of high-permeability glass, the pure cotton friction cloth will have structural fractures. In the alcohol friction resistance test, the friction cloth is easily damaged during the friction with the wear-resistant material. At this time, it needs to be replaced, which will affect the test results. Therefore, the pure cotton friction cloth is not suitable for use as a friction cloth for alcohol wear resistance test.

[0133] Comparative Example 2 uses polyester fiber as the friction cloth. The prepared friction cloth has good air permeability and good wear resistance, but poor hydrophilicity, resulting in poor performance of the polyester fiber friction cloth in storing alcohol. In the process of testing high-wear-resistant materials, the friction cloth needs to be rubbed with the high-wear-resistant material for many times. Heat is generated during the friction process, which will accelerate the volatilization of alcohol. As a result, during the testing of high-wear-resistant materials, the alcohol in the friction cloth will evaporate completely, requiring additional addition, which will affect the results of the alcohol wear resistance test and cause deviations in the inspection.

[0134] Comparative Example 3 uses a friction cloth blended with cotton / polyester fibers in a mass ratio of 80%:20%. Compared with Examples 1-3, it has poor hydrophilicity and air permeability, indicating that when the mass ratio of cotton to polyester fibers is 40%-60% cotton and 60%-40% polyester, the blended friction cloth has good air permeability and hydrophilicity, and after long-term friction with highly wear-resistant materials, the friction cloth will not undergo structural fractures, thereby meeting the standards for alcohol friction resistance tests in various industries.

[0135] Example 4 uses hydrophilic modified polyester fiber and cotton for blending, so that the hydrophilicity of the friction cloth is better, which is beneficial to the storage of alcohol by the friction cloth.

[0136] In Example 5-7, polyol monomers are used to modify polyester fibers to obtain hydrophilic modified polyester fibers, and the hydrophilic modified polyester fibers are blended with cotton. The grafting of polyol monomers introduces more hydrophilic hydroxyl groups into the polyester fibers, thereby improving the hydrophilicity and air permeability of the polyester fibers, thereby improving the hydrophilicity and air permeability of the friction cloth. This makes it unnecessary to add additional alcohol to the friction cloth in a test, avoiding test differences caused by adding alcohol, increasing air permeability, and further ensuring that high-concentration alcohol will not flash under friction heat, thereby improving test safety.

[0137] In Examples 8-9, the polyol monomer used for modification is specifically limited to a mixture of 1,4-butanediol and tetramethyldisiloxanediol, and the mixing ratio is limited. By introducing silicon element into the polyester fiber, the dyeing performance of the hydrophilic modified polyester fiber is improved.

[0138] The implementation principle of a composite friction material in the embodiment of the present application is: when the friction cloth is used in the alcohol friction resistance test, the test steps are:

[0139] 1. Turn on the power, wait for 15 minutes, and turn on the switch.

[0140] 2. Adjust the speed to 30 times / minute, the number of frictions to 15 times / cycle, and the weight to 1kg.

[0141] 3. Place the sample and fix it on the friction table.

[0142] 4. The friction part of the friction rod is wrapped with a three-layer folded friction cloth and fixed in place with a rope to prevent the friction cloth from loosening during inspection; high-purity alcohol is poured into the hollow position of the upper part of the friction rod to ensure that the friction cloth is fully moistened with alcohol; and weights are placed in.

[0143] 5. Preset the friction cycle and start the instrument.

[0144] 6. After the instrument is finished, take out the weight, remove the friction rod and remove the friction cloth (each time a new sample is tested, the four steps need to be repeated to prevent the friction cloth from being stained with sample particles and affecting the test results of subsequent samples).

[0145] 7. Use a transmission density meter detector to detect friction loss.

[0146] 7. Record data.

[0147] 8. Turn off the switch and power.

[0148] The embodiments of this specific implementation are all preferred embodiments of this application, and are not intended to limit the protection scope of this application. Therefore, any equivalent changes made based on the structure, shape, and principle of this application should be included in the protection scope of this application.

Claims

1. A composite friction material, characterized in that: It includes a friction cloth, which is made of a mixture of cotton and polyester fibers, and the mass percentages of the cotton and the polyester fibers in the friction cloth are: 40%-60% cotton and 60%-40% polyester fibers; It also includes alcohol, which is used to wet the friction cloth, and the alcohol is selected from edible alcohol with a volume concentration of ≥95%; The polyester fiber is a hydrophilic modified polyester fiber; The hydrophilic modified polyester fiber is made of the following raw materials in parts by weight: 160-170 parts of purified terephthalic acid; 65-75 parts of ethylene glycol; 2-5 parts of polyol monomer; Catalyst 0.5-1 part; 1-3 parts of additives.

2. A composite friction material according to claim 1, characterized in that: The polyol monomer is selected from one or more of sorbitol, polyethylene glycol, tetramethyl disiloxane diol, 1,4-butanediol, and dimethyl diphenyl disiloxane diol.

3. A composite friction material according to claim 2, characterized in that: The polyol monomer is a mixture of 1,4-butanediol and tetramethyldisiloxanediol, and the mass ratio of the 1,4-butanediol to the tetramethyldisiloxanediol is (1.2-1.5):(1.0-1.1).

4. A composite friction material according to claim 1, characterized in that: The catalyst is selected from one or more of antimony trioxide, antimony acetate, and ethylene glycol antimony.

5. The composite friction material according to claim 1, characterized in that: The auxiliary agent is selected from one or more of trimethyl phosphate, triethyl phosphate, tripropyl phosphate and triphenyl phosphate.

6. The composite friction material according to claim 1, characterized in that: The preparation of the friction cloth comprises the following steps: Wash the cotton and polyester fibers separately to remove impurities and dirt, and then dry the cotton and polyester fibers; Using a carding machine, cotton and polyester fibers are mixed according to a mass ratio to form a uniform fiber mixture; The fiber mixture is spun through a spinning frame to obtain yarn; The yarn is finished and dyed to obtain a friction cloth.

7. The composite friction material according to claim 1, characterized in that: The preparation of the hydrophilic modified polyester fiber comprises the following steps: Purified terephthalic acid, ethylene glycol, a catalyst and an auxiliary agent are added together to an esterification reaction kettle for esterification, and then a polyol monomer is added to continue esterification for 40-60 minutes. After the esterification is completed, vacuum is drawn to carry out polycondensation reaction. After the reaction is completed, stirring is stopped, and nitrogen is used to break the vacuum and discharge the material to obtain a hydrophilic modified polyester chip; The hydrophilic modified polyester chips are made into hydrophilic modified polyester fibers by adopting the HOY process: metering, spinneret extrusion, cooling, oiling and high-speed winding.

Citation Information

Patent Citations

  • Polyester HOY (High-Oriented Fibre) and preparation method thereof

    CN109666985A

  • Rubbing fabric

    JP2004332136A