Preparation method and application of a highly active persulfate oxide type solid superacid catalyst
By preparing a highly active persulfate oxide solid super acid catalyst, the synergistic action of metal and acid sites is used to solve the problems of low activity and high cost in the hydrocracking reaction of existing catalysts, and the high diphenyl ether is achieved Conversion rate and generation of single ring products, suitable for industrial applications.
Patent Information
- Application Number
- CN202410357701.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-27
Smart Images

Figure BDA0004761893860000051 
Figure BDA0004761893860000061 
Figure HDA0004761893870000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a preparation method and application of a highly active persulfate oxide type solid superacid catalyst. Background Art
[0002] Compared with liquid acid catalysts, solid superacid catalysts have the advantages of stronger acidity, stability, reusability and no pollution to the environment, and are environmentally friendly catalysts. However, they are currently mainly used in reactions such as esterification, isomerization, and alkylation, and are less used in the field of hydrocracking.
[0003] Lignin is one of the three main components of lignocellulosic biomass and is the main renewable aromatic biopolymer on earth. It can replace fossil fuels and serve as a raw material for the production of alternative chemicals, materials and biofuels. The structure of lignin contains many CO bonds, mainly including α-O-4, β-O-4 and 4-O-5 bonds. Among them, the 4-O-5 bond has the highest bond energy and is the most difficult to break. Therefore, it is of great significance to select diphenyl ether with a 4-O-5 bond as a lignin model compound for depolymerization. At present, a lot of research has been carried out on the hydrogenation cracking catalysts of lignin and its model compounds, especially metal hydrogenation catalysts. However, transition metal catalysts have poor catalytic effects and low activity. Although precious metal catalysts have high hydrogenation activity, their low yield and high price are not conducive to large-scale industrial applications. Although catalysts prepared using solid superacids as carriers to load metals have been less studied in the field of hydrocracking, their unique acidic characteristics and the synergistic effect between acidic sites and metal active centers also show very high catalytic activity and selectivity in hydrocracking, providing a new idea for the application of solid superacid catalysts in the direction of hydrogenation. Summary of the invention
[0004] One of the purposes of the present invention is to provide a method for preparing a highly active persulfate oxide type solid superacid catalyst, which is simple to prepare and safe to operate.
[0005] The second object of the present invention is to provide a persulfate oxide type solid superacid catalyst prepared by the above preparation method, which does not require the use of precious metals and has high catalytic activity.
[0006] The third object of the present invention is to provide the application of the above-mentioned persulfate oxide type solid superacid catalyst.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] In a first aspect, the present invention provides a method for preparing a highly active persulfate oxide type solid superacid catalyst, comprising the following steps:
[0009] (1) immersing zirconium oxide powder in 0.01-0.015 mol / L ammonium persulfate methanol solution, first ultrasonicating for 10-15 min, then mixing and stirring for 5-7 h; the mass volume ratio of zirconium oxide to ammonium persulfate methanol solution is 1 g:50 mL;
[0010] (2) filtering the mixture obtained in step (1), drying the filter cake, and grinding to obtain a solid powder;
[0011] (3) placing the solid powder obtained in step (2) into a muffle furnace for calcination, and grinding after cooling to obtain S2O8 / ZrO2 solid;
[0012] (4) immersing the S2O8 / ZrO2 solid obtained in step (3) in a nickel precursor aqueous solution and ultrasonicating for 10-15 min;
[0013] (5) adding sodium borohydride to the mixed solution in step (4) for reduction, and then stirring for 5-7 hours;
[0014] (6) Filter by suction, dry the filter cake, and grind to obtain a Ni-S2O8 / ZrO2 solid superacid catalyst.
[0015] Preferably, the drying temperature in step (2) is 100-120° C., and the drying time is 16-20 h.
[0016] Preferably, in step (3), the calcination temperature is 550° C., the calcination time is 3 h, and the heating rate is 10° C. / min.
[0017] Preferably, the nickel precursor in step (4) is selected from nickel nitrate hexahydrate, and the Ni loading amount is 10%.
[0018] Preferably, the drying method in step (6) is vacuum drying, the drying temperature is 110° C., and the drying time is 16-20 hours.
[0019] In a second aspect, the present invention provides a highly active persulfate oxide type solid superacid catalyst prepared by the above-mentioned preparation method. The catalyst has a small metal particle size, high dispersibility, and strong acidity. Through the synergistic effect between the metal site and the acid site, hydrogen can be well adsorbed, activated, and dissociated to form hydrogen free radicals that overflow to the Lewis acid site and attack the O in the diphenyl ether, thereby breaking the CO bond. The reaction is carried out at 180° C. and 1MPa H2 pressure for 2h, and the conversion rate of diphenyl ether can reach 100%.
[0020] In a third aspect, the present invention provides the use of the above-mentioned highly active persulfate oxide-type solid superacid catalyst in the hydrocracking reaction of diphenyl ether.
[0021] The specific application steps include: placing the substrate diphenyl ether, Ni-S2O8 / ZrO2 solid superacid catalyst and isopropanol into a reactor, sealing it, and replacing the air with hydrogen 3-4 times; pressurizing the reactor at 1-2MPa with hydrogen at room temperature; then raising the temperature to 160℃-200℃, and vigorously stirring at 800rpm for 60-120min; after the experiment, naturally cooling the reaction system to room temperature and releasing the pressure; filtering, and obtaining the organic phase by gas chromatography-mass spectrometry and gas phase analysis.
[0022] Preferably, the catalyst is a 10% Ni-S2O8 / ZrO2 catalyst.
[0023] Preferably, the catalyst accounts for 50% of the substrate by mass.
[0024] Preferably, the reaction conditions of the hydrogenation reaction are: 180°C, 1 MPa, and 120 min.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention prepares a Ni-based solid superacid catalyst, which utilizes the synergistic catalytic effect of the metal active center and the acidic component to well control the direct cleavage of the CO bond of diphenyl ether and inhibit the hydrogenation reaction of its aromatic ring, thereby producing more monocyclic target products.
[0027] 2. In the catalyst of the present invention, the metal Ni is highly dispersed on the solid superacid carrier, showing good catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is the XRD spectrum of the catalyst prepared in Example 1 of the present invention;
[0029] Figure 2 is a SEM image of the catalyst prepared in Example 1 of the present invention;
[0030] Figure 3 is an XPS curve diagram of the catalyst prepared in Example 1 of the present invention;
[0031] Figure 4 is the effect of reaction temperature on the hydrogenation conversion of diphenyl ether;
[0032] Figure 5 It is the effect of hydrogen pressure on the hydrogenation conversion of diphenyl ether. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0034] Example 1: Preparation of 10% Ni-S2O8 / ZrO2 Catalyst by NaBH4 Reduction
[0035] Weigh 0.12g of ammonium persulfate (NH4)2S2O8 in a beaker, add 50mL of methanol, ultrasonicate for 10-15min, weigh 1g of commercial ZrO2 powder (particle size of about 200nm) and add it to the beaker, ultrasonicate for 10-15min, then magnetically stir for 5-7h, filter, put the filter cake into an oven and dry it at 110°C overnight, grind it to obtain a solid powder; then put the solid powder into a muffle furnace and roast it at 550°C for 3h with a heating rate of 3°C / min to obtain a single-component solid superacid S2O8 / ZrO2; according to the Ni loading of 10%, weigh 0.2753g of nickel nitrate hexahydrate in a beaker, add 15mL of deionized water, ultrasonicate for 10min, and then weigh 0.5g Add S2O8 / ZrO2 into the beaker and continue ultrasonication for 10 minutes. Then weigh excess sodium borohydride NaBH4 powder and add it into the biscuit for reduction. Then stir magnetically for 5-7 hours. After filtration, put it into a vacuum drying oven at 110°C and dry it overnight. After grinding, 10% Ni-S2O8 / ZrO2 catalyst was obtained.
[0036] like Figure 1 As shown, XRD characterization shows that the diffraction peaks of metallic nickel appear at 2θ of 45.5℃, 53.04℃ and 78.3℃, corresponding to the (111), (200) and (220) crystal planes of Ni, respectively. The intensity of the diffraction peaks is very low and almost unobservable, indicating that the nickel metal is highly dispersed. Particularly obvious diffraction peaks appear at 2θ of 28.2℃, 31.5℃, 34.1℃ and 50.1℃, respectively, belonging to the (-111), (111), (002) and (220) crystal planes of ZrO2.
[0037] like Figure 2 As shown, SEM characterization shows that metal Ni is uniformly coated on the single-component solid superacid carrier, the dispersion is relatively uniform, and the surface morphology of the carrier is relatively rough.
[0038] like Figure 3 As shown, XPS characterization shows that Ni 2p3 / 2 in the 10% Ni-S2O8 / ZrO2 solid superacid catalyst presents corresponding peak intensities at binding energies of 852.4 eV and 856.7 eV, which belong to the metallic state and oxidized state of nickel, respectively.
[0039] Comparative Example 1: Preparation of 10% Ni-S2O8 / ZrO2 Catalyst by H2 Reduction
[0040] The preparation method of S2O8 / ZrO2 is roughly the same as that of Example 1, except for the reduction method: after Ni is loaded onto S2O8 / ZrO2 and dried, the solid powder is calcined at 450°C for 2 h at an argon flow rate of 70 mL / min, and then reduced at 450°C for 2 h at the same flow rate of hydrogen at a heating rate of 15°C / min. After calcination and reduction, it is cooled to room temperature under an argon atmosphere to obtain a 10% Ni-S2O8 / ZrO2 catalyst.
[0041] Example 2: Hydrogenation application of 10% Ni-S2O8 / ZrO2 solid superacid catalyst
[0042] Take the catalytic reaction of diphenyl ether as an example:
[0043] All catalytic reactions were carried out in a 100 mL stainless steel autoclave. In a typical experiment, 0.1 g of reaction substrate (diphenyl ether), catalyst (50 mg) and isopropanol (20 mL) were placed in the reactor. After sealing, the residual air was removed by passing hydrogen three times. Subsequently, the reactor was pressurized to the desired pressure (2 MPa) with hydrogen at room temperature and then the temperature was raised to the desired temperature (180 ° C) and maintained for a certain time (2 h) at a vigorous stirring speed of 800 rpm. After the experiment, the reaction system was naturally cooled to room temperature and the pressure was released. The reaction mixture was filtered to remove the catalyst, and the organic phase obtained was analyzed by gas chromatography-mass spectrometry (GC-MS) and gas phase (GC).
[0044] Table 1 Catalytic performance of catalysts for hydrogenation of diphenyl ether under different reduction methods
[0045]
[0046] Reaction conditions: 0.1 g diphenyl ether, 50 mg catalyst, 20 mL isopropanol, 180 °C, 2 MPa H2, 2 h.
[0047] Table 1 summarizes the results of the hydrogenation reaction of diphenyl ether by 10% Ni-S2O8 / ZrO2 solid superacid catalyst prepared by different reduction methods. Obviously, when no catalyst is added, diphenyl ether is not hydrogenated under the reaction conditions studied; when a single-component S2O8 / ZrO2 catalyst without metal loading is added, diphenyl ether undergoes a weak conversion and the catalytic activity is poor. However, when a 10% Ni-S2O8 / ZrO2 catalyst loaded with metal nickel prepared by different reduction methods is added, the catalytic activity is greatly improved, and the catalytic activities of the two are also different. The catalyst prepared by hydrogen reduction has a conversion rate of 30% for diphenyl ether under the reaction conditions of 180℃, 2MPa H2 and 2h; while the catalyst prepared by sodium borohydride reduction has a conversion rate of 100% for diphenyl ether under the same reaction conditions, and the products obtained are mainly cyclohexane, cyclohexanol and dicyclohexyl ether. At the same time as diphenyl ether is cracked, there are also a lot of aromatic ring hydrogenation products dicyclohexyl ether. It can be seen that after loading metal, the catalytic activity of the catalyst is greatly improved. This is because the increased metal sites promote the adsorption and activation of hydrogen, causing hydrogen to dissociate and generate more active hydrogen, thereby promoting the hydrogenation cracking reaction of diphenyl ether.
[0048] Comparative Example 2: Application of solid superacid catalysts loaded with different transition metals to catalytic hydrogenation of diphenyl ether.
[0049] The following three solid superacid catalysts were prepared by impregnation method using different metal sources including nickel nitrate hexahydrate, cobalt nitrate hexahydrate and copper nitrate trihydrate, namely 10% Ni-S2O8 / ZrO2, 10% Co-S2O8 / ZrO2 and 10% Cu-S2O8 / ZrO2
[0050] In order to screen out which transition metal has the best hydrogenation performance, all catalytic reactions were carried out in a 100mL stainless steel autoclave. In a typical experiment, 0.1g of reaction substrate (diphenyl ether), catalyst (50mg) and isopropanol (20mL) were placed in the reactor. After sealing, the residual air was removed by passing hydrogen 3 times. Subsequently, the reactor was pressurized to the desired pressure (2MPa) with hydrogen at room temperature and then the temperature was raised to the required temperature (180°C), and maintained for a certain time (2h) at a vigorous stirring speed of 800rpm. After the experiment, the reaction system was naturally cooled to room temperature and the pressure was released. The reaction mixture was filtered to remove the catalyst, and the organic phase obtained was analyzed by gas chromatography-mass spectrometry (GC-MS) and gas phase (GC).
[0051] Table 2 Catalytic performance of different transition metal solid superacid catalysts for diphenyl ether hydrogenation
[0052]
[0053] Reaction conditions: 0.1 g diphenyl ether, 50 mg catalyst, 20 mL isopropanol, 180 °C, 2 MPa H2, 2 h.
[0054] The experimental results show that under the same reaction conditions, compared with solid superacid catalysts without metal loading and loaded with copper and cobalt, the catalytic activity of the 10% Ni-S2O8 / ZrO2 catalyst prepared by loading metal nickel has been significantly improved, and the conversion rate of diphenyl ether can be increased from less than 20% to 100%. The products obtained are mainly cyclohexane, cyclohexanol and many aromatic ring hydrogenation products dicyclohexyl ether. In this catalyst system, the catalytic activity of transition metal nickel is higher.
[0055] Example 3: Effect of reaction temperature on diphenyl ether hydrogenation conversion
[0056] Reaction conditions: 0.1 g diphenyl ether, 50 mg catalyst, 20 mL isopropanol, 1 MPa H2, 2 h.
[0057] Depend on Figure 4 It can be seen that the conversion rate of diphenyl ether catalyzed by 10% Ni-S2O8 / ZrO2 catalyst gradually increases with the increase of reaction temperature. At 140℃, the conversion rate is only about 30%. When the temperature reaches 180℃, it increases to 100%, and the temperature continues to rise and remains unchanged. The products are mainly cyclohexane and cyclohexanol. When the temperature exceeds 160℃, cyclohexylphenyl ether disappears in the product, its CO bond breaks, and the cracking product continues to undergo hydrogenation reaction to generate more cyclohexane and cyclohexanol.
[0058] Example 4: Effect of hydrogen pressure on diphenyl ether hydrogenation conversion
[0059] Reaction conditions: 0.1 g diphenyl ether, 50 mg catalyst, 20 mL isopropanol, 180 °C, 2 h.
[0060] Depend on Figure 5 It can be seen that the conversion rate of diphenyl ether catalyzed by 10% Ni-S2O8 / ZrO2 catalyst increases with the increase of hydrogen pressure. At 1MPa H2, the conversion rate reaches a maximum of 100%, and then remains unchanged. The products are mainly cyclohexane, cyclohexanol and some dicyclohexyl ether. When the hydrogen pressure increases from 0.5Mpa to 1MPa, benzene is first hydrogenated to form cyclohexane, and then the CO bond is cracked to form more benzene and phenol. The cracked products are further hydrogenated to form cyclohexane and cyclohexanol.
[0061] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a highly active persulfate oxide type solid superacid catalyst, It is characterized in that The following steps are involved: (1) Immerse zirconium oxide powder in 0.01-0.015 mol / L ammonium persulfate methanol solution, first ultrasonicate for 10-15 min, then mix and stir for 5-7 h; the mass volume ratio of zirconium oxide to ammonium persulfate methanol solution is 1 g:50 mL; (2) filtering the mixture obtained in step (1), drying the filter cake, and grinding to obtain a solid powder; (3) The solid powder obtained in step (2) is placed in a muffle furnace for calcination, and after cooling, is ground to obtain S 2 O 8 / ZrO 2 solid; (4) Substitute the S obtained in step (3) 2 O 8 / ZrO 2 The solid was immersed in the nickel precursor aqueous solution and ultrasonicated for 10-15 min; (5) adding sodium borohydride to the mixed solution in step (4) for reduction, and then stirring for 5-7 hours; (6) Filter, dry the filter cake, and grind to obtain Ni-S 2 O 8 / ZrO 2 Solid superacid catalyst, Ni loading is 10wt%.
2. A method for preparing a highly active persulfate oxide type solid superacid catalyst according to claim 1, It is characterized in that The drying temperature in step (2) is 100-120 o C, drying time is 16-20h.
3. A method for preparing a highly active persulfate oxide type solid superacid catalyst according to claim 1, It is characterized in that The calcination temperature in step (3) is 550 o C, calcination time was 3 h, heating rate was 10 o C / min.
4. A method for preparing a highly active persulfate oxide type solid superacid catalyst according to claim 1, It is characterized in that The nickel precursor in step (4) is selected from nickel nitrate hexahydrate.
5. A method for preparing a highly active persulfate oxide type solid superacid catalyst according to claim 1, It is characterized in that The drying method in step (6) is vacuum drying, and the drying temperature is 110 o C, drying time is 16-20h.
6. A highly active persulfate oxide type solid superacid catalyst, It is characterized in that The method is prepared according to any one of claims 1 to 5.
7. Use of a highly active persulfate oxide type solid superacid catalyst as claimed in claim 6 in the hydrocracking reaction of diphenyl ether.
8. The use according to claim 7, It is characterized in that The specific steps include: substrate diphenyl ether, Ni-S 2 O 8 / ZrO 2 The solid superacid catalyst and isopropanol were placed in a reactor, sealed, and the air was replaced 3-4 times with hydrogen. The reactor was pressurized at 1-2 MPa with hydrogen at room temperature. The temperature was then raised to 160 o C-200 o C, and vigorously stirred at 800 rpm for 60-120 min; after the experiment, the reaction system was naturally cooled to room temperature and the pressure was released; the organic phase was filtered and analyzed by gas chromatography-mass spectrometry and gas phase analysis.
9. The use according to claim 8, It is characterized in that The mass ratio of the catalyst to the substrate is 50%.
10. The use according to claim 8, It is characterized in that The reaction conditions of the hydrogenation reaction are: 180 o C, 1MPa, 120min.