A durable high temperature resistant steam enamel powder coating and its preparation method and application
By using silicone modified epoxy resin, o-cresol epoxy resin and other components in powder coatings, combined with aerogel and modified basalt scales, the durability and adhesion of the coating under high-temperature steam environment is solved, and the durability and adhesion of the coating is achieved. It can provide long-lasting high-temperature steam-resistant coating properties and reduce environmental pollution.
Patent Information
- Application Number
- CN202410247149.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-05
AI Technical Summary
The prior art is difficult to develop a powder coating that can exhibit long-lasting high temperature, water resistance and aging resistance in high temperature steam environments, and there are problems of storage instability and environmental pollution.
Using silicone modified epoxy resin, o-cresol epoxy resin, bisphenol A type epoxy resin, aerogel and modified basalt scales and other components, a durable resistance is prepared through specific ratios and processes. Powder coatings of high temperature steam, combined with curing agents and additives to improve the hardness and adhesion of the coating.
The resulting coating showed good durability and adhesion under high temperature steam environment. It was tested without bubbles and cracks after 50 days of steam boiling, and maintained level 0 adhesion. It has a imitation enamel effect and is suitable for steam pipes and replacement. Heaters and other fields.
Smart Images

Figure BDA0004726357460000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin powder coatings, and in particular to a durable high-temperature resistant steam enamel powder coating and a preparation method and application thereof. Background Art
[0002] Powder coating is a coating containing 100% solids, which is applied in powder form to form a coating film. It does not use solvents, reduces pollution, and meets environmental protection requirements. Epoxy resin powder coating is a common powder coating. Its advantages are good adhesion, wear resistance, hardness and chemical resistance. It is widely used in household appliances, building materials, machinery, pipeline industry and other fields. However, for some special application areas, such as pipeline coatings, heat exchangers, and kitchen appliance coatings used in high-temperature steam environments, since the coating surface is often surrounded by high-temperature steam, the coating used in this application field needs to have excellent long-lasting high-temperature steam resistance, water resistance, aging resistance and other properties in order to extend the service life of the coated substrate. Therefore, the development of a powder coating that is durable and resistant to high-temperature steam is an urgent problem to be solved.
[0003] Chinese patent application number 202311622135.7 discloses a high temperature resistant steam powder coating for a micro steam oven, which is prepared from food grade methyl silicone resin, polyester resin, epoxy modified silicone resin, polyether modified siloxane, polyurethane, isocyanate curing agent and other raw materials. However, polyester resin has poor high temperature resistance, polyurethane resin has poor aging resistance, and isocyanate curing agent has strong reactivity, which is easy to react with resin or water in the air during the preparation of the coating, and the resulting coating is not easy to store.
[0004] Chinese patent application number 201010523979.2 discloses a flexible, water vapor-resistant non-stick coating, which is prepared from polyester-modified silicone resin, epoxy resin and other raw materials, but the coating does not include a curing agent, and it is difficult to form a coating with excellent mechanical properties through curing and cross-linking. In addition, the coating contains an organic solvent, which will cause environmental pollution during the manufacturing and use of the coating.
[0005] Chinese patent application number 201310283801.9 discloses a high temperature resistant and water resistant coating for steam pipes and a preparation method thereof. The coating is prepared from raw materials such as boron phenolic resin, water glass and water, and uses water as a dispersion medium. However, boron phenolic resin is difficult to be stably dispersed in water. After the coating is prepared, the boron phenolic resin and inorganic filler will settle. Moreover, boron phenolic resin is not a common film-forming resin in the art. Therefore, the patent is difficult to obtain a coating with good film-forming property and good storage stability.
[0006] The Chinese patent application number 20130447640.2 discloses a special wear-resistant powder coating for anti-corrosion of downhole oil pipes and pumping rods, which is prepared from raw materials such as o-cresol epoxy resin, epoxy resin, and curing agent. The coating has good wear resistance and corrosion resistance, but the high-temperature steam resistance of the coating is not studied, and the patent document does not involve the coating's long-term high-temperature steam resistance.
[0007] The Chinese patent application number 202010920441.9 discloses a black imitation ceramic high temperature resistant powder coating, which is prepared from raw materials such as epoxy resin and curing agent. The obtained coating has a pencil hardness of 6H, a heat resistance of more than 50% of the light retention rate at 260℃*2h, and an application performance that can maintain good adhesion after boiling in boiling water for 1h. However, the heat resistance of the coating still does not meet the requirements of long-term high temperature steam resistance, and the patent document does not involve the long-term high temperature steam resistance of the coating. Summary of the invention
[0008] In order to solve the above problems, the present invention provides a durable high-temperature resistant steam enamel powder coating and its preparation method and application. The powder coating obtained by the present invention has the characteristics of safety, environmental protection, good storage stability, corrosion resistance, high-temperature hydrolysis resistance, and good adhesion. The obtained coating has high hardness and has an enamel-like effect. After being tested by an enamel boiling water erosion resistance experimental device for 50 days (1200 hours), the coating after the test has no bubbles or cracks, and the adhesion of the coating after the test can still reach level 0. The coating obtained by the present invention can be used for surface coating in the fields of steam pipes, heat exchangers, kitchen utensils, household appliances, etc.
[0009] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0010] A durable high temperature resistant steam enamel powder coating comprises the following components by mass percentage:
[0011] 5-25% of organosilicon modified epoxy resin, 10-30% of o-cresol epoxy resin, 20-50% of bisphenol A epoxy resin, 0.5-5% of aerogel, 0.5-10% of modified basalt flakes, 5-20% of curing agent, 0.5-5% of curing accelerator, 1-5% of pigment, 1-10% of filler and 0.5-5% of auxiliary agent. The sum of the weight percentages of the various components is 100%.
[0012] Furthermore, the organosilicon-modified epoxy resin is a reaction product obtained by using bisphenol A epoxy resin and siloxane and / or silicone oil, which can be obtained by a known preparation method. The preparation method can be referred to in the journal article: "Study on Organosilicon-Modified Epoxy Resin for Powder Coatings", Zheng Yaping et al., May 2005.
[0013] The bisphenol A type epoxy resin can be selected from one or more of E12, E-20, E-44, and E-51. The silicone oil can be selected from hydroxy silicone oil or amino silicone oil. The siloxane can be selected from siloxane containing epoxy groups or amino groups.
[0014] The hydroxy silicone oil can be selected from one or more of Shin-Etsu KF-9701, Shin-Etsu X-21-5841, Shandong Dayi DY-107, and Dow Corning PMX-0156. The amino silicone oil can be selected from one or more of Dow Corning OFX-8040 and CM-226.
[0015] The mass proportion of siloxane and / or silicone oil in the organosilicon-modified epoxy resin reaction system can be 10-60%, or 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%.
[0016] Furthermore, the organosilicon-modified epoxy resin can be prepared by reacting hydroxy silicone oil with epoxy resin E-20, bisphenol A, a catalyst and a solvent at 140-200° C. for 1-3 hours; and the weight proportion of hydroxy silicone oil in the reaction raw materials of the organosilicon-modified epoxy resin is 10-60%, the mass proportion of E-20 is 40-70%, the mass proportion of bisphenol A is 2-8%, the mass proportion of the catalyst is 0.1-1%, and the balance is solvent.
[0017] Furthermore, the catalyst is a combination of triphenylphosphine and butyl titanate.
[0018] The o-cresol epoxy resin can be selected from one or more of CNE-202, NPCN-704, CYDCN-200, and EOCN-6850.
[0019] The bisphenol A type epoxy resin can be selected from one or more of E-20, E-12, and E-06.
[0020] The aerogel is one or more of silicon dioxide aerogel, aluminum oxide aerogel, titanium dioxide aerogel, and zirconium dioxide aerogel.
[0021] The modified basalt flakes are basalt flakes with a mesh size of 200-1000 that are surface-modified by a silane coupling agent KH-560.
[0022] The preparation of the modified basalt flakes comprises: adding 1-10 parts by weight of basalt flakes with a particle size of 200-1000 meshes into 30-150 parts by weight of an ethanol aqueous solution containing KH-560, wherein the ethanol aqueous solution is obtained by mixing an ethanol aqueous solution with a concentration of 30-60wt% and KH-560, and the mass concentration of KH-560 in the solution is 2-10wt%, and then stirring at 40-65°C for 5-20h, filtering and drying the solid matter, and crushing it through a 400-1000 mesh sieve to obtain the silane coupling agent KH-560 modified basalt flakes.
[0023] The curing agent is one or more of dicyandiamide, phenolic curing agent and acid anhydride curing agent, and the curing accelerator is 2-methylimidazole.
[0024] The pigment is one or more of titanium dioxide, zinc oxide, and carbon black; the filler is one or more of calcium carbonate, precipitated barium sulfate, mica powder, and kaolin; and the additive is one or more of a leveling agent, a degassing agent, a brightening agent, and benzoin.
[0025] The present invention also provides a method for preparing a durable high temperature resistant steam enamel powder coating, the preparation method comprising the following steps:
[0026] S1: Weigh each raw material component according to weight percentage;
[0027] S2: uniformly mixing the raw material components at high speed to obtain a mixture;
[0028] S3: heating, extruding, tableting, cooling and crushing the mixed material;
[0029] S4: Repeat step S3 1-5 times, sieve, and obtain a finished powder coating.
[0030] The present invention also provides an application of a durable high temperature resistant steam enamel powder coating, which is applied to the surface coating of industrial pipes, heat exchangers, kitchen utensils, household appliances, etc. The application method of the powder coating can be carried out according to the well-known hot melt coating process or cold coating process.
[0031] The present invention has the following beneficial effects:
[0032] The present invention adopts silicone modified epoxy resin with good heat resistance and o-cresol epoxy resin in combination with bisphenol A epoxy resin with good flexibility and adhesion as film-forming resins of powder coatings, effectively balancing the heat resistance of the powder coating film and the adhesion to the substrate. The obtained coating film is subjected to a 50d (1200h) steam boiling test, and the coating film has no bubbles and cracks, and the adhesion can still reach level 0.
[0033] The present invention uses basalt flakes modified by silane coupling agent KH-560 as inorganic filler, which effectively improves the compatibility of basalt flakes with epoxy resin, a film-forming resin, on the one hand. On the other hand, the scaly basalt has a "maze effect" due to the layer structure formed in the coating, which effectively prevents the high-temperature steam from penetrating the coating, thereby improving the durability of the coating to resist high-temperature steam.
[0034] The present invention adds aerogel with low thermal conductivity and high thermal insulation performance to the coating, which effectively improves the thermal insulation performance of the coating and reduces the heat conduction of high-temperature steam to the coating, thereby effectively improving the durability of the coating's resistance to high-temperature steam. Moreover, experimental data proves that the modified basalt flakes and aerogel in the coating of the present invention have a synergistic effect on the coating's durable resistance to high-temperature steam.
[0035] The o-cresol epoxy resin in the coating of the present invention can provide 2.5 times of crosslinking points when cured, and can easily form a three-dimensional structure with a high degree of crosslinking. The silicone-modified epoxy resin has a higher operating temperature. The resin combination in the coating of the present invention forms a three-dimensional structure with a high crosslinking density through a curing reaction with a curing agent. Combined with the high hardness of the inorganic material, the resulting coating has a higher surface hardness. And by adjusting the type and amount of auxiliary agents such as leveling agents, pigments, degassing agents, benzoin, and brighteners, the resulting coating has an enamel-like effect. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with specific embodiments:
[0037] It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are merely used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] For the purpose of simplicity and illustration, the principles of the embodiments are described mainly by reference to examples. In the following description, many specific details are proposed to provide a thorough understanding of the embodiments. However, it is obvious. For those of ordinary skill in the art, these embodiments may not be limited to these specific details in practice. In some instances, known methods and structures are not described in detail to avoid making these embodiments unnecessarily difficult to understand. In addition, all embodiments may be used in combination with each other.
[0039] Example 1
[0040] The mass percentage of each raw material in the powder coating is: 20% of silicone modified epoxy resin, 20% of o-cresol epoxy resin, 28% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0041] Example 2
[0042] The mass percentage of each raw material in the powder coating is: 5% of silicone modified epoxy resin, 30% of o-cresol epoxy resin, 33% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0043] Example 3
[0044] The mass percentage of each raw material in the powder coating is: 25% of silicone modified epoxy resin, 10% of o-cresol epoxy resin, 33% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0045] Comparative Example 1
[0046] The mass percentage of each raw material in the powder coating is: 0% of silicone modified epoxy resin, 20% of o-cresol epoxy resin, 48% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0047] Comparative Example 2
[0048] The mass percentage of each raw material in the powder coating is: 20% of silicone modified epoxy resin, 0% of o-cresol epoxy resin, 48% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0049] Comparative Example 3
[0050] The mass percentage of each raw material in the powder coating is: 30% of silicone modified epoxy resin, 20% of o-cresol epoxy resin, 18% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0051] Comparative Example 4
[0052] The mass percentage of each raw material in the powder coating is: 10% of silicone modified epoxy resin, 40% of o-cresol epoxy resin, 18% of bisphenol A epoxy resin, 2% of aerogel, 5% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0053] Comparative Example 5
[0054] The mass percentage of each raw material in the powder coating is: 20% of organosilicon-modified epoxy resin, 20% of o-cresol epoxy resin, 28% of bisphenol A epoxy resin, 0% of aerogel, 7% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0055] Comparative Example 6
[0056] The mass percentage of each raw material in the powder coating is: 20% of silicone modified epoxy resin, 20% of o-cresol epoxy resin, 28% of bisphenol A epoxy resin, 7% of aerogel, 0% of modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0057] Comparative Example 7
[0058] The mass percentage of each raw material in the powder coating is: 20% of silicone modified epoxy resin, 20% of o-cresol epoxy resin, 28% of bisphenol A epoxy resin, 2% of aerogel, 5% of unmodified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0059] Comparative Example 8
[0060] The mass percentage of each raw material in the powder coating is: 20% of silicone modified epoxy resin, 20% of o-cresol epoxy resin, 28% of bisphenol A epoxy resin, 2% of aerogel, 5% of KH-550 modified basalt flakes, 10% of curing agent, 1% of curing accelerator, 3% of pigment, 8% of filler and 3% of auxiliary agent.
[0061] The preparation method of the organosilicon-modified epoxy resin in the above-mentioned embodiment and comparative example is as follows: it is prepared by reacting Shin-Etsu KF-9701 hydroxy silicone oil with epoxy resin E-20, bisphenol A and catalyst at 160°C for 2.5 hours, and the catalyst is a combination of triphenylphosphine and butyl titanate in a mass ratio of 1:1. Among them, the mass proportion of hydroxy silicone oil in the reaction raw materials of the organosilicon-modified epoxy resin is 25%, the mass proportion of E-20 is 45%, the mass proportion of bisphenol A is 3.5%, the mass proportion of catalyst is 0.5%, and the balance is solvent toluene. The preparation method can refer to the journal literature: "Research on organosilicon-modified epoxy resin for powder coating", Zheng Yaping et al., May 2005.
[0062] In the above embodiments and comparative examples, the o-cresol resin is EOCN-6850; the bisphenol A epoxy resin is E-12; the aerogel is silica aerogel AG-D aerogel, Shenzhen Zhongning Technology Co., Ltd.; the curing agent is a combination of dicyandiamide and a phenolic curing agent, the phenolic curing agent is Dow DEH84, and the mass ratio of the two is 3:1; the curing accelerator is 2-methylimidazole.
[0063] The basalt flakes in the examples and comparative examples were sourced from Baotou Meitu Chemical Co., Ltd., and the powders were screened to a size of 200-400 mesh.
[0064] The modified basalt flakes in Examples 1-3 and Comparative Examples 1-6 are basalt flakes modified with silane coupling agent KH-560, and the preparation method thereof is as follows: 8 parts by mass of 200-400 mesh basalt flakes are added to 80 parts by mass of an ethanol aqueous solution containing KH-560, wherein the solution is a mixture of 45 wt% ethanol aqueous solution and KH-560, and the mass concentration of KH-560 in the solution is 5 wt%, and then the mixture is stirred at 50°C for 12 hours, the solid matter is filtered and dried, and the solid matter is crushed and sieved through a 400 mesh sieve to obtain basalt flakes modified with silane coupling agent KH-560.
[0065] The difference between the preparation methods of the KH-550 modified basalt flakes in the comparative example and the above-mentioned KH-560 modified basalt flakes is the difference in the modifier silane coupling agent, and the other preparation steps are the same.
[0066] The selection of pigment, filler and auxiliary agent components in the above embodiment and the comparative example is the same. The pigment is titanium dioxide; the filler is a combination of precipitated barium sulfate and calcium carbonate, and the mass ratio of the two is 2:1; the auxiliary agent is a combination of BASF Perenol-F 30P silicon-free leveling agent, Clariant wax powder 3910 degassing agent, Huangshan Jinfeng 701 brightener, and Runda LD-5705 benzoin, and the mass ratio of the four is 1:1:1:1.
[0067] The preparation method of the coating in the above embodiment and comparative example comprises the following steps:
[0068] S1: Weigh each raw material component according to weight percentage;
[0069] S2: uniformly mixing the raw material components at high speed to obtain a mixture;
[0070] S3: heating the mixture to 100°C, extruding, tableting, cooling and crushing;
[0071] S4: Repeat step S3 twice, sieve and select particles of 300-500 mesh to obtain a finished powder coating product.
[0072] Performance Test:
[0073] The coatings obtained in Examples 1-3 and Comparative Examples 1-8 were applied to the metal substrates that had been pre-treated by sandblasting by electrostatic spraying. The coatings were sprayed once with a thickness of ≥300 μm, and then cured at 230° C. for 15 min. The application performance indicators of the obtained coatings were tested. The relevant test standards are as follows:
[0074] Adhesion: GB / T9286-2021; Gloss: GB / T5739-2006; Hardness: GB / T5739-2006; Impact resistance: GB / T1732-1993; Heat resistance: GB / T1735-2009, test conditions are 500℃*24h; Salt spray resistance: GB / T1771-2007, test time 480h.
[0075] High temperature steam resistance: QB / T 2590-2003, uses enamel boiling water erosion resistance test equipment to conduct 50d (1200h) steam boiling test, requiring the coating to be free of bubbles and cracks, and the adhesion of the coating after 50d steam boiling test can still reach level 0.
[0076] The test results are as follows:
[0077]
[0078] It can be seen from the above test results that the coatings obtained in Examples 1-3 have good hardness, adhesion, high temperature steam resistance and other properties. Comparative Examples 1 and 2 do not add silicone modified epoxy resin and o-cresol epoxy resin on the basis of Example 1, and adjust the amount of bisphenol A epoxy resin. The hardness, salt spray resistance and high temperature steam resistance of the obtained coatings deteriorate. Comparative Examples 3 and 4 adjust the amount of resin combination on the basis of Example 1, and the adhesion of the obtained coating deteriorates, and the salt spray resistance and high temperature steam resistance of the coating deteriorate. Comparative Examples 5 and 6 do not add aerogel and modified basalt flakes on the basis of Example 1, and increase the amount of modified basalt flakes and aerogels accordingly. The impact resistance, heat resistance, salt spray resistance and high temperature steam resistance of the obtained coatings are significantly deteriorated. It can be seen that aerogel and modified basalt flakes have a synergistic effect on improving the application performance of the coating. In Comparative Example 6, the aerogel content is too high, the film-forming property of the obtained coating is poor, and the cured coating has defects, which leads to poor application performance of the coating. Comparative Example 7 replaces the modified basalt flakes with unmodified basalt flakes on the basis of Example 1. The compatibility of the unmodified basalt flakes with the resin is poor. During the film-forming process, the basalt flakes are easy to agglomerate and it is difficult to play a barrier role, resulting in poor high-temperature steam resistance and salt spray resistance of the coating. From the test results of Comparative Examples 1-4 and Comparative Examples 5-6, it can be seen that the selection of resin combination in powder coatings has the same significant effect on coating performance as aerogel and modified basalt flakes. Comparative Example 8 replaces KH-560 modified basalt flakes with KH-550 modified basalt flakes on the basis of Example 1. The hardness, heat resistance and salt spray resistance of the obtained powder coating are comparable to those of Example 1. However, the gloss and adhesion of the coating are slightly poor, and the high-temperature steam resistance is significantly deteriorated. This is because the dispersion performance of KH-550 modified basalt flakes in the epoxy resin matrix is not as good as that of KH-560 modified basalt flakes, and it is easy to form agglomeration and excessive cross-linking during the curing process of the coating, which leads to defects in the coating formation process and then causes the coating's high temperature steam resistance to deteriorate.
[0079] It can be seen that the selection of each component and its amount in the coating of the present invention is obtained by the inventors after balancing multiple application properties of the coating, and is the result of a lot of experimental work by the inventors.
[0080] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A durable high temperature resistant steam enamel powder coating, characterized in that: The powder coating is composed of the following components by mass percentage: 5-25% of silicone modified epoxy resin, 10-30% of o-cresol epoxy resin, 20-50% of bisphenol A epoxy resin, 0.5-5% of aerogel, 0.5-10% of modified basalt flakes, 5-20% of curing agent, 0.5-5% of curing accelerator, 1-5% of pigment, 1-10% of filler, 0.5-5% of additive, the sum of the weight percentages of each component is 100%; The modified basalt flakes are 200-1000 mesh basalt flakes surface-modified by silane coupling agent KH-560; The organosilicon-modified epoxy resin is a product obtained by reacting bisphenol A epoxy resin with siloxane and / or silicone oil; The o-cresol epoxy resin is one or more of CNE-202, NPCN-704, CYDCN-200, and EOCN-6850; The bisphenol A type epoxy resin is one or more of E-20, E-12, and E-06; The aerogel is one or more of silicon dioxide aerogel, aluminum oxide aerogel, titanium dioxide aerogel, and zirconium dioxide aerogel.
2. The powder coating according to claim 1, characterized in that The curing agent is one or more of dicyandiamide, phenolic curing agent and acid anhydride curing agent.
3. The powder coating according to claim 1, characterized in that The curing accelerator is 2-methylimidazole, and the pigment is one or more of titanium dioxide, zinc oxide, and carbon black.
4. The powder coating according to claim 1, characterized in that The filler is one or more of calcium carbonate, precipitated barium sulfate, mica powder, and kaolin, and the auxiliary agent is one or more of a leveling agent, a degassing agent, a brightening agent, and benzoin.
5. The method for preparing a powder coating according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1: Weigh each raw material component according to weight percentage; S2: uniformly mixing the raw material components at high speed to obtain a mixture; S3: heating, extruding, tableting, cooling and crushing the mixed material; S4: Repeat step S3 1-5 times, sieve, and obtain a finished powder coating.
6. The use of the powder coating according to any one of claims 1 to 4, characterized in that: The powder coating is used for coating industrial pipes, heat exchangers, kitchen utensils, and household appliances.