A kind of wipe-resistant artificial leather and preparation method thereof
Patent Information
- Application Number
- CN202410449146.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-15
AI Technical Summary
Existing artificial leather has poor wear resistance and is prone to wear and tear, resulting in shortened service life, affecting user experience and increasing environmental pollution.
Nanofibers are prepared using electrospinning technology, and nano-calcium carbonate is formed through temperature-controlled reaction and ultrasonic vibration. It is combined with modified polyvinyl chloride and pyrophyllite to form a composite film layer to improve interface strength and wear resistance.
By forming nano-calcium carbonate with a large particle size structure and a dense fiber network, the wear resistance of artificial leather is significantly improved, the service life is extended and environmental pollution is reduced.
Smart Images

Figure BDA0004792052880000121 
Figure BDA0004792052880000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of leather materials, and in particular relates to a kind of wipe-resistant artificial leather and a preparation method thereof. Background Art
[0002] Artificial leather is a plastic product similar to leather. It is usually made of fabric as the base, on which a layer of resin mixture is coated or pasted, then heated to plasticize it, and rolled flat or embossed to make its appearance, texture, texture and color very similar to natural leather, giving people a high-end and fashionable texture, which is very popular with consumers. Due to market demand, most of the artificial leather currently on the market usually uses synthetic fiber materials, such as polyurethane, polyester, etc., which are simpler in structure and organization than natural leather. The molecular chain structure of these synthetic fiber materials is relatively loose and easily affected by external friction and wear, resulting in poor wear resistance. It is easy to wear and break during use, resulting in a significant shortening of its service life, increasing the frequency of people changing products, reducing user satisfaction with artificial leather products, affecting their user experience, and also generating more waste, which has a negative impact on the environment. Summary of the invention
[0003] The invention discloses a kind of artificial leather resistant to wiping and a preparation method thereof, belonging to the technical field of leather materials. The preparation of the artificial leather comprises the following steps: mixing polyvinyl alcohol, sodium polystyrene sulfonate and deionized water, cooling and degassing, electrostatic spinning to obtain material A; placing material A in a glass airflow dryer containing glutaraldehyde solution, controlling temperature for reaction, drying to obtain material B; mixing and drying the nano calcium carbonate, deionized water and material B to obtain material C; mixing and grinding modified polyvinyl chloride, material C, antioxidant 1076 and pyrophyllite, and mixing and grinding with dioctyl terephthalate to obtain a paste; applying glue, coating the paste, setting a substrate to form a preform; treating the surface of the preform, embossing, cutting and packaging to obtain artificial leather with excellent wiping resistance.
[0004] The technical problem to be solved by the present invention is to prepare an artificial leather with excellent wear resistance and wiping resistance.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A kind of wipe-resistant artificial leather and preparation method thereof, the preparation of the artificial leather comprises the following steps:
[0007] (1) mixing calcium oxide and deionized water to prepare a calcium hydroxide suspension with a concentration of 0.65-0.75 mol / L;
[0008] (2) placing the calcium hydroxide suspension in a hydrothermal carbonization tabletop reactor, introducing carbon dioxide and nitrogen, and stirring the reaction at 16-22° C. for 5-6 minutes;
[0009] (3) then adding oxalic acid and introducing carbon dioxide, maintaining the temperature in step (2) unchanged and continuing to stir and react for 12-15 minutes to obtain nano calcium carbonate, wherein the particle size of the nano calcium carbonate is 370-380 nm;
[0010] (4) Mix polyvinyl alcohol, sodium polystyrene sulfonate and deionized water, stir at 90°C for 1-2h, cool and degas, and electrospin to obtain material A; the electrospinning refers to using an electrospinning machine to perform electrospinning at a temperature of 23-27°C and a humidity of 43-47%, injecting the mixed material of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water into a syringe with a volume of 5mL and a needle diameter of 0.5mm, and continuously spinning for 8-10h under the conditions of a spinning voltage of 17-25kV, a spinning receiving distance of 18-25cm, a liquid supply speed of 1.0-1.5mL / h, and a drum speed of 300-400r / min, and drying at 40°C after spinning;
[0011] (5) placing the material A in a glass air flow dryer containing a glutaraldehyde solution, avoiding direct contact between the material A and the glutaraldehyde solution, controlling the temperature for reaction, and drying to obtain material B;
[0012] (6) Mix the nano calcium carbonate and deionized water, add the material B, perform ultrasonic vibration for 20-30 minutes, and dry to obtain material C;
[0013] (7) adding the modified polyvinyl chloride, material C, antioxidant 1076, and pyrophyllite to a mortar grinder, grinding at 75-80° C. for 30-60 min, cooling to room temperature, and passing through a 200-mesh sieve to obtain a mixed material; adding the mixed material and dioctyl terephthalate to a vacuum grinding mixer, grinding at -0.06 to -0.08 MPa for 20-30 min to obtain a paste;
[0014] (8) The base fabric is glued by a cloth opening machine, with a glue amount of 3-6g / m 2 ; Apply the paste on the base fabric after gluing, the coating amount of the paste is 10-16g / m 2 ; performing drying treatment, the drying temperature is 110° C., and the drying speed is 2-3 m / min; then laying the substrate on the base cloth coated with the paste by a four-roll calender using a calendering method to form a preform; coating the preform with an isocyanate-based water-based polyurethane surface treatment agent for surface treatment, embossing the preform after the surface treatment, the embossing molding temperature is 145° C., cutting, and packaging to obtain the artificial leather;
[0015] The glue used in the gluing treatment is water-based PU glue slurry, which includes water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water, and the mass ratio of the water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water is 100:3:150;
[0016] The waterborne polyurethane dispersion was purchased from Hunan Binghang New Materials Co., Ltd.
[0017] The Bayer 401-70 water-based curing agent was purchased from Wuhan Kanos Technology Co., Ltd.
[0018] The substrate is made of thermoplastic polyurethane elastomer;
[0019] The isocyanate-based waterborne polyurethane surface treatment agent comprises the following components in parts by mass: 100 parts of hydrophilic aliphatic polyisocyanate and 0.25 parts of free isocyanate.
[0020] As a preferred technical solution of the present invention, the dosage ratio of the calcium hydroxide suspension in step (2), the carbon dioxide in step (2), the nitrogen in step (2), the oxalic acid in step (3), and the carbon dioxide in step (3) is 20-30 mL: 0.35-0.40 mol: 0.60-0.65 mol: 12-15 mL: 0.1-0.15 mol.
[0021] As a preferred technical solution of the present invention, in step (4), the dosage ratio of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water is 7-10g:3-4g:100mL.
[0022] As a preferred technical solution of the present invention, in step (5), the dosage ratio of material A and glutaraldehyde solution is 30-50g:100-120mL; the concentration of the glutaraldehyde solution is 2.2-2.5mol / L; the temperature-controlled reaction refers to the reaction at 24-27°C for 4-10h; and the drying refers to drying in an oven at 60°C for 30-40min.
[0023] As a preferred technical solution of the present invention, in step (6), the dosage ratio of the nano-calcium carbonate, deionized water and material B is 2-3 g: 150-200 mL: 1-1.5 mol.
[0024] As a preferred technical solution of the present invention, in step (7), the mass ratio of the modified polyvinyl chloride, material C, antioxidant 1076, pyrophyllite, and dioctyl terephthalate is 60-80:15-25:5-8:4-7:10-15.
[0025] As a preferred technical solution of the present invention, the preparation of the modified polyvinyl chloride includes the following steps: mixing polyvinyl chloride, dipentadienyl bis(25-nitropropene), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate, and extruding and granulating at 225-230°C to obtain the modified polyvinyl chloride.
[0026] As a preferred technical solution of the present invention, the mass ratio of polyvinyl chloride, dipentadienyl bis(250), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate is 100: 0.1-0.2: 0.2-0.3: 0.15-0.2: 0.5-0.8: 20-35.
[0027] A scratch-resistant artificial leather prepared by the preparation method.
[0028] Beneficial effects of the present invention:
[0029] The scratch-resistant artificial leather and preparation method thereof disclosed in the present invention obtains nano calcium carbonate with a large-particle structure in a flake shape, which has a larger specific surface area and a smoother contact surface and can better resist external wear and tear.
[0030] Furthermore, nanofibers are formed by electrospinning polyvinyl alcohol and sodium polystyrene sulfonate, and then a dense network structure is formed by cross-linking, which has good structural stability and rigidity and improves wear resistance.
[0031] Furthermore, the sulfonic acid groups in sodium polystyrene sulfonate form calcium sulfonate with calcium ions, so that the nano-calcium carbonate is evenly distributed on the surface of the nanofibers, increasing the interface stability; at the same time, after the polyvinyl chloride is modified, it has good interface compatibility, so that the formed composite film layer has a higher interface strength and improves the wear resistance. DETAILED DESCRIPTION
[0032] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0033] Example 1
[0034] A method for preparing a wipe-resistant artificial leather comprises the following steps:
[0035] (1) Calcium oxide and deionized water were mixed and stirred at 80° C. for 3 h to prepare a calcium hydroxide suspension with a concentration of 0.65 mol / L;
[0036] (2) placing the calcium hydroxide suspension in a hydrothermal carbonization tabletop reactor, introducing carbon dioxide and nitrogen, and stirring the reaction at 16° C. for 5 min;
[0037] (3) then adding oxalic acid, introducing carbon dioxide, stirring and reacting at 16° C. for 12 min to obtain nano calcium carbonate, wherein the particle size of the nano calcium carbonate is 370 nm;
[0038] (4) Mix polyvinyl alcohol, sodium polystyrene sulfonate and deionized water, stir at 90°C for 1h, cool and degas, and electrospin to obtain material A; the electrospinning refers to using an electrospinning machine to perform electrospinning at a temperature of 23°C and a humidity of 43%, injecting the mixed material of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water into a syringe with a volume of 5mL and a needle diameter of 0.5mm, and continuously spinning for 8h under the conditions of a spinning voltage of 17kV, a spinning receiving distance of 18cm, a liquid supply speed of 1.0mL / h, and a drum speed of 300r / min, and drying at 40°C after spinning;
[0039] (5) placing the material A in a glass air flow dryer containing a glutaraldehyde solution, avoiding direct contact between the material A and the glutaraldehyde solution, controlling the temperature for reaction, and drying to obtain material B;
[0040] (6) Mix the nano calcium carbonate and deionized water, add the material B, perform ultrasonic vibration for 20 minutes, and dry to obtain material C;
[0041] (7) adding the modified polyvinyl chloride, material C, antioxidant 1076, and pyrophyllite to a mortar grinder, grinding at 75° C. for 30 min, cooling to room temperature, and passing through a 200-mesh sieve to obtain a mixed material; adding the mixed material and dioctyl terephthalate to a vacuum grinding mixer, grinding at -0.06 MPa for 20 min, and obtaining a paste;
[0042] (8) The base fabric is glued by a cloth opening machine, and the glue amount is 3g / m 2 ; Apply the paste on the base fabric after gluing, the coating amount of the paste is 10g / m 2 ; drying treatment, the drying temperature is 110 ° C, the drying speed is 2m / min; then the substrate is laid on the base cloth coated with the paste by a four-roll calender using a calendering method to form a preform; an isocyanate-based water-based polyurethane surface treatment agent is applied to the preform for surface treatment, and the preform after the surface treatment is embossed at an embossing molding temperature of 145 ° C, cut, and package to obtain the artificial leather;
[0043] The glue used in the gluing treatment is water-based PU glue slurry, which includes water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water, and the mass ratio of the water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water is 100:3:150;
[0044] The substrate is made of thermoplastic polyurethane elastomer;
[0045] The isocyanate-based waterborne polyurethane surface treatment agent comprises the following components in parts by mass: 100 parts of hydrophilic aliphatic polyisocyanate and 0.25 parts of free isocyanate.
[0046] The dosage ratio of the calcium hydroxide suspension in step (2), the carbon dioxide in step (2), the nitrogen in step (2), the oxalic acid in step (3), and the carbon dioxide in step (3) is 20 mL: 0.35 mol: 0.60 mol: 12 mL: 0.1 mol.
[0047] In step (4), the dosage ratio of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water is 7g:3g:100mL.
[0048] In step (5), the dosage ratio of material A to glutaraldehyde solution is 30 g:100 mL; the concentration of the glutaraldehyde solution is 2.2 mol / L; the temperature-controlled reaction refers to the reaction at 24°C for 4 hours; and the drying refers to drying in an oven at 60°C for 30 minutes.
[0049] In step (6), the dosage ratio of the nano-calcium carbonate, deionized water and material B is 2g:150mL:1mol.
[0050] In step (7), the mass ratio of the modified polyvinyl chloride, material C, antioxidant 1076, pyrophyllite and dioctyl terephthalate is 60:15:5:4:10.
[0051] The preparation of the modified polyvinyl chloride comprises the following steps: polyvinyl chloride, dipentadienyl bis(250-80), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate are mixed, and extruded and granulated at 225° C. to obtain the modified polyvinyl chloride; the mass ratio of the polyvinyl chloride, dipentadienyl bis(250-80), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate is 100:0.1:0.2:0.15:0.5:20.
[0052] Example 2
[0053] A method for preparing a wipe-resistant artificial leather comprises the following steps:
[0054] (1) Calcium oxide and deionized water were mixed and stirred at 80° C. for 3 h to prepare a calcium hydroxide suspension with a concentration of 0.70 mol / L;
[0055] (2) placing the calcium hydroxide suspension in a hydrothermal carbonization tabletop reactor, introducing carbon dioxide and nitrogen, and stirring the reaction at 19° C. for 5.5 min;
[0056] (3) then adding oxalic acid, introducing carbon dioxide, and stirring the mixture at 19° C. for 14 min to obtain nano calcium carbonate, wherein the particle size of the nano calcium carbonate is 375 nm;
[0057] (4) Mix polyvinyl alcohol, sodium polystyrene sulfonate and deionized water, stir at 90°C for 1.5h, cool and degas, and electrospin to obtain material A; the electrospinning refers to using an electrospinning machine to perform electrospinning at a temperature of 25°C and a humidity of 45%, injecting the mixed material of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water into a syringe with a volume of 5mL and a needle diameter of 0.5mm, and continuously spinning for 9h under the conditions of a spinning voltage of 21kV, a spinning receiving distance of 22cm, a liquid supply speed of 1.2mL / h, and a drum speed of 350r / min, and drying at 40°C after spinning;
[0058] (5) placing the material A in a glass air flow dryer containing a glutaraldehyde solution, avoiding direct contact between the material A and the glutaraldehyde solution, controlling the temperature for reaction, and drying to obtain material B;
[0059] (6) Mix the nano calcium carbonate and deionized water, add the material B, perform ultrasonic vibration for 25 minutes, and dry to obtain material C;
[0060] (7) adding the modified polyvinyl chloride, material C, antioxidant 1076, and pyrophyllite to a mortar grinder, grinding at 78° C. for 45 min, cooling to room temperature, and passing through a 200-mesh sieve to obtain a mixed material; adding the mixed material and dioctyl terephthalate to a vacuum grinding mixer, grinding at -0.07 MPa for 25 min, and obtaining a paste;
[0061] (8) The base fabric is glued by a cloth opening machine, and the glue amount is 4.5g / m 2 ; Apply the paste on the base fabric after gluing, the coating amount of the paste is 13g / m 2 ; drying treatment, the drying temperature is 110 ° C, the drying speed is 2.5 m / min; then the substrate is laid on the base cloth coated with the paste by a four-roll calender using a calendering method to form a preform; an isocyanate-based water-based polyurethane surface treatment agent is applied to the preform for surface treatment, and the preform after the surface treatment is embossed at an embossing molding temperature of 145 ° C, cut, and package to obtain the artificial leather;
[0062] The glue used in the gluing treatment is water-based PU glue slurry, which includes water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water, and the mass ratio of the water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water is 100:3:150;
[0063] The substrate is made of thermoplastic polyurethane elastomer;
[0064] The isocyanate-based waterborne polyurethane surface treatment agent comprises the following components in parts by mass: 100 parts of hydrophilic aliphatic polyisocyanate and 0.25 parts of free isocyanate.
[0065] The dosage ratio of the calcium hydroxide suspension in step (2), the carbon dioxide in step (2), the nitrogen in step (2), the oxalic acid in step (3), and the carbon dioxide in step (3) is 25 mL: 0.38 mol: 0.63 mol: 14 mL: 0.13 mol.
[0066] In step (4), the dosage ratio of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water is 8g:3.5g:100mL.
[0067] In step (5), the dosage ratio of material A to glutaraldehyde solution is 40 g:110 mL; the concentration of the glutaraldehyde solution is 2.4 mol / L; the temperature-controlled reaction refers to reaction at 26°C for 8 hours; and the drying refers to drying in an oven at 60°C for 35 minutes.
[0068] In step (6), the dosage ratio of the nano-calcium carbonate, deionized water and material B is 2.5 g: 180 mL: 1.5 mol.
[0069] In step (7), the mass ratio of the modified polyvinyl chloride, material C, antioxidant 1076, pyrophyllite and dioctyl terephthalate is 70:20:6:6:13.
[0070] The preparation of the modified polyvinyl chloride comprises the following steps: polyvinyl chloride, dipentadienyl bis(250-80), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate are mixed, and extruded and granulated at 228° C. to obtain the modified polyvinyl chloride; the mass ratio of the polyvinyl chloride, dipentadienyl bis(250-80), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate is 100:0.15:0.25:0.18:0.7:28.
[0071] Example 3
[0072] A method for preparing a wipe-resistant artificial leather comprises the following steps:
[0073] (1) Calcium oxide and deionized water were mixed and stirred at 80° C. for 3 h to prepare a calcium hydroxide suspension with a concentration of 0.75 mol / L;
[0074] (2) placing the calcium hydroxide suspension in a hydrothermal carbonization tabletop reactor, introducing carbon dioxide and nitrogen, and stirring the reaction at 22° C. for 6 minutes;
[0075] (3) then adding oxalic acid, introducing carbon dioxide, stirring and reacting at 22° C. for 15 min to obtain nano calcium carbonate, wherein the particle size of the nano calcium carbonate is 380 nm;
[0076] (4) Mix polyvinyl alcohol, sodium polystyrene sulfonate and deionized water, stir at 90°C for 2h, cool and degas, and electrospin to obtain material A; the electrospinning refers to using an electrospinning machine to perform electrospinning at a temperature of 27°C and a humidity of 47%, injecting the mixed material of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water into a syringe with a volume of 5mL and a needle diameter of 0.5mm, and continuously spinning for 10h under the conditions of a spinning voltage of 25kV, a spinning receiving distance of 25cm, a liquid supply speed of 1.5mL / h, and a drum speed of 400r / min, and drying at 40°C after spinning;
[0077] (5) placing the material A in a glass air flow dryer containing a glutaraldehyde solution, avoiding direct contact between the material A and the glutaraldehyde solution, controlling the temperature for reaction, and drying to obtain material B;
[0078] (6) Mix the nano calcium carbonate and deionized water, add the material B, ultrasonically vibrate for 30 minutes, and dry to obtain material C;
[0079] (7) adding the modified polyvinyl chloride, material C, antioxidant 1076, and pyrophyllite to a mortar grinder, grinding at 80° C. for 60 min, cooling to room temperature, and passing through a 200-mesh sieve to obtain a mixed material; adding the mixed material and dioctyl terephthalate to a vacuum grinding mixer, grinding at -0.08 MPa for 30 min, and obtaining a paste;
[0080] (8) The base fabric is glued by a cloth opening machine, and the glue amount is 6g / m 2 ; Apply the paste on the base fabric after gluing, the coating amount of the paste is 16g / m 2 ; drying treatment, the drying temperature is 110 ° C, the drying speed is 3m / min; then the substrate is laid on the base cloth coated with the paste by a four-roll calender using a calendering method to form a preform; an isocyanate-based water-based polyurethane surface treatment agent is applied to the preform for surface treatment, and the preform after the surface treatment is embossed at an embossing molding temperature of 145 ° C, cut, and package to obtain the artificial leather;
[0081] The glue used in the gluing treatment is water-based PU glue slurry, which includes water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water, and the mass ratio of the water-based polyurethane dispersion, Bayer 401-70 water-based curing agent and deionized water is 100:3:150;
[0082] The substrate is made of thermoplastic polyurethane elastomer;
[0083] The isocyanate-based waterborne polyurethane surface treatment agent comprises the following components in parts by mass: 100 parts of hydrophilic aliphatic polyisocyanate and 0.25 parts of free isocyanate.
[0084] The dosage ratio of the calcium hydroxide suspension in step (2), the carbon dioxide in step (2), the nitrogen in step (2), the oxalic acid in step (3), and the carbon dioxide in step (3) is 30 mL: 0.40 mol: 0.65 mol: 15 mL: 0.15 mol.
[0085] In step (4), the dosage ratio of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water is 10g:4g:100mL.
[0086] In step (5), the dosage ratio of material A to glutaraldehyde solution is 50 g:120 mL; the concentration of the glutaraldehyde solution is 2.5 mol / L; the temperature-controlled reaction refers to the reaction at 27°C for 10 hours; and the drying refers to drying in an oven at 60°C for 40 minutes.
[0087] In step (6), the dosage ratio of the nano calcium carbonate, deionized water and material B is 3 g: 200 mL: 1.5 mol.
[0088] In step (7), the mass ratio of the modified polyvinyl chloride, material C, antioxidant 1076, pyrophyllite and dioctyl terephthalate is 80:25:8:7:15.
[0089] The preparation of the modified polyvinyl chloride comprises the following steps: polyvinyl chloride, dipentadienyl bis(250-80), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate are mixed, and extruded and granulated at 230° C. to obtain the modified polyvinyl chloride; the mass ratio of the polyvinyl chloride, dipentadienyl bis(250-80), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate is 100:0.2:0.3:0.2:0.8:35.
[0090] Comparative Example 1
[0091] The difference from Example 1 is the preparation of nano calcium carbonate;
[0092] Calcium oxide and deionized water are mixed and stirred at 80°C for 3 hours to obtain a calcium hydroxide suspension with a concentration of 0.65 mol / L; the calcium hydroxide suspension is placed in a hydrothermal carbonization table reactor, carbon dioxide and nitrogen are introduced, and the reaction is stirred at 16°C for 5 minutes; carbon dioxide is continued to be introduced, and the reaction is stirred at 16°C for 12 minutes to obtain nano calcium carbonate, and the particle size of the nano calcium carbonate is 45 nm; the dosage ratio of the calcium hydroxide suspension, the carbon dioxide introduced for the first time, the nitrogen, and the carbon dioxide introduced for the second time is 20 mL: 0.35 mol: 0.60 mol: 0.1 mol;
[0093] Comparative Example 2
[0094] The difference from Example 1 is the preparation of nano calcium carbonate;
[0095] Calcium oxide and deionized water are mixed, stirred at 80°C for 3 hours to obtain a calcium hydroxide suspension with a concentration of 0.65 mol / L; the calcium hydroxide suspension is placed in a hydrothermal carbonization table reactor, carbon dioxide and nitrogen are introduced, and the reaction is stirred at 40°C for 5 minutes; then oxalic acid is added, carbon dioxide is introduced, and the reaction is stirred at 40°C for 12 minutes to obtain nano calcium carbonate, the particle size of the nano calcium carbonate is 108nm; the concentration of the oxalic acid is 1 mol / L; the dosage ratio of the calcium hydroxide suspension, the carbon dioxide introduced for the first time, the nitrogen, the oxalic acid, and the carbon dioxide introduced for the second time is 20mL: 0.35mol: 0.60mol: 12mL: 0.1mol;
[0096] Comparative Example 3
[0097] The difference from Example 1 is that no nano calcium carbonate is added;
[0098] Comparative Example 4
[0099] The difference from Example 1 is that sodium polystyrene sulfonate is not added.
[0100] Comparative Example 5
[0101] The difference from Example 1 is that the material A is not placed in the glass air flow dryer containing glutaraldehyde solution.
[0102] Comparative Example 6
[0103] The difference from Example 1 is that in step (7), unmodified polyvinyl chloride is used.
[0104] Comparative Example 7
[0105] The difference from Example 1 is that pyrophyllite is not added in step (7).
[0106] Performance Testing
[0107] Abrasion resistance test according to ASTM D 3885-2004;
[0108] The artificial leathers prepared in Examples 1-3 and Comparative Examples 1-7 were tested for wear resistance at a temperature of (20±2)° C. and a relative humidity of (25±4)% according to the above standard. The test results are shown in Table 1.
[0109] Table 1
[0110]
[0111]
[0112] As can be seen from Table 1, the nano-calcium carbonate prepared in Comparative Examples 1-2 has a smaller particle size, resulting in a significant decrease in the wear resistance of the prepared artificial leather; Comparative Example 3 does not add nano-calcium carbonate, which significantly reduces its wear resistance; the nano-calcium carbonate in Comparative Example 4 is in a free state, which reduces its wear resistance; Comparative Example 5 does not undergo a cross-linking reaction, resulting in a decrease in the wear resistance of the prepared artificial leather; Comparative Example 6 does not modify the polyvinyl chloride, resulting in poor interface compatibility, which reduces its wear resistance; Comparative Example 7 does not add pyrophyllite, which significantly reduces its wear resistance; and the friction resistance times measured by Comparative Example 3 and Comparative Example 7 are close, and the wear resistance is poor. This is because the present application enhances the wear resistance of the prepared artificial leather through the synergistic-reinforcement effect of nano-calcium carbonate and pyrophyllite.
[0113] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a wipe-resistant artificial leather, characterized in that: The preparation of the artificial leather comprises the following steps: (1) mixing calcium oxide and deionized water to prepare a calcium hydroxide suspension with a concentration of 0.65-0.75 mol / L; (2) placing the calcium hydroxide suspension in a hydrothermal carbonization tabletop reactor, introducing carbon dioxide and nitrogen, and stirring the reaction at 16-22° C. for 5-6 minutes; (3) then adding oxalic acid and introducing carbon dioxide, maintaining the temperature in step (2) unchanged and continuing to stir and react for 12-15 minutes to obtain nano calcium carbonate, wherein the particle size of the nano calcium carbonate is 370-380 nm; (4) Mix polyvinyl alcohol, sodium polystyrene sulfonate and deionized water, stir at 90° C. for 1-2 h, cool and degas, and electrospin to obtain material A; (5) placing the material A in a glass air flow dryer containing glutaraldehyde solution, controlling the temperature for reaction, and drying to obtain material B; (6) Mix the nano calcium carbonate and deionized water, add the material B, perform ultrasonic vibration for 20-30 minutes, and dry to obtain material C; (7) adding the modified polyvinyl chloride, material C, antioxidant 1076, and pyrophyllite to a mortar grinder, grinding at 75-80° C. for 30-60 min, cooling to room temperature, and passing through a 200-mesh sieve to obtain a mixed material; adding the mixed material and dioctyl terephthalate to a vacuum grinding mixer, grinding at -0.06 to -0.08 MPa for 20-30 min to obtain a paste; (8) applying glue to the base fabric by a fabric opening machine, coating the paste on the glued base fabric, and drying the base fabric; and then laying the substrate on the base fabric coated with the paste by a four-roll calender using a calendering method to form a preform; The preform is subjected to surface treatment, embossing treatment, cutting and packaging to obtain the artificial leather; Preparation of the modified polyvinyl chloride The method comprises the following steps: mixing polyvinyl chloride, dipentadienyl bis(250mg / kg), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate, and extruding and granulating at 225-230°C to obtain the modified polyvinyl chloride; the mass ratio of the polyvinyl chloride, dipentadienyl bis(250mg / kg), maleic anhydride, antioxidant 168, calcium ricinoleate and dioctyl adipate is 100: 0.1-0.2: 0.2-0.3: 0.15-0.2: 0.5-0.8: 20-35.
2. The method for preparing the wipe-resistant artificial leather according to claim 1, characterized in that: The dosage ratio of the calcium hydroxide suspension in step (2), the carbon dioxide in step (2), the nitrogen in step (2), the oxalic acid in step (3), and the carbon dioxide in step (3) is 20-30 mL: 0.35-0.40 mol: 0.60-0.65 mol: 12-15 mL: 0.1-0.15 mol.
3. The method for preparing the wipe-resistant artificial leather according to claim 1, characterized in that: In step (4), the dosage ratio of polyvinyl alcohol, sodium polystyrene sulfonate and deionized water is 7-10g:3-4g:100mL.
4. The method for preparing the wipe-resistant artificial leather according to claim 1, characterized in that: In step (5), the dosage ratio of material A to glutaraldehyde solution is 30-50 g: 100-120 mL; the concentration of the glutaraldehyde solution is 2.2-2.5 mol / L; the temperature-controlled reaction refers to reacting at 24-27° C. for 4-10 h; and the drying refers to drying in an oven at 60° C. for 30-40 min.
5. The method for preparing the scratch-resistant artificial leather according to claim 1, characterized in that: In step (6), the dosage ratio of the nano-calcium carbonate, deionized water and material B is 2-3 g: 150-200 mL: 1-1.5 mol.
6. The method for preparing the scratch-resistant artificial leather according to claim 1, characterized in that: In step (7), the mass ratio of the modified polyvinyl chloride, material C, antioxidant 1076, pyrophyllite and dioctyl terephthalate is 60-80:15-25:5-8:4-7:10-15.
7. A scratch-resistant artificial leather obtained by the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Wear-resistant high-strength polyvinyl chloride insulation sheathing material and preparation method therefor
CN105086205A
Scrubbing-resistant polyurethane water-based surface treating agent
CN108978238A