A spray film waterproof material for skin-type waterproof lining and its application

The spray-film waterproofing material that combines powder and liquid materials uses components such as white Portland cement and reactants to solve the problems of slow construction speed and poor durability of existing spray-film waterproofing materials, achieving efficient and stable waterproofing effects. , suitable for tunnel projects.

CN118125763BActive Publication Date: 2024-10-25SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410246727.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2024-10-25
Estimated Expiration
2044-03-05

AI Technical Summary

Technical Problem

Existing spray-film waterproofing materials have problems during the construction process, such as difficulty in deployment, slow construction speed, poor mechanical properties, easy damage and poor durability. Especially in humid environments, they are easy to lose their waterproofing effect.

Method used

The skin-type spray film waterproofing material uses a combination of powder and liquid materials, including white Portland cement, fillers, catalysts and reactants. It forms a closely packed layer of solid particles through spray construction, relying on reactive groups to interact with airborne particles. Moisture reacts and cures, improving waterproof performance and durability.

Benefits of technology

The strength, tensile strength and bonding strength of waterproof materials are significantly improved, the waterproof performance is enhanced, the material remains stable in humid environments, the construction period and preparation costs are reduced, and it is suitable for waterproofing treatment in tunnel projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004726196480000111
    Figure BDA0004726196480000111
Patent Text Reader

Abstract

The present invention discloses a spray film waterproof material for skin-type waterproof lining and its application, which belongs to the technical field of waterproof materials, including powder and liquid; in terms of weight, the powder includes 5-15 parts of white silicate cement, 1-10 parts of filler, 5-15 parts of catalyst and 0.4-1.5 parts of improver; the liquid includes 70-85 parts of reactant, 1-1.5 parts of improver and 40-60 parts of water. The present invention also discloses the application of the spray film waterproof material for skin-type waterproof lining in waterproofing of underground or tunnel projects. The present invention can significantly reduce the construction period, and is convenient for transportation and preparation, has stable performance and is not easy to deteriorate, has a stable waterproof effect, can provide the spraying requirements for the construction of skin-type waterproof lining, and creates conditions for the large-scale use of skin-type waterproof lining structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproof materials for underground and tunnel engineering, and in particular relates to a spray film waterproof material for skin-type waterproof lining and application thereof. Background Art

[0002] Water leakage is crucial to the safety of underground projects. When the tunnel construction is between the application of initial support and the secondary lining, it is necessary to carry out tunnel drainage construction in time. However, at the current construction site, synthetic polymers and polymer modified asphalt waterproofing membranes are still the main waterproofing methods used, but the waterproofing effect is not ideal. Over-excavation and under-excavation are inevitable during tunnel excavation. Synthetic polymers and polymer modified asphalt waterproofing membranes are easily crushed and broken, and the base anchor ends cause puncture and damage to the waterproofing membranes. There is a cavity between the waterproof board and the initial support base, resulting in a loose lining system, easy water leakage from the back, and difficult construction in complex shapes such as joints, and poor durability. The waterproof membrane material is applied to the inner wall of the initial support by spraying. After a certain period of polymerization, the waterproof membrane achieves stable mechanical properties and waterproofing effects. The waterproof membrane material can be tightly attached to the surface of the main body of the project by spraying, making the waterproofing construction more convenient and reliable. Therefore, more and more projects use spraying waterproofing as the waterproof layer of the tunnel.

[0003] For example, Chinese patent application No. 201510162073.5 discloses a two-component spray film waterproof material, the main body of which is a magnesium acrylate monomer solution. This material improves the mechanical strength and waterproofness in a strong alkaline water environment, solves the problem of material deterioration during storage and transportation, and reduces costs. The prior art also includes the use of cross-linking technology and protective colloids to improve the strength, waterproofness and adhesion of the material.

[0004] Spray film waterproofing materials need to be easy to mix and construct. Two-component spray film waterproofing materials can achieve rapid polymerization, but the solution components are complex and difficult to mix, and the solution is difficult to transport. It requires manual spraying, which leads to slow construction speed, poor mechanical properties and bonding strength. Acrylate spray film materials need a humid environment to play a better role. After absorbing water and saturation, the mechanical properties will decrease. As a waterproof layer, it will crack after drying, resulting in the loss of waterproof effect. There are great defects. It is easy to mold when it is saturated with water and cannot maintain its performance for a long time.

[0005] Therefore, how to provide a powdered organic spray waterproof material suitable for skin-type waterproof lining, which is easy to prepare, has strong hydrophobicity, high film-forming quality and strong durability is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a spray film waterproof material for skin-type waterproof lining and its application.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A spray film waterproof material for skin-type waterproof lining, comprising powder material and liquid material;

[0009] In parts by weight, the powder includes 5 to 15 parts of white silicate cement, 5 to 10 parts of filler, 5 to 15 parts of catalyst and 0.4 to 1.5 parts of improver;

[0010] The liquid material comprises 70-85 parts of a reactant, 1-1.5 parts of an improver and 40-60 parts of water.

[0011] Beneficial effects: The amount of white silicate cement added in the present invention can affect the waterproof performance of the sprayed waterproof material. It has high strength after hydration and can support the material skeleton to enhance the strength of the waterproof membrane material. White silicate cement has strong anti-seepage ability and corrosion resistance, and its light color makes it easy to prepare eye-catching waterproof membrane materials.

[0012] The film-forming mechanism of the spray-film waterproof material obtained by the present invention is as follows: after spraying, the solvent in the material components evaporates to form a tightly packed solid particle layer to form a film, which is cured by the reaction of the reactive groups contained in the material with moisture in the air. In this process, the catalyst can catalyze the film-forming and curing process.

[0013] Preferably, the mass ratio of the powder to the liquid is 100:(10-25).

[0014] Preferably, the reactant is a terpolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester.

[0015] Beneficial effect: the reactant in the present invention has anti-saponification performance, is redispersible in water, contains a high ethylene component, enhances the flexibility of the waterproof membrane material, the material is highly hydrophobic, has no effect on rheological properties, improves the elongation at break and tensile strength of the material, and can also improve the bonding strength and waterproof performance of the product. The amount of reactant added shall not be less than 70% of the total mass of the raw material, and the ratio of the reactant to the amount of white silicate cement affects the waterproof performance of the waterproof membrane material.

[0016] Preferably, the filler comprises calcium carbonate and / or fine sand.

[0017] More preferably, the fine sand is 200 mesh quartz sand.

[0018] Beneficial effects: The filler in the present invention is low in cost, abundant in source, stable in nature, water-resistant, and not easy to burn. The fine sand in the present invention can enhance the strength of the waterproof membrane and is a good raw material for reducing production costs.

[0019] Preferably, the catalyst comprises calcium oxide and / or calcium sulfate.

[0020] Beneficial effects: The calcium sulfate in the present invention can play the role of increasing viscosity, improving rheology and improving water resistance. Calcium sulfate can react with the moisture in the waterproof membrane material to form a hardened calcium sulfate hydrate, thereby improving the adhesion and tensile strength of the material, and at the same time reducing the shrinkage rate of the material after expansion. In addition, since calcium sulfate itself has good water resistance and chemical corrosion resistance, it can keep the waterproof membrane stable in a humid environment and extend its service life. The calcium oxide in the present invention reacts with water to form calcium hydroxide. The exothermic catalytic polymerization reaction in the process accelerates the polymerization and curing of the waterproof membrane material into a film, and the expansion does not shrink, and does not affect the performance of the waterproof membrane material.

[0021] Preferably, the improver includes one or any combination of calcium borate, an anti-sagging agent, a powder defoaming agent, and a mildew preventer.

[0022] Preferably, the anti-sagging agent is hydroxypropyl starch ether.

[0023] Preferably, the powder defoamer includes modified polyether defoamer FS-202.

[0024] Preferably, the mildew preventer comprises an epoxy compound, and the epoxy compound is an epoxy resin.

[0025] Beneficial effects: The calcium borate in the present invention is used as a flame retardant. Calcium borate is flame-retardant physically by absorbing heat, and chemically by reacting with oxygen and combustible substances in the flame. It can form a protective layer to wrap and cover the material, reducing the contact between oxygen and heat. At the same time, calcium borate can also play a certain mildew-proof effect. It can change the osmotic pressure of microbial cells, prevent the mold inside the polymer latex powder, and affect the performance of the waterproof membrane material. Hydroxypropyl starch ether can improve the rheological properties of the spray waterproof membrane material, and avoid the insufficient thickness of the waterproof membrane construction and material waste caused by the sagging phenomenon of the material during the spraying process. The powder defoamer can reduce the bubbles introduced by stirring during the material preparation process and improve the strength of the waterproof membrane material. In addition, the oxygen atoms in the epoxy compound molecules have a strong bactericidal effect, thereby playing a good mildew-proof effect.

[0026] A method for preparing a spray film waterproof material for skin-type waterproof lining comprises the following steps:

[0027] (1) mixing the white silicate cement, filler, catalyst and improver to obtain powder;

[0028] (2) After the reactant and the improver are mixed, they are mixed evenly with water and powder to obtain the spray film waterproof material for skin-type waterproof lining.

[0029] The invention discloses an application of a spraying waterproof material for skin-type waterproof lining in waterproofing of underground or tunnel projects.

[0030] Preferably, the application process is carried out by spraying construction using wet spraying equipment.

[0031] Compared with the prior art, the present invention provides a spray film waterproof material for skin-type waterproof lining and its application, which can significantly reduce the construction period, is easy to transport and prepare, has stable performance and is not easy to deteriorate, has a stable waterproof effect, can provide the spraying requirements for skin-type waterproof lining construction, and creates conditions for the large-scale use of skin-type waterproof lining structures. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.

[0034] The embodiment of the present invention discloses a spray film waterproof material for skin-type waterproof lining, including powder material and liquid material;

[0035] In parts by weight, the powder includes 5 to 15 parts of white silicate cement, 5 to 10 parts of filler, 5 to 15 parts of catalyst and 0.4 to 1.5 parts of improver;

[0036] The liquid material comprises 70 to 85 parts of a reactant, 1 to 1.5 parts of an improver and 40 to 60 parts of water. The film-forming mechanism of the spray film waterproof material obtained by the present invention is as follows: after spray filming, the solvent in the material components evaporates to form a tightly packed solid particle layer to form a film, and the reactive groups contained in the material react with moisture in the air to solidify into a film, and in this process, the catalyst can catalyze the film-forming and curing process.

[0037] In a preferred embodiment, the mass ratio of the powder to the liquid is 100:(10-25).

[0038] In a preferred embodiment, the reactant is a terpolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester. The reactant in the present invention has anti-saponification performance, is redispersible in water, contains a relatively high ethylene component, enhances the flexibility of the waterproof membrane material, improves the elongation at break and tensile strength of the material, and can also improve the bonding strength and waterproof performance of the product. The amount of the reactant added shall not be less than 70% of the total mass of the raw material, and the ratio of the reactant to the amount of white silicate cement affects the waterproof performance of the waterproof membrane material.

[0039] In a preferred embodiment, the filler includes calcium carbonate and / or fine sand. More preferably, the fine sand is 200 mesh quartz sand. The filler in the present invention is low in cost, abundant in source, stable in nature, water-resistant, and not easy to burn. The fine sand in the present invention can enhance the strength of the waterproof membrane and is a good raw material for reducing production costs.

[0040] In a preferred embodiment, the catalyst includes calcium oxide and / or calcium sulfate. The calcium sulfate in the present invention can play the role of increasing viscosity, improving rheology and improving water resistance. Calcium sulfate can react with moisture in the waterproof membrane material to form a hardened calcium sulfate hydrate, thereby improving the adhesion and tensile strength of the material, and at the same time reducing the shrinkage rate of the material after expansion. In addition, since calcium sulfate itself has good water resistance and chemical corrosion resistance, it can keep the waterproof membrane stable in a humid environment and extend its service life. The calcium oxide in the present invention reacts with water to form calcium hydroxide. The exothermic catalytic polymerization reaction in the process accelerates the polymerization and curing of the waterproof membrane material into a film, and the expansion does not shrink, and does not affect the performance of the waterproof membrane material.

[0041] In a preferred embodiment, the improver includes one or any combination of calcium borate, an anti-sagging agent, a powder defoaming agent, and an anti-mildew agent.

[0042] In a preferred embodiment, the anti-sagging agent is hydroxypropyl starch ether.

[0043] In a preferred embodiment, the powder defoamer includes modified polyether defoamer FS-202.

[0044] In a preferred embodiment, the mildew inhibitor comprises an epoxy compound, specifically epoxy resin.

[0045] The calcium borate in the present invention is used as a flame retardant. Calcium borate is flame retardant physically by absorbing heat, and chemically by reacting with oxygen and combustible materials in the flame to retard. It can form a protective layer to wrap and cover the material, reduce the contact between oxygen and heat, and calcium borate can play a certain mildew-proof effect. It can change the osmotic pressure of microbial cells, prevent the mold inside the polymer latex powder, and affect the performance of the waterproof film material. Hydroxypropyl starch ether can improve the rheological properties of the spray waterproof film material, and avoid the insufficient thickness of the waterproof film construction and material waste caused by the sagging phenomenon of the material during the spraying process. The powder defoamer can reduce the bubbles introduced by stirring during the material preparation process and improve the strength of the waterproof film material. In addition, the oxygen atoms in the epoxy compound molecules have a strong bactericidal effect, thereby playing a good mildew-proof effect.

[0046] The embodiment of the present invention also discloses a method for preparing a spray film waterproof material for skin-type waterproof lining, comprising the following steps:

[0047] (1) mixing the white silicate cement, filler, catalyst and improver to obtain powder;

[0048] (2) After the reactant and the improver are mixed, they are mixed evenly with water and powder to obtain the spray film waterproof material for skin-type waterproof lining.

[0049] The embodiment of the present invention also provides an application of a spray-film waterproof material for skin-type waterproof lining in waterproofing of underground or tunnel projects.

[0050] In a preferred embodiment, the application process is carried out by spraying construction using wet spraying equipment.

[0051] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources;

[0052] The epoxy resin was purchased from Shandong Hongyu Engineering Technology Co., Ltd., with an epoxide equivalent of 183-200 g eq. -1 , density is 1.16g / cm 3 ;

[0053] The terpolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester was purchased from Wacker (China) Chemical Co., Ltd. 8034H, which has a solid content of 98%.

[0054] Example 1

[0055] A spray film waterproof material for skin-type waterproof lining comprises a liquid component and a powder component, wherein the mixing ratio of the liquid component to the powder component is 100:23 by mass.

[0056] In parts by mass, the liquid material components include 70 parts of terpolymer powder of vinyl acetate, ethylene and higher fatty acid vinyl ester, 60 parts of water, 1 part of hydroxypropyl starch ether, 0.05 parts of modified polyether defoamer FS-202, and 0.05 parts of epoxy resin;

[0057] The powder components include 12 parts of white silicate cement, 7 parts of calcium oxide, 8 parts of calcium sulfate, 2 parts of fine sand, 3.5 parts of calcium carbonate and 1.4 parts of calcium borate.

[0058] A method for preparing a spray film waterproof material for skin-type waterproof lining comprises the following steps:

[0059] (1) mixing white silicate cement, calcium oxide, calcium sulfate, fine sand, calcium carbonate and calcium borate to obtain a powder component;

[0060] (2) Mix vinyl acetate, ethylene and higher fatty acid vinyl ester terpolymer rubber powder, water, hydroxypropyl starch ether, modified polyether defoamer FS-202 and epoxy resin to obtain a liquid component, and then mix it evenly with the powder component to obtain a spray film waterproof material for skin-type waterproof lining. After the mixture is completed, the curing time is 28 days.

[0061] Example 2

[0062] A spray film waterproof material for skin-type waterproof lining comprises a liquid component and a powder component, wherein the mixing ratio of the liquid component to the powder component is 100:20 by mass.

[0063] Calculated by mass, the liquid component includes 75 parts of ternary copolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester, 50 parts of water, 1 part of hydroxypropyl starch ether, 0.05 parts of modified polyether defoamer FS-202, and 0.05 parts of epoxy resin to form a polymer colloid.

[0064] The powder components include 12 parts of white silicate cement, 6 parts of calcium oxide, 6 parts of calcium sulfate, 2 parts of fine sand, 2.5 parts of calcium carbonate, and 1.4 parts of calcium borate.

[0065] A method for preparing a spray film waterproof material for skin-type waterproof lining comprises the following steps:

[0066] (1) mixing white silicate cement, calcium oxide, calcium sulfate, fine sand, calcium carbonate and calcium borate to obtain a powder component;

[0067] (2) Mix vinyl acetate, ethylene and higher fatty acid vinyl ester terpolymer rubber powder, water, hydroxypropyl starch ether, modified polyether defoamer FS-202 and epoxy resin to obtain a liquid component, and then mix it evenly with the powder component to obtain a spray film waterproof material for skin-type waterproof lining. After the mixture is completed, the curing time is 28 days.

[0068] Example 3

[0069] A spray film waterproof material for skin-type waterproof lining comprises a liquid component and a powder component, wherein the mixing ratio of the liquid component to the powder component is 100:17 by mass.

[0070] Calculated by mass, the liquid component includes 80 parts of ternary copolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester, 40 parts of water, 1 part of hydroxypropyl starch ether, 0.05 parts of modified polyether defoamer FS-202, and 0.05 parts of epoxy resin to form a polymer colloid.

[0071] The powder components include 10 parts of white silicate cement, 5 parts of calcium oxide, 5 parts of calcium sulfate, 1 part of fine sand, 1.5 parts of calcium carbonate, and 1.4 parts of calcium borate.

[0072] A method for preparing a spray film waterproof material for skin-type waterproof lining comprises the following steps:

[0073] (1) mixing white silicate cement, calcium oxide, calcium sulfate, fine sand, calcium carbonate and calcium borate to obtain a powder component;

[0074] (2) Mix vinyl acetate, ethylene and higher fatty acid vinyl ester terpolymer rubber powder, water, hydroxypropyl starch ether, modified polyether defoamer FS-202 and epoxy resin to obtain a liquid component, and then mix it evenly with the powder component to obtain a spray film waterproof material for skin-type waterproof lining. After the mixture is completed, the curing time is 28 days.

[0075] Example 4

[0076] A spray film waterproof material for skin-type waterproof lining comprises a liquid component and a powder component, wherein the mixing ratio of the liquid component to the powder component is 100:14 by mass.

[0077] Calculated by mass, the liquid component includes 85 parts of ternary copolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester, 40 parts of water, 1 part of hydroxypropyl starch ether, 0.05 parts of modified polyether defoamer FS-202, and 0.05 parts of epoxy resin to form a polymer colloid.

[0078] The powder components include 10 parts of white silicate cement, 4 parts of calcium oxide, 3 parts of calcium sulfate, 0.5 parts of fine sand, 1 part of calcium carbonate, and 0.4 parts of calcium borate.

[0079] A method for preparing a spray film waterproof material for skin-type waterproof lining comprises the following steps:

[0080] (1) mixing white silicate cement, calcium oxide, calcium sulfate, fine sand, calcium carbonate and calcium borate to obtain a powder component;

[0081] (2) Mix vinyl acetate, ethylene and higher fatty acid vinyl ester terpolymer rubber powder, water, hydroxypropyl starch ether, modified polyether defoamer FS-202 and epoxy resin to obtain a liquid component, and then mix it evenly with the powder component to obtain a spray film waterproof material for skin-type waterproof lining. After the mixture is completed, the curing time is 28 days.

[0082] Comparative Example 1

[0083] A spray film waterproof material for skin-type waterproof lining, which is different from Example 1 only in that the reactant vinyl acetate and ethylene and higher fatty acid vinyl ester ternary copolymer rubber powder is not included. Other raw materials, process steps and parameters are the same as those in Example 1.

[0084] Comparative Example 2

[0085] A spray film waterproof material for skin-type waterproof lining, which is different from Example 1 only in that the addition amount of the reactant vinyl acetate and ethylene and higher fatty acid vinyl ester ternary copolymer rubber powder is 25% (less than 70%).

[0086] Comparative Example 3

[0087] A spray film waterproof material for skin-type waterproof lining, which is different from Example 1 only in that the addition amount of white silicate cement is 50%.

[0088] Technical effects:

[0089] The performance of the materials obtained in each embodiment was tested, and the thickness of the tested coatings was 3 mm, which is actually required for the project. The test results are shown in Table 1.

[0090] Among them, the detection standards in the embodiments of the present invention are as follows:

[0091] The bond strength with concrete refers to GB / T 16777;

[0092] Tensile strength refers to GB / T 528;

[0093] Elongation at break refers to GB / T 23445-2009;

[0094] Waterproofness refers to GB / T16777;

[0095] Flame retardancy refers to DIN 4102-B2.

[0096] Surface drying time refers to GB / T 23446;

[0097] For mildew resistance, refer to GB T 1741-2007.

[0098] Table 1 Material performance test results of each embodiment

[0099]

[0100] It can be seen from the results in Table 1 that the high molecular polymer spray material obtained by the present invention has good waterproof performance and mechanical properties, is easy to use and construct, can be used in dry and humid environments, has good durability, and can be applied to skin-type waterproof lining tunnel waterproofing treatment.

[0101] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A spray film waterproof material for skin-type waterproof lining, characterized in that: Including powder and liquid; In parts by weight, the powder includes 5 to 15 parts of white silicate cement, 1 to 10 parts of filler, 5 to 15 parts of catalyst and 0.4 to 1.5 parts of improver; The liquid material comprises 70-85 parts of a reactant, 1-1.5 parts of an improver and 40-60 parts of water; The mass ratio of the liquid material to the powder material is 100:23 or 100:20 or 100:17 or 100:14; The reactant is a ternary copolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester; The catalyst includes calcium oxide and / or calcium sulfate.

2. The spray film waterproof material for skin-type waterproof lining according to claim 1, characterized in that: The filler includes calcium carbonate and / or fine sand; The fine sand is 200 mesh quartz sand.

3. The spray film waterproof material for skin-type waterproof lining according to claim 1, characterized in that: The improver includes one or any combination of calcium borate, anti-sagging agent, powder defoamer, and mildew inhibitor; The powder defoamer includes modified polyether defoamer FS-202.

4. The spray film waterproof material for skin-type waterproof lining according to claim 3, characterized in that: The anti-sagging agent is hydroxypropyl starch ether.

5. The spray film waterproof material for skin-type waterproof lining according to claim 3, characterized in that: The mildewproofing agent comprises an epoxy compound, and the epoxy compound is an epoxy resin.

6. Application of the spray waterproof material for skin-type waterproof lining as described in any one of claims 1 to 5 in waterproofing of underground or tunnel projects.