An asymmetric PP hollow fiber porous membrane for degassing, its preparation method and application
By adding suitable hydrophobic additives to PP hollow fiber membranes and optimizing the internal and external surface structures, the problems of tolerance and degassing rate of PP membranes in wastewater deammoniation applications were solved, achieving efficient and durable degassing effects.
Patent Information
- Application Number
- CN202410003622.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-02
AI Technical Summary
Existing PP hollow fiber membranes have poor resistance in wastewater deammoniation applications, especially the inner surface is easily corroded by acidic or alkaline liquids, resulting in a reduced service life and low degassing rate.
By adding hydrophobic additives with appropriate weight-average molecular weight and proportion to PP material, an asymmetric PP hollow fiber porous membrane is formed. The membrane has suitable pore size and porosity on the inner surface, good hydrophobicity on the outer surface, and combines overall structural tolerance and degassing rate.
It improves the tolerance of hollow fiber membranes to acidic and alkaline environments, extends their service life, and maintains a high degassing rate and efficiency, making it suitable for applications such as wastewater ammonia removal and carbon dioxide capture.
Smart Images

Figure CN118142362B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of membrane materials, and in particular to an asymmetric PP hollow fiber porous membrane for degassing, its preparation method, and its application. Background Technology
[0002] Degassing refers to the process of removing gas from a liquid or solid. Commonly used degassing methods include vacuum degassing, membrane degassing, dissolution degassing, and gas displacement degassing. Membrane degassing utilizes the selective permeability of special membrane materials to separate gases (such as oxygen, carbon dioxide, nitrogen, and ammonia) from liquids or solids. Hollow fiber membranes are fibrous membrane fibers with a self-supporting structure and a hollow interior. Compared to other separation membranes (such as flat sheet membranes), hollow fiber membranes have a smaller diameter, allowing for close packing in the device, resulting in a higher packing density per unit volume and a larger surface area (for gas exchange). Therefore, hollow fiber membranes are widely used in various degassing applications such as ultrapure water degassing, ink degassing, and wastewater ammonia removal.
[0003] Commonly used hollow fiber membrane materials include poly(4-methyl-1-pentene) (PMP) and polypropylene (PP). Membrane fibers prepared from PMP generally have better durability than those made from PP. However, due to the lower crystallinity of PMP compared to PP, PP membrane fibers typically have higher porosity and air permeability. For example, Chinese Patent CN111346519B, "A Method for Preparing an Asymmetric Polyolefin Membrane" (applied by Hangzhou Kebote Filter Material Co., Ltd.), discloses hollow fiber membranes made from PP or PMP, which exhibit good tensile properties and corrosion resistance, making them suitable for degassing applications in inks, photoresists, and electroplating solutions.
[0004] In degassing applications involving inks and electroplating solutions, the outer surface of the hollow fiber membrane is typically in long-term contact with the liquid, while the inner surface is usually degassed under vacuum. The driving force for degassing is the pressure difference across the hollow fiber membrane. However, in some degassing applications where the inner surface of the hollow fiber membrane needs to be in long-term contact with acidic or alkaline liquids, the inner surface is usually in contact with the acidic or alkaline absorbent. The liquid to be removed moves to the inner surface under the influence of the partial pressure difference and gas concentration, and combines with the absorbent to achieve removal. For example, in wastewater ammonia removal applications, the outer surface of the hollow fiber membrane is the ammonia-nitrogen-containing wastewater to be treated, and the inner surface is the acidic absorbent (dilute sulfuric acid). The NH4+ in the ammonia-nitrogen-containing wastewater... +In an alkaline environment, NH3 is converted into a free state. NH3 diffuses through the concentration boundary layer into the hollow fiber membrane. Driven by the partial pressure difference of NH3 across the hollow fiber membrane, NH3 moves to the inner side of the membrane and combines with dilute sulfuric acid, thus achieving NH3 removal. The driving force for degassing is closely related to the NH3 concentration difference across the hollow fiber membrane. Therefore, the hollow fiber membrane usually needs to have a high NH3 permeation rate to ensure that NH3 quickly combines with the acid after passing through the membrane, guaranteeing the continuous progress of the ammonia removal process. Although PMP membrane fibers have good tolerance, their porosity is usually low, resulting in a low permeation rate for gases such as NH3. Therefore, PMP membrane fibers cannot adequately meet the requirements for degassing applications where the inner surface of the hollow fiber membrane needs to be in long-term contact with acidic or alkaline liquids, such as in wastewater ammonia removal.
[0005] Chinese Patent CN103551046A, published by Tianjin Fengyun Water Resources Technology Co., Ltd., discloses a method for preparing a hydrophobic ammonia nitrogen removal membrane using a melt stretching method. The hollow fiber membrane has a wall thickness of 65-75 μm, a pore size of 0.3-0.5 μm, and a porosity of 65%-85%. The membrane fibers prepared from polypropylene exhibit a certain degree of hydrophobicity. Although PP membrane fibers have a higher NH3 permeation rate, which can better meet the requirements for wastewater ammonia removal, their durability is relatively poor compared to PMP. In wastewater ammonia removal applications, both the inner and outer surfaces of the hollow fiber membrane are in prolonged contact with acidic or alkaline liquids. Therefore, in wastewater ammonia removal applications, both the inner and outer surfaces of the hollow fiber membrane are easily corroded by the liquid to be degassed or by acidic or alkaline liquids. However, those skilled in the art often focus more on the durability of the outer surface and neglect the durability of the inner surface. Typically, to ensure the degassing rate during degassing, the inner surface pore size of PP membrane fibers is usually large and the porosity is usually high. For example, in the aforementioned patent, the pore size of the PP membrane fibers is 300-500nm, and its porosity can reach 65%-85%. However, such PP membrane fibers are prone to inner surface erosion in wastewater deammoniation applications, resulting in poor long-term durability of the membrane fibers. Ultimately, this leads to a reduction in the service life of PP membrane fibers in the field of wastewater deammoniation. Therefore, there is an urgent need for a hollow fiber membrane with a high degassing rate, good long-term durability, and suitable for application in the field of wastewater deammoniation. Summary of the Invention
[0006] The purpose of this invention is to provide an asymmetric PP hollow fiber porous membrane for degassing, its preparation method and application. The PP material is hydrophobically treated by using hydrophobic additives with appropriate weight-average molecular weight and proportion, aiming to obtain a hollow fiber porous membrane with high degassing rate, good long-term tolerance and suitable for application in the field of wastewater deammoniation.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: An asymmetric PP hollow fiber porous membrane for degassing includes a main body, one side of which is an inner surface facing the inner cavity, and the other side is an outer surface. The main body has a non-directional tortuous channel, the inner surface has internal degassing pores, and the pore area ratio of the outer surface is not greater than 5%, and the pore area ratio of the outer surface is less than that of the inner surface. The average SEM pore size of the internal degassing pores is 30-150 nm, and the pore area ratio of the inner surface is 10%-40%. The overall porosity of the porous membrane is 20%-65%; the thickness of the porous membrane is 30-75 μm. The polymer constituting the porous membrane includes at least a hydrophobic additive and PP, wherein the weight-average molecular weight of the PP is 100,000 to 600,000 and the molecular weight distribution is 2 to 7. The hydrophobic additive contains only carbon and hydrogen elements and is a pentene-based substance; the weight-average molecular weight of the hydrophobic additive is 50,000-200,000. The hydrophobic additives in the polymer constituting the porous membrane account for 5%-30% of the total polymer mass.
[0008] As is well known, in various degassing applications (such as degassing of ultrapure water, inks, and electroplating solutions), the tolerance of hollow fiber membranes is currently mainly reflected in the structure and properties of the outer surface of the hollow fiber membrane. This is because, in degassing applications such as ultrapure water, inks, and electroplating solutions, the outer surface of the hollow fiber membrane is the side that is in primary contact with the liquid to be degassed, while the inner surface of the hollow fiber membrane is usually used as the vacuum side. Therefore, under normal circumstances, when considering the overall tolerance of hollow fiber membranes, those skilled in the art usually mainly consider the tolerance of the outer surface of the hollow fiber membrane, and rarely consider the tolerance of the inner surface of the hollow fiber membrane.
[0009] Unlike the common degassing applications mentioned above, in wastewater ammonia removal, the outer surface of the hollow fiber membrane is the ammonia-nitrogen-containing wastewater to be treated, while the inner surface is an acidic absorbent (dilute sulfuric acid). This means that during the degassing process of ammonia-nitrogen-containing wastewater, both the inner and outer surfaces of the hollow fiber membrane are in contact with alkaline and acidic liquids. Therefore, the overall durability of the hollow fiber membrane depends on the structure and properties of its inner and outer surfaces. It is well known that PP membrane fibers are relatively more reactive than PMP membrane fibers, and their durability is worse. Furthermore, PP membrane fibers have relatively good crystallinity. Therefore, when PP membrane fibers are prepared using the melt-stretching method, the pore size and overall porosity of the inner surface are generally relatively large. When such PP membrane fibers are applied to wastewater ammonia removal, their inner surface is more susceptible to erosion by solutions such as dilute sulfuric acid due to the pore size and overall porosity, leading to a decrease in the overall durability of the PP membrane fibers.
[0010] As one of the inventive aspects of this invention, by adding hydrophobic additives to the polymer constituting the hollow fiber porous membrane, the overall hydrophobicity of the hollow fiber porous membrane is further improved. This can reduce the surface energy of the hollow fiber porous membrane to a certain extent, making the hollow fiber porous membrane relatively hydrophobic. As a result, in applications such as wastewater deammoniation, the inner surface of the hollow fiber porous membrane can better resist the erosion of solutions such as dilute sulfuric acid, thus giving the inner surface of the hollow fiber porous membrane better resistance.
[0011] However, under normal circumstances, using conventional hydrophobic additives to hydrophobize PP materials can easily lead to the following problems: The poor compatibility between the hydrophobic additive and the PP material may result in uneven mixing, thus failing to effectively improve the overall hydrophobic properties of the PP film fibers. Furthermore, hydrophobic additives are typically non-crystalline substances with relatively poor crystallinity compared to PP materials. Therefore, the addition of hydrophobic additives can negatively impact the crystallinity of the PP material, especially when using melt stretching to prepare PP film fibers. When the crystallization properties are affected, the crystallinity of PP membrane fibers may decrease, ultimately affecting the pore structure of the PP membrane fibers. This may reduce the porosity and pore size of the PP membrane fibers, leading to a decrease in the degassing rate and efficiency. In severe cases, it may also reduce the strength of the PP membrane fibers, affecting their application in degassing. In wastewater ammonia removal applications, we hope that the hollow fiber membrane has a high degassing rate, so that the NH3 generated on the wastewater side can quickly pass through the hollow fiber membrane and combine with dilute sulfuric acid, promoting a good concentration gradient difference on both sides of the hollow fiber membrane.
[0012] As one of the key inventive aspects of this invention, through the selection of suitable hydrophobic additives and suitable PP materials—specifically, using pentenes containing only carbon and hydrogen elements as hydrophobic additives to hydrophobize PP materials—we were pleasantly surprised to find that when the weight-average molecular weight of the PP material is controlled between 100,000 and 600,000, and the molecular weight distribution is controlled between 2 and 7, while the weight-average molecular weight of the hydrophobic additive is controlled within the range of 50,000 to 200,000, combined with the appropriate mass ratio of the hydrophobic additive to the PP material (the hydrophobic additive accounts for 5%-30% of the total polymer mass, where the total polymer mass refers to the sum of the total mass of the hydrophobic additive and the PP material), the compatibility between the PP material and the hydrophobic additive is good (because the hydrophobic additive contains only carbon and hydrogen elements and is a pentene, while the PP material also contains only carbon). The presence of both hydrogen and PP elements, both of which are olefins, indicates similar properties, allowing for good compatibility between the hydrophobic additive and the PP material during the melting process. This results in a more uniform mixing of the hydrophobic additive and the PP material, significantly improving the hydrophobic properties of the inner and outer surfaces of the PP membrane fibers. Furthermore, at this suitable ratio of hydrophobic additive to PP material, we found that the crystallinity of the PP membrane fibers did not decrease significantly as expected, but remained at a relatively good level. Consequently, when stretching the membrane fibers to form pores, we were able to obtain suitable pore sizes and thus ideal pore structures. This resulted in the formation of PP membrane fibers with suitable overall porosity (20%-65%) and suitable internal surface pore structure (SEM average pore size of internal degassing pores is 30-150 nm, and the pore area ratio of the internal surface is 10%-40%).
[0013] Generally, it is believed that degassing rate and tolerance of hollow fiber membranes are relatively mutually exclusive. This is because a high degassing rate often indicates a high pore size and porosity, resulting in a larger gas exchange area and more gas flow channels during degassing. This allows the gas to be degassed to permeate through the hollow fiber membrane relatively quickly, thus manifesting as a high degassing rate. On the other hand, the tolerance of hollow fiber membranes refers to their ability to withstand erosion by corrosive liquids such as the liquid to be degassed. When both the pore size and porosity of the hollow fiber membrane are maintained at a high level, corrosive liquids such as the liquid to be degassed can more easily penetrate the pore structure and enter the interior of the hollow fiber membrane, causing erosion. This results in insufficient tolerance of hollow fiber membranes with such pore size and porosity.
[0014] However, we were pleasantly surprised to find that when PP materials were modified with appropriate hydrophobic additives of suitable weight-average molecular weight and proportion, the PP membrane fibers could possess suitable pore size (SEM average pore size of internal degassing pores is 30-150 nm), pore area ratio of the inner surface (10%-40%), and suitable overall porosity (20%-65%). Under the influence of such suitable pore size, pore area of the inner surface, and suitable overall porosity, the hollow fiber membrane of this invention can exhibit high degassing rate and degassing efficiency. Simultaneously, the hollow fiber membrane with such a membrane pore structure, under the influence of appropriate hydrophobic additives, combined with the external surface... With a pore area not exceeding 5%, a suitable overall porous membrane thickness (30-75 μm), and a non-directional tortuous pathway, the hollow fiber membrane of this invention exhibits high tolerance on both its inner and outer surfaces. This results in the hollow fiber porous membrane demonstrating good long-term tolerance while also possessing high degassing rates and efficiencies. It effectively meets the needs of applications requiring prolonged contact with acidic or alkaline liquids on both the inner and outer surfaces during degassing processes such as ammonia removal and carbon dioxide capture in wastewater (e.g., landfill leachate, industrial wastewater, and chemical industry wastewater), thus generating significant economic value. Furthermore, research has shown that the hollow fiber membrane of this invention is effective in degassing applications where water vapor easily forms and condenses into a liquid film. It significantly alleviates the formation of a liquid film within the hollow fiber membrane and effectively reduces water vapor condensation losses. For example, in ultrapure water applications, it significantly reduces ultrapure water losses during degassing, improving ultrapure water utilization.
[0015] In this invention, the non-directional tortuous pathways refer to randomly oriented groove structures and / or discretely distributed pore structures, and each non-directional tortuous pathway is interconnected; and the fibers forming the porous membrane structure are continuous. It can be understood that "continuous" means that essentially all the fibers are interconnected as a whole and are formed integrally without the need for additional adhesives or the like to connect them. Unless torn by external force, the network of fibers cannot be separated from each other. That is, the porous membrane of this invention is a single-layer membrane structure, rather than a composite membrane structure.
[0016] In this invention, the pore area ratio of the outer surface is no more than 5% means that when observing the outer surface of the hollow fiber membrane with a SEM electron microscope at a magnification of 50,000, the pore structure cannot be observed or only a very small number of pore structures can be observed.
[0017] In this invention, the pore size, pore area ratio, and other characteristics of the inner surface of the hollow fiber membrane can be characterized by scanning electron microscopy (SEM) to obtain a corresponding SEM image. This image is then measured using computer software (such as Matlab, NIS-Elements, etc.) or manually, and the results are calculated accordingly. During membrane fabrication, the pore size and distribution are generally uniform and consistent in the direction perpendicular to the membrane thickness (planar if the membrane is a flat sheet, and perpendicular to the radius if it is a hollow fiber membrane). Therefore, the pore area ratio in a specific region of the corresponding plane can reflect the overall pore area ratio. In actual measurement, the inner surface of the membrane fibers can be characterized using an SEM to obtain the corresponding image. Since the pore size and distribution on the inner surface are generally uniform, a specific area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 100μm 2 (10μm x 10μm) or, the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to determine the pore area ratio and pore size on that area. Perform several tests and take the average value to obtain the pore area ratio and pore size on the inner surface of the membrane. Of course, those skilled in the art can also obtain the above parameters through other measurement methods. The above measurement methods are for reference only.
[0018] The internal degassing pores in this invention may have two morphologies when observed by SEM: one is a relatively regular circular pore, and the other is a pore that is similar to an ellipse. The SEM average pore diameter of the internal degassing pores claimed in this invention specifically refers to the diameter of the relatively regular circular pores and the length of the minor axis of the elliptical pores.
[0019] The thickness of the hollow fiber membrane in this invention can be obtained by characterizing the cross-section of the hollow fiber membrane using SEM electron microscopy, and then measuring it using computer software (such as Matlab, NIS-Elements, etc.) or manually, and performing corresponding calculations.
[0020] In this invention, the weight-average molecular weight of PP and hydrophobic additives refers to the statistical average molecular weight per unit weight, which is obtained by averaging the molecular weight by mass. The weight-average molecular weight can be obtained by GPC (gel permeation chromatography).
[0021] Commonly used porosity testing methods include mercury intrusion porosimetry, density method, and wet-dry membrane weighing method. The overall porosity of the hollow fiber membrane in this invention can be obtained by any of the above testing methods.
[0022] Furthermore, the infrared absorption spectra of the inner and outer surfaces of the porous membrane were tested using the ATR method, and the hydrophobic additive doping coefficient X of the porous membrane was calculated. X=ABS 720 / ABS 1460 ; Among them ABS 720 For porous membranes at a wavenumber of 720 cm⁻¹ -1 The absorption intensity in the vicinity; ABS 1460 For porous membranes at a wavenumber of 1460 cm⁻¹ -1 The absorption intensity in the vicinity; Hydrophobic additive doping coefficient X 内 =ABS 内表面720 / ABS 内表面1460 ; Where X 内 The value range is 0.0005-0.15; preferably 0.001-0.08. ABS 内表面720 For the inner surface of the porous membrane at a wavenumber of 720 cm⁻¹ -1 The absorption intensity in the vicinity; ABS 内表面1460 For the inner surface of the porous membrane at a wavenumber of 1460 cm⁻¹ -1 The absorption intensity in the vicinity.
[0023] This invention utilizes the same hollow fiber membrane for infrared spectroscopy testing using an instrument including, but not limited to, Fourier transform infrared spectrometers. It ensures consistency in factors such as testing pressure and the selection of the testing area for the hollow fiber membrane. The obtained infrared spectra are then processed to eliminate errors (such as baseline calibration) and analyzed using a wavenumber of 720 cm⁻¹. -1 The absorption intensity near the peak (this invention uses peak area to characterize absorption intensity, which is more accurate and objective) is a characteristic absorption peak used to characterize pentene. Its value is related to the amount of hydrophobic additive (the hydrophobic additive is a pentene-like substance containing only hydrocarbons). Generally, the higher the amount of hydrophobic additive, the larger the absorption intensity (peak area) at this point. To ensure a more objective reflection of the doping coefficient of the hydrophobic additive, this invention uses a wavenumber of 1460 cm⁻¹. -1 The absorption intensity (peak area) near the peak is used as the standard peak, due to the wavenumber of 1460 cm⁻¹. -1 The nearby peaks are bending vibration peaks used to characterize the CH structure; their values are relatively stable and show little variation. Ultimately, after further research, a wavenumber of 720 cm⁻¹ was determined to be the optimal value. -1 The absorption intensity (peak area) and wavenumber near 1460 cm⁻¹ -1 The ratio of the absorption intensities (peak areas) in the vicinity can be used to reflect the degree of distribution of hydrophobic additives on different surfaces of the hollow fiber membrane, that is, the hydrophobic additive doping coefficient on the inner and outer surfaces.
[0024] In degassing applications where the inner surface of hollow fiber membranes needs to be in long-term contact with reactive liquids such as acids and alkalis (e.g., ammonia removal from wastewater and carbon dioxide capture), the inner surface typically has more pores than the outer surface to ensure degassing rate and efficiency. This makes the inner surface more susceptible to erosion by these reactive liquids, leading to decreased membrane durability and reduced lifespan, significantly lowering its economic value. This invention addresses this issue by controlling the hydrophobic additive doping coefficient X on the inner surface. 内 Within the range of 0.0005-0.15, preferably 0.001-0.08, the value can reflect the distribution of hydrophobic additives on the inner surface of the hollow fiber membrane to a certain extent, that is, the degree of hydrophobicity of the inner surface of the hollow fiber membrane. This reflects that the inner surface of the hollow fiber membrane has good hydrophobic properties, which on the one hand enables the inner surface of the hollow fiber membrane to have good resistance to the erosion and penetration of active liquids such as acids and alkalis; on the other hand, it also enables the inner surface of the hollow fiber membrane to have good resistance to the formation of liquid films, thereby ensuring the long-term durability of the hollow fiber membrane in the above-mentioned application fields, improving the service life of the hollow fiber membrane, and thus generating higher economic value.
[0025] If X 内 An excessively high concentration of hydrophobic additives on the inner surface of the hollow fiber membrane indicates a high degree of distribution. Since these additives are typically non-crystalline, this could negatively impact the pore structure of the inner surface, potentially affecting the stability of the membrane during degassing and consequently its degassing efficiency. Even if the overall proportion of hydrophobic additives is within a relatively suitable range, a higher concentration can lead to problems. 内 If the value is too high, it means that the distribution of hydrophobic additives in the hollow fiber membrane is relatively uneven, which may also affect the tensile strength and elongation at break of the hollow fiber membrane; if X 内 If the density is too low, it means that the distribution of hydrophobic additives on the inner surface of the hollow fiber membrane is relatively low. Although the inner surface of the hollow fiber membrane still has good hydrophobic properties and tolerance, after long-term erosion by active solutions such as acids and alkalis, the stability and pressure resistance of the pore structure on the inner surface of the hollow fiber membrane during degassing may be affected and decreased, which may affect the degassing efficiency of the hollow fiber membrane.
[0026] Furthermore, the hydrophobic additive doping coefficient X 外 =ABS 外表面720 / ABS 外表面1460 ; Where X 外The value range is 0.001-0.3; preferably 0.005-0.1. ABS 外表面720 For the outer surface of the porous membrane at a wavenumber of 720 cm⁻¹ -1 The absorption intensity in the vicinity; ABS 外表面1460 For the outer surface of the porous membrane at a wavenumber of 1460 cm⁻¹ -1 The absorption intensity in the vicinity.
[0027] As is well known, the outer surface of a hollow fiber membrane is typically in long-term contact with various liquids to be degassed, and is currently the side that those skilled in the art are more concerned with regarding its durability. Furthermore, in applications such as wastewater ammonia removal, the ammonia-nitrogen-containing wastewater that the outer surface is in long-term contact with is generally more corrosive to the outer surface than the dilute sulfuric acid solution that the inner surface is in long-term contact with. Studies have found that the doping coefficient of the hydrophobic additive on the outer surface can be appropriately increased to better enhance its hydrophobic properties, thereby improving the long-term durability of the hollow fiber membrane. However, it is important to note that the doping coefficient of the hydrophobic additive on the outer surface cannot be too high. This is because a high doping coefficient means a high degree of hydrophobic additive distribution on the outer surface. Since the hydrophobic additive is a non-crystalline substance, this may reduce the compressive strength and stability of the hollow fiber membrane's outer surface during degassing, and also affect the overall tensile strength and elongation at break of the hollow fiber membrane. Therefore, this invention controls X... 外 Within the range of 0.001-0.3, preferably 0.005-0.1, studies have found that by having a suitable hydrophobic additive doping coefficient on the outer surface of the hollow fiber membrane, the membrane fiber's tolerance is significantly improved. At the same time, after long-term exposure to the liquid to be removed, the overall degassing efficiency, pressure resistance, tensile strength, and elongation at break of the membrane fiber can still maintain a good level.
[0028] Furthermore, the porous membrane was tested by XRD, and the XRD crystallinity of the porous membrane was 60%-90%; the overall porosity of the porous membrane was 25%-60%; and the thickness of the porous membrane was 40-65 μm.
[0029] This invention uses XRD to test the crystallinity of porous membranes. We were surprised to find that by selecting hydrophobic additives consisting only of hydrocarbon-containing pentenes, although hydrophobic additives are typically non-crystalline while polypropylene (PP) is crystalline, the XRD crystallinity of the porous membrane did not decrease significantly as expected, but remained at a relatively good level (60%-90%). This reflects that by selecting appropriate hydrophobic additives, this invention significantly reduces the impact of adding non-crystalline substances on the crystallinity of the porous membrane. Simultaneously, the appropriate XRD crystallinity of this invention results in hollow fiber porous membranes with good degassing stability and mechanical strength. Combined with the suitable overall porosity (25%-60%) and thickness (40-65 μm) of the porous membrane, this gives the hollow fiber porous membrane a high degassing rate and degassing efficiency. In addition, with such overall porosity and porous membrane thickness, combined with the hydrophobic treatment of hollow fiber porous membranes using hydrophobic additives, hollow fiber porous membranes can exhibit excellent tolerance in degassing applications such as wastewater ammonia removal and carbon dioxide capture, where both the inner and outer surfaces of the hollow fiber membrane need to come into contact with the liquid to be degassed or acidic or alkaline active liquids.
[0030] In this invention, the XRD crystallinity of the porous membrane refers to the XRD diffraction pattern of the porous membrane obtained by X-ray diffraction, and the sum of the diffraction peak areas representing the crystalline form and the diffraction peak areas representing the amorphous form are calculated separately. The XRD crystallinity value of the porous membrane is obtained by the sum of the diffraction peak areas of the crystalline form and the diffraction peak areas of the amorphous form.
[0031] Furthermore, the porous membrane has a full width at half maximum (FWHM) of 0.2-0.7 at a 2θ angle of approximately 14.1°, and the grain size is not less than 150 angstroms.
[0032] This invention uses XRD to test porous membranes and obtain their X-ray diffraction patterns. The diffraction peak near 14.1° (2θ angle) contributes the most to the overall pattern; therefore, it is used as the performance related to the diffraction peak near 14.1° (2θ angle) to characterize the crystallization-related properties of the porous membrane. Half-width at half-maximum (HWHM) refers to the width of each diffraction peak in an XRD diffraction pattern, usually expressed as an angle or a 2θ value. HWHM can be used to measure the variation of lattice parameters in a crystal structure. Generally, a smaller HWHM indicates a more ordered atomic arrangement and fewer crystal defects; a larger HWHM indicates a more disordered atomic arrangement and more crystal defects. Therefore, the HWHM in the XRD pattern can be used to assess the quality and defect level of a crystal. The diffraction peak of this invention at a 2θ angle of approximately 14.1° has a half-width of 0.2-0.7 within a suitable range, and the grain size is not less than 150 angstroms. This means that the more ordered the atomic arrangement and the fewer the crystal defects in the porous membrane crystal of this invention, the easier it is to form pores during the stretching process, and the more stable the pore structure formed. This results in better degassing stability of the porous membrane during degassing. At the same time, the more ordered the atomic arrangement and the fewer the crystal defects, the better the mechanical strength and heat resistance of the porous membrane. In addition, the more ordered the atomic arrangement and the fewer the crystal defects, the better the hollow fiber membrane may be able to maintain good degassing stability and mechanical strength after being subjected to long-term erosion by the liquid to be degassed and / or active liquids such as acids and alkalis. This allows the hollow fiber membrane to still have a high degassing rate and degassing efficiency.
[0033] Furthermore, the water contact angle of the inner surface is 95°-120°, and the roughness Ra of the inner surface is 20-60 μm; and / or; The water contact angle of the outer surface is 100°-130°, and the roughness Ra of the outer surface is 15-70μm.
[0034] The size of the water contact angle depends on the properties of the material itself and the properties of the material surface. The water contact angle of the outer surface of the degassing membrane of this invention is 100°-130°. Generally, the larger the water contact angle, the better the hydrophobicity of the material. This means that the outer surface of the degassing membrane of this invention has good hydrophobicity, and the degassing membrane can have good tolerance and service life when applied to various applications of degassing active liquids such as acidic and alkaline substances. At the same time, the outer surface has a suitable roughness (15-70μm). The roughness can reflect the degree of contact between the outer surface and the gas to be degassed to a certain extent, so that the hollow fiber membrane has a suitable gas permeation rate. Ultimately, the hollow fiber membrane has a high degassing rate and degassing efficiency while also having good tolerance. In addition, due to the presence of a suitable surface roughness and a relatively hydrophobic outer surface, water vapor will encounter greater resistance when it permeates into the hollow fiber membrane through the outer surface, thereby effectively suppressing the permeation rate of water vapor. As a result, the hollow fiber membrane of the present invention can significantly reduce the loss of water vapor evaporation and condensation when applied to degassing fields where water vapor is easily formed and condenses to form a liquid film.
[0035] The hollow fiber membrane of this invention has a water contact angle of 95°-120° on its inner surface and a surface roughness controlled within the range of 20-60 μm. This gives the inner surface of the hollow fiber membrane good hydrophobicity, enabling it to withstand conditions where its inner surface needs to be in long-term contact with acidic or alkaline liquids for degassing (such as ammonia removal from wastewater and carbon dioxide capture), or in degassing applications where water vapor easily forms and condenses into a liquid film. This also effectively inhibits liquid film formation, thereby reducing water vapor evaporation and condensation losses. In carbon dioxide capture applications, the inner surface of the hollow fiber membrane is typically an alkaline solution, used to react with and capture carbon dioxide.
[0036] The water contact angles of the inner and outer surfaces of the hollow fiber membrane in this invention were measured and obtained by Krüger Scientific Instruments (Shanghai) Co., Ltd. using the Williams dynamic contact angle method with a K100 surface tension meter. In the water contact angle test, tools such as glass slides are used to flatten the degassed membrane fibers to form a thin sheet before the water contact angle of the outer surface is tested.
[0037] The roughness of the inner and outer surfaces of the hollow fiber membrane in this invention was measured and obtained using a Keyence 3D scanning microscope.
[0038] Furthermore, some adjacent internal degassing pores are separated by supporting fibers, the SEM average length of the supporting fibers is 50-500nm, and the ratio of the SEM average length of the supporting fibers to the SEM average width of the supporting fibers is 1.5-15:1. The length direction of the supporting fibers is consistent with the circumferential direction of the porous membrane, and the width direction of the supporting fibers is consistent with the length direction of the porous membrane.
[0039] In some degassing applications such as inks, electroplating solutions, and ultrapure water, the inner surface of the hollow fiber membrane is subjected to relatively high gas pressure during degassing. This invention addresses this by forming supporting fibers between some adjacent internal degassing pores. By controlling the SEM average length of the supporting fibers to be 50-500 nm and the ratio of their SEM average length to SEM average width to be within the range of 1.5-15:1, the stability of the internal degassing pores during degassing is enhanced, resulting in better pressure resistance and stability of the inner surface during degassing. Simultaneously, the supporting fibers with a suitable aspect ratio can support and separate the internal degassing pores, improving the stability of the internal degassing zone during degassing. Furthermore, combined with the action of hydrophobic additives, it can also hinder and resist the erosion of the internal degassing pore structure by acidic, alkaline, or other active liquids that come into contact with the inner surface, thereby improving the hollow fiber membrane's resilience.
[0040] If the ratio of the average SEM length to the average SEM width of the supporting fibers is too large, the supporting fibers may become too long and thin, failing to effectively improve the compressive strength and stability of the inner surface during degassing. This could even lead to the supporting fibers breaking under gas pressure or being eroded and broken by reactive liquids such as acids or alkalis, thus negatively impacting the compressive strength and degassing stability of the hollow fiber membrane's inner surface. More seriously, if the supporting fibers break, adjacent internal degassing pores may merge, resulting in excessively large pore sizes, which could also affect the durability of the hollow fiber membrane's inner surface. Conversely, if the ratio of the average SEM length to the average SEM width of the supporting fibers is too small, it means the average SEM length of the supporting fibers is too short. In this case, the presence of the supporting fibers may actually affect the permeation rate of gases such as NH3 in wastewater ammonia removal, O2 in ultrapure water applications, and CO2 in carbon dioxide capture, thus impacting the degassing rate and efficiency of the hollow fiber membrane and hindering efficient and rapid degassing.
[0041] Furthermore, the internal degassing pores are stacked to form an internal degassing zone, and some adjacent internal degassing zones are separated by dense regions. The average SEM width of the internal degassing zone is 80-1200 nm, and the average SEM length of the internal degassing zone is at least 1.5 times the average SEM width of the internal degassing zone. The length of the internal degassing zone is aligned with the circumferential direction of the porous membrane, while the width of the internal degassing zone is aligned with the length of the porous membrane.
[0042] In this invention, the degassing pores on the inner surface are not uniformly distributed, but relatively concentrated in certain areas of the inner surface, which we call the inner degassing zone. That is, there are several inner degassing zones on the inner surface, in which the inner degassing pores are stacked and arranged. Simultaneously, the appropriate pore size (30-150nm) of the inner degassing pores ensures a suitable pore area ratio within the inner degassing zone, thereby ensuring a high overall degassing rate for the hollow fiber membrane. This facilitates efficient degassing, making it particularly suitable for applications requiring high degassing rates, such as ammonia removal from wastewater where NH3 needs to quickly pass through the hollow fiber membrane and combine with dilute sulfuric acid. The inner degassing zone is a region on the inner surface of the hollow fiber membrane with a relatively high pore area ratio. It needs to have a certain area (if its area is too small, it will affect the degassing rate of the hollow fiber membrane and thus the degassing efficiency; if its area is too large, it will affect the pressure resistance of the inner surface of the hollow fiber membrane, and may even affect...). (This affects the tensile strength and elongation at break of the hollow fiber membrane, thus influencing the stability of degassing during internal degassing). Through regulation, the average SEM width of the internal degassing zone is controlled to be 80-1200 nm, while the average SEM length of the internal degassing zone is at least 1.5 times its average SEM width. At this point, the area occupied by the internal degassing zone is relatively suitable, which can ensure a high degassing rate and thus high degassing efficiency on the inner surface of the hollow fiber membrane, while minimizing the impact on the compressive strength of the inner surface of the hollow fiber membrane, allowing the internal degassing pores to degas efficiently for a long time. In addition, with the combined effect of a suitable area for the internal degassing zone and a suitable pore size for the internal degassing pores, combined with the increased hydrophobicity of the inner surface brought about by hydrophobic additives, the inner surface of the hollow fiber membrane has a good ability to resist the erosion of active liquids such as acids and alkalis, and at the same time, the inner surface can also effectively inhibit the formation of liquid films after water vapor condenses.
[0043] Furthermore, the internal degassing pores include a plurality of elliptical air pores, the average major axis of the air pores being 100-600 nm according to SEM, the ratio of the average major axis of the air pores to the average pore diameter of the air pores being 1.5-10:1, and the ratio of the average pore diameter of the air pores to the average width of the supporting fibers being 1.5-12:1. The major axis of the pores is aligned with the length of the porous membrane.
[0044] The internal degassing pores in this invention also include several elliptical vents. Compared to the circular shape of the internal degassing pores, the elliptical vents have a larger area than the circular vents, provided that the minor axis length is the same as the diameter of the circular vents. Therefore, even when the pore size of the internal degassing pores is relatively small, the elliptical vents can still allow the gas to be degassed to pass through relatively well, resulting in a better degassing rate for the hollow fiber membrane. At the same time, the durability of the hollow fiber membrane is also enhanced to some extent as the internal degassing pores decrease in size. In this invention, the average major diameter of the permeable pores is controlled within the range of 100-600 nm using SEM. Combined with the internal degassing pores of suitable size, the appropriate pore area ratio of the inner surface, and the hydrophobic additives, the hollow fiber membrane can achieve a high degassing rate and efficiency. At the same time, the hollow fiber membrane also has good tolerance and can be well applied in some fields where the inner surface of the hollow fiber membrane needs to be in long-term contact with active liquids such as acidic and alkaline substances for degassing (such as ammonia removal from wastewater and carbon dioxide capture), and in some degassing fields where water vapor is easily formed and condenses to form a liquid film.
[0045] Meanwhile, the ratio of the average major axis to the average pore diameter (SEM value) of the vent holes in this invention is controlled within the range of 1.5-10:1. This ensures that although the air permeability area of the elliptical vent holes is effectively increased, the vent holes remain relatively narrow and elongated. In other words, the presence of the elliptical vent holes does not significantly affect the pressure resistance and degassing stability of the inner surface; thus, the inner surface of the degassing membrane still possesses good pressure resistance and degassing stability. By controlling the ratio of the average pore diameter to the average width of the supporting fibers within a suitable range, this invention can further enhance the mechanical strength of the inner surface of the degassing membrane and improve the stability of degassing through the internal degassing pores.
[0046] Furthermore, the average SEM width of the dense region is 60-800nm, and the ratio of the average SEM width of the supporting fiber to the average SEM width of the dense region is 1:4-10. The width of the dense region is aligned with the length of the porous membrane.
[0047] The dense region, to a certain extent, reflects the spacing between adjacent internal degassing regions along the length of the porous membrane. Simultaneously, the dense region serves as the basis for the good resistance of the inner surface. In this invention, the SEM average width of the dense region of the hollow fiber membrane is controlled within the range of 60-800 nm, reflecting a suitable spacing between adjacent internal degassing regions on the inner surface. This ensures a fast degassing rate for the hollow fiber membrane while minimizing the impact of excessively dense distribution of internal degassing regions on the pressure resistance and stability of the inner surface during degassing. Furthermore, the ratio of the SEM average width of the supporting fiber to the SEM average width of the dense region is controlled within the range of 1:4-10. As the solid part within the internal degassing region, the supporting fiber also reflects the resistance and corrosion resistance of the internal degassing region to a certain extent. Studies have shown that when the ratio is controlled within the above range, the hollow fiber membrane exhibits good resistance, and even after prolonged exposure to active liquids such as acids and alkalis, it maintains high degassing efficiency and mechanical strength.
[0048] In this invention, a dense region refers to a region on an inner surface that, when photographed with a scanning electron microscope at 50,000x magnification, has no observable pore structure or only a very small number of pores, and has a pore area ratio of less than 1%.
[0049] Furthermore, the main body includes a skin layer and a support layer, with one side of the support layer being an inner surface and one side of the skin layer being an outer surface. The other side of the skin layer and the other side of the support layer transition through continuous fibers. The support layer contains porous fibers for forming a porous structure, the average SEM diameter of the porous fibers being 30-200 nm, and the density of the porous fibers being 10-300 fibers / μm. 2 .
[0050] The hollow fiber membrane of this invention controls the skin layer and the support layer, combining the appropriate diameter (30-200 nm) and number (10-300 per 1 μm) within the support layer. 2The hollow fiber membrane has good resistance to damage due to the combined action of porous fibers, and at the same time has a high degassing rate and high degassing efficiency. This is because the porosity of the hollow fiber membrane skin is relatively low. Combined with the effect of hydrophobic additives, the resistance when the liquid to be degassed permeates the skin is greatly increased, thus giving the hollow fiber membrane good resilience and ensuring its service life in various degassing applications such as ultrapure water and wastewater ammonia removal. In addition, the porous fibers with such a pore size and density in the support layer give the hollow fiber membrane good pressure resistance and degassing stability of the membrane pore structure in the support layer. Through the combined action of porous fibers of such diameter and number, the support layer has a suitable number of non-directional tortuous pathways, thus giving the degassing membrane a good degassing rate. Although the porosity in the support layer is relatively large, the permeation rate of water vapor in the support layer is still slow under the action of appropriate hydrophobic additives. This is due to the combined effect of porous fibers (hydrophobicity) and tortuous pathways in the hollow fiber membrane. Therefore, hollow fiber membranes can be well applied in degassing fields where water vapor easily forms and condenses to form a liquid film.
[0051] The hollow fiber membrane of the present invention comprises a skin layer and a support layer. Specifically, by observing the cross-sectional structure of the hollow fiber membrane using SEM electron microscopy, it was found that the main structure of the hollow fiber membrane mainly includes two regions. The skin layer refers to a certain region (near the outer surface) where the membrane pore size is very small and the porosity is low. The support layer refers to a certain region (near the inner surface) where the membrane pore size is relatively large and the porosity is relatively high.
[0052] Furthermore, the average diameter variation gradient of the porous fiber under SEM is 0.1-1.2 nm / μm; The gradient of the average SEM diameter of porous fibers = (average SEM diameter of porous fibers near the inner surface - average SEM diameter of porous fibers far from the inner surface) / thickness of the support layer.
[0053] The diameter of the porous fibers within the support layer of this invention is not constant. In some membrane fibers, the porous fibers near the inner surface are relatively thicker, while those farther from the inner surface (closer to the skin layer) are relatively thinner. In this invention, the variation of the average SEM diameter of the porous fibers within the membrane support layer is represented by the gradient of the average SEM diameter of the porous fibers. Therefore, this value is obtained by first subtracting the average SEM diameter of the porous fibers near the inner surface from the average SEM diameter of the porous fibers far from the inner surface, and then dividing this difference by the thickness of the support layer. In this invention, the region far from the inner surface refers to the region within the cross-section of the support layer with a distance of 1 μm from the interface between the skin layer and the support layer as the starting line. In this invention, the region near the inner surface refers to the region within the cross-section of the support layer with a distance of 1 μm from the inner surface as the starting line (inner surface).
[0054] In this invention, the gradient of the average diameter variation of porous fibers directly reflects the trend of a gradual increase in the average diameter of the porous fibers under SEM measurements along the thickness direction of the hollow fiber membrane (from the outer surface to the inner surface). This is because both the inner and outer surfaces of the hollow fiber membrane require a certain compressive strength to maintain stability during degassing. The relatively dense skin structure near the outer surface provides both good compressive strength and good durability. Meanwhile, the relatively large diameter of the porous fibers near the inner surface provides better support for the inner surface. The supporting effect gives the inner surface good compressive strength. On the other hand, when hollow fiber membranes are used in fields where the inner surface of hollow fiber membranes needs to be in long-term contact with acidic, alkaline and other active liquids for degassing (such as wastewater ammonia removal, carbon dioxide capture, etc.), the distribution of relatively large-diameter porous fibers near the inner surface, combined with the action of hydrophobic additives, enables the inner surface of the hollow fiber membrane to have good resistance. At the same time, even when the inner surface is subjected to long-term erosion by acidic, alkaline and other active liquids, the inner surface of the hollow fiber membrane can still have a good degassing rate and compressive strength.
[0055] Furthermore, the outer surface is a dense surface with a pore area ratio of less than 1%, the skin layer thickness is 0.1-3 μm, and the support layer thickness is at least 29 μm greater than the skin layer thickness.
[0056] The hollow fiber membrane of this invention has a dense outer surface with a pore area ratio of less than 1%, and the skin thickness is controlled within the range of 0.1-3 μm. This allows the outer surface of the hollow fiber membrane to have good durability, enabling it to be used in various applications such as degassing of active solutions. Simultaneously, the outer surface of the hollow fiber membrane has a relatively low gas permeation rate, making it relatively difficult for water vapor to penetrate into the hollow fiber membrane during processes such as ultrapure water degassing, thanks to the dense surface and hydrophobic additives. This reduces the amount of water vapor that can permeate into the membrane. The amount of water vapor inside the hollow fiber membrane greatly reduces the probability of water vapor condensing and forming a liquid film after penetrating into the hollow fiber membrane. On this basis, combined with the internal degassing pores with suitable pore size and suitable pore area ratio on the inner surface of the present invention, and the combined effect of porous fibers with suitable diameter and density (suitable support layer thickness) in the support, the degassing rate of the hollow fiber membrane is not significantly reduced due to the density of the outer surface. Instead, the degassing rate of the hollow fiber membrane still has a suitable numerical range, thereby enabling the hollow fiber membrane to still have a suitable degassing rate and high degassing efficiency.
[0057] The dense surface in this invention specifically refers to the outer surface of the degassing membrane photographed at 50,000x magnification using a scanning electron microscope, where no pore structure can be observed on the outer surface or only a very small number of pores can be observed, and the pore area ratio of the outer surface is less than 1%.
[0058] Furthermore, the outer surface has an external degassing region and an external dense region. The porosity of the external dense region is less than 1%, and the external degassing region has a plurality of external degassing pores. The SEM average pore size of the external degassing pores in the external degassing region is 10-90 nm, and the density of the external degassing pores is 10-80 pores / μm. 2 .
[0059] The hollow fiber membrane of this invention has an external degassing zone and an external dense zone on its outer surface. The external degassing pores are concentrated in the external degassing zone, meaning they are not uniformly distributed on the outer surface. This is achieved by combining the appropriate SEM average pore size (10-90 nm) and the appropriate pore density (10-80 pores / μm) within the external degassing zone. 2Simultaneously, the combined effect of suitable internal degassing pore size (30-150nm) and suitable pore area ratio (10%-40%) on the inner surface of the hollow fiber membrane results in extremely high degassing rate and efficiency. This is likely because the concentrated distribution of external degassing pores in the external degassing zone makes the airflow in the external degassing zone more concentrated, which to some extent makes oxygen and other gas molecules more prone to in-molecular collisions during permeation. This reduces the resistance of oxygen and other gases when permeating through the external degassing pores and reduces the influence of airflow scattering and diffusion, thereby increasing the permeation rate of gases such as NH3 and oxygen. At the same time, due to the existence of the external dense zone (relatively dense with almost no pore structure) and the effect of hydrophobic additives, the outer surface of the hollow fiber membrane has good compressive strength and good tolerance. In short, due to the combined effects of the outer and inner surface pore structures and hydrophobic additives, hollow fiber membranes exhibit extremely high degassing rates and efficiencies, while also possessing good pressure resistance and durability. They are suitable for applications such as wastewater ammonia removal where rapid removal of NH3 (the gas to be removed) is required, and both the inner and outer surfaces of the hollow fiber membrane need to have good durability.
[0060] In this invention, the outer dense region and the outer degassing region specifically refer to the regions with small pore structures and relatively dense regions that can be clearly observed on the outer surface of the hollow fiber membrane by SEM electron microscopy. The pore area ratio of the outer dense region is less than 1%, which means that when the outer dense region is photographed at 50,000x magnification, no pore structure can be observed or only a very small number of pores can be observed.
[0061] Furthermore, the outer surface has a plurality of uniformly distributed external degassing pores, the SEM average pore diameter of which is 10-90 nm, and the density of which is 1-30 pores / 10 μm. 2 .
[0062] The hollow fiber membrane of this invention has uniformly distributed external degassing pores on its outer surface. Compared to hollow fiber membranes with unevenly distributed external degassing pores on their outer surface, the uniformly distributed external degassing pores with suitable pore size (10-90 nm) combined with a suitable external degassing pore density (1-30 pores / 10 μm) are superior. 2With the combined effect of the degassing agent and hydrophobic additives, the outer surface of the hollow fiber membrane can have a relatively low water vapor permeation rate. This is because the density of the external degassing pores on the outer surface of the hollow fiber membrane is relatively low, which means that the spacing between adjacent external degassing pores is relatively large. Combined with the relatively small pore size (10-90nm) of the external degassing pores and the combined effect of the hydrophobic additives, the rate at which water vapor enters the hollow fiber membrane through the external degassing pores is greatly reduced. As a result, the hollow fiber membrane has a high degassing rate and high degassing efficiency, while also having good tolerance. At the same time, it can also prevent water vapor from permeating into the hollow fiber membrane and condensing to form a liquid film layer. It is particularly suitable for degassing applications such as ultrapure water, where water vapor is easily generated and condenses to form a liquid film inside the hollow fiber membrane.
[0063] The uniformly distributed external degassing pores in this invention specifically refer to the fact that, through multiple observations of the outer surface of the hollow fiber membrane using SEM electron microscopy, it can be clearly observed that there are basically no relatively dense areas on the outer surface of the hollow fiber membrane, and the membrane pores are basically uniformly distributed on the outer surface.
[0064] Furthermore, the ammonia removal efficiency of the porous membrane is at least greater than 80%; The O2 permeation rate of the porous membrane is not less than 30 L / (min·bar·0.1m). 2 ); The water evaporation rate of the porous membrane is no higher than 0.1 ml / m. 2 / min; The deoxygenation efficiency of the porous membrane is greater than or equal to 90%.
[0065] The hollow fiber membrane of this invention possesses good tensile strength and elongation at break, and exhibits high ammonia removal efficiency, exceeding 80%, effectively removing NH3 from ammonia-nitrogen-containing wastewater. It also boasts extremely high deoxygenation efficiency, exceeding 90%, effectively removing gases such as dissolved oxygen from ultrapure water. Furthermore, the hollow fiber membrane exhibits a high degassing rate, characterized by the O2 permeation rate. In addition, the hollow fiber membrane has a low water evaporation rate, making it suitable for degassing applications in fields such as ultrapure water where water vapor easily generates and condenses within the hollow fiber membrane to form a liquid film.
[0066] The deoxygenation efficiency of this invention can be achieved by assembling a membrane module using the hollow fiber membrane of this invention as raw material, and connecting the module to the process section and polishing section of the ultrapure water preparation process. Under rated flow conditions, the inlet water temperature is tested at 25 ℃, and the inlet water oxygen concentration should meet the following requirements: the inlet water oxygen concentration of the deoxygenation membrane module in the process section is 6-8 mg / L and the inlet water oxygen concentration of the deoxygenation membrane module in the polishing section is ≤10 μg / L. The absolute vacuum degree is 0.006 MPa, and the nitrogen purging rate is 0.012 times the rated flow rate of the inlet water. The deoxygenation efficiency of the deoxygenation membrane module is tested respectively. In this invention, deoxygenation efficiency is used to represent degassing efficiency, mainly because the oxygen content in ultrapure water has a significant impact on semiconductor applications, and the oxygen content in ultrapure water is generally relatively high.
[0067] The ammonia removal efficiency of this invention can be achieved by assembling a membrane module using the hollow fiber membrane of this invention as raw material, and using the membrane module to degas ammonia-nitrogen-containing wastewater. The ammonia-nitrogen-containing wastewater has a concentration of 1000 ppm, a pH value of 11, a controlled temperature of 35°C, a flow rate of 100 L / hr for the ammonia-nitrogen-containing wastewater, and a flow rate ratio of acid (dilute sulfuric acid with a pH value of 1.5) to ammonia-nitrogen-containing wastewater of 4:1. The concentration of ammonia-nitrogen-containing wastewater before and after degassing is obtained by measuring the ammonia-nitrogen concentration according to the method for determining ammonia nitrogen in HJ 535-2009. Finally, the ammonia removal efficiency is calculated.
[0068] The O2 permeation rate of this invention can be measured using the following method: Under conditions of 25°C, 0.1 bar pressure, and a membrane sample area of 0.1 square meters, one side of the membrane sample is subjected to the test gas (oxygen / carbon dioxide); the test gas (oxygen / carbon dioxide) is supplied into the inner cavity of the hollow fiber membrane; the volumetric flow rate of the gas permeating through the membrane wall is measured using a flow meter (KOFLOC / 4800, Japan); the test is performed three times from inside the membrane to outside, and three times from outside the membrane to inside, and the average value is taken. This average value is the oxygen / carbon dioxide permeation rate of the membrane, expressed in ml / (min·bar·0.1m²). 2 ).
[0069] The water evaporation rate of the present invention can be measured by the following test method: using the hollow fiber membrane of the present invention as raw material, assembling it into a membrane module, connecting the water channel and the module for testing, so that water fills the outer surface of the membrane fibers, controlling the pressure at 0.4 MPa, and after 12 hours, collecting the amount of condensed water after condensation on the vacuum side of the hollow fiber membrane.
[0070] Furthermore, this invention discloses a process for preparing an asymmetric PP hollow fiber porous membrane for degassing, comprising the following steps: S1, spinning, involves blending and melting PP material and hydrophobic additives, then extruding through a die to form a molded product with a hollow inner cavity. The extrusion screw is a special single-screw screw, with a feed section compression ratio of 1.05-1.4 and a mixing section compression ratio of 1.4-2.7. The mixing section includes a mixing thread, and the metering section length / screw diameter is 5-12. The die extrusion temperature is 165-180℃. The melting process includes melting, mixing, and metering steps. The metering temperature is 10-20℃ higher than the die extrusion temperature, and the die length-to-diameter ratio is 2-8. The isotacticity of the PP is not less than 95%. The melt index of the PP raw material is 1~7 g / min@(190℃, 5kg). S2, Pre-crystallization, involves placing the molded product in the air section for pre-crystallization; S3, air-cooled crystallization: the molded product obtained in step S2 is cooled by blowing air in an air atmosphere to obtain nascent fibers; S4, First heat setting, involves heat setting the nascent fibers for the first time and then stretching them. The first heat setting temperature is 80-110℃, and the stretching elongation is 0.5-2%, resulting in a heat-set semi-finished product. S5, cold drawing to form holes: The heat-set semi-finished product is subjected to two cold drawing processes, wherein the ratio of the temperature of the first cold drawing to the temperature of the first heat setting is 1:(2-5), and the cold drawing rate of both cold drawing processes is not higher than 20% / min. The cold drawing rate of the first cold drawing process is less than the cold drawing rate of the second cold drawing process, and a cold-drawn semi-finished product is obtained. The elongation rate of the first cold drawing is 5%-20%, and the elongation rate of the second cold drawing is 10%-30%. S6, hot drawing and hole expansion: The cold-drawn semi-finished product is subjected to two hot drawing and hole expansion processes. The temperature of the two hot drawing processes is 100-120℃, and the hot drawing rate of the two hot drawing processes is not higher than 5% / min. The hot drawing rate of the first hot drawing process is less than the hot drawing rate of the second hot drawing process, so as to obtain the hot-drawn semi-finished product. S7, Secondary heat setting: The hot-drawn semi-finished product undergoes a second heat setting process to obtain a hollow fiber porous membrane.
[0071] Furthermore, in step S2, the temperature of the air section is 40-70℃, and the residence time of the air section is 0.01-0.1s; In step S3, the blowing temperature is 30-70℃ and the blowing speed is 20-80m / min.
[0072] Furthermore, in step S4, the first heat setting time is 20-50 minutes; In step S7, the temperature for the second heat setting is 110-140℃, and the time for the second heat setting is 2-5 minutes.
[0073] Furthermore, in step S5, the cold drawing rate of the first cold drawing is 5-10% / min, the cold drawing rate of the second cold drawing is 15%-20%, and the temperature of the second cold drawing is 0-5℃ higher than that of the first cold drawing. In step S6, the hot stretching rate of the first hot stretch is 0.2-0.8% / min, the hot stretching rate of the second hot stretch is 1.5-2%, the elongation of the first hot stretch is 20%-80%, and the elongation of the second hot stretch is 40%-100%.
[0074] This invention describes a method for preparing porous PP hollow fiber membranes using a melt stretching method. Melt stretching refers to the crystallization of polymer melt under tensile stress during extrusion, resulting in a parallel crystalline structure. The semi-finished product, after heat treatment, separates between the crystals after stretching to form micropores, which are then heat-set to obtain the microporous membrane. However, hydrophobic additives are typically non-crystalline, while polypropylene (PP) is crystalline. While using hydrophobic additives to hydrophobize PP can improve the hydrophobic properties of the resulting membrane fibers, it can also affect the crystallinity of the PP material. This is especially true during the melt stretching process, which may reduce the number of crystal nuclei formed in the PP membrane fibers, thus affecting parameters such as porosity and pore size. Furthermore, there may be compatibility issues between the hydrophobic additives and the PP material, leading to poor mixing during melt stretching and hindering the overall improvement of the hydrophobic properties of the PP membrane fibers.
[0075] Considering the above factors, the hydrophobic additive of this invention is a pentene-based substance (pentene-based substances refer to olefins containing a pentene structure) that only includes carbon and hydrogen elements. Both the pentene-based hydrophobic additive and polypropylene (PP) only include carbon and hydrogen elements, and their properties are similar, which allows the pentene-based hydrophobic additive and PP material to have better compatibility during the melting process. This results in a more uniform mixing of the hydrophobic additive and PP material, which in turn significantly improves the hydrophobic properties of PP film fibers, enabling both the inner and outer surfaces of the PP film fibers to have lower surface energy and stronger hydrophobicity.
[0076] It is expected that the properties of hydrophobic additives and PP can influence and determine the surface properties and microporous structure of hollow fiber membranes to a certain extent. Studies have found that parameters such as the weight-average molecular weight of hydrophobic additives, the weight-average molecular weight of PP, and its molecular weight fraction index all have a significant impact on hollow fiber membranes. Isotacticity refers to the distribution of methyl groups on the polypropylene molecular chain. The isotacticity of the polypropylene raw material in this invention is not less than 95%, meaning that the more regularly the methyl groups on the molecular chain are arranged, the more complete the crystal structure is formed during melt stretching, and the easier it is to obtain an ideal membrane structure. The melt index of the PP material is controlled at 1~7 g / min@(190℃, 5kg), meaning that the PP material has good fluidity after melting. Molecular weight distribution index (MDI) refers to the degree of dispersion of molecular weight. The MDI of the PP material in this invention is controlled within the range of 2-7, meaning that the molecular weight of the PP material is relatively uniform, resulting in good processing stability and mechanical properties. Combined with the control of the weight-average molecular weight of the PP material at 100,000-600,000 and the weight-average molecular weight of the hydrophobic additive at 50,000-200,000, the PP material and hydrophobic additive can be mixed more thoroughly and uniformly during the blending and melting process, which is beneficial for obtaining PP filaments with good hydrophobic properties. Furthermore, by controlling the addition ratio of the hydrophobic additive and PP material within a suitable range (the mass ratio of hydrophobic additive to PP is 1:10-3:7), this invention enables the mixed molten material to have good fluidity. Unexpectedly, the crystallinity of the prepared PP filaments did not decrease significantly as expected, but rather still maintained relatively good crystallinity, allowing for the formation of PP filaments with suitable porosity and membrane pore structure and good hydrophobic properties.
[0077] In this invention, step S1 involves blending PP material and hydrophobic additives, followed by melt extrusion. Under the action of an inert gas as the core liquid, a molded product with inner and outer surfaces is formed. The process begins with melting the PP material and hydrophobic additives (primarily involving conveying, pushing, and preheating the hydrophobic additives and PP material to gradually melt and eventually achieve complete molten state for blending), mixing (primarily involving mixing, compression, and pressurized degassing of the hydrophobic additives and PP material), and metering (primarily involving mixing, melting, and conveying, providing sufficient pressure to maintain uniform raw material temperature and a stable melt flow rate). This invention controls the metering temperature to be 10-20°C higher than the die extrusion temperature. When the molten mixture is extruded through the die, internal heat conduction occurs, lowering its temperature. During the cooling process, the temperature of the inner and outer surfaces becomes more uniform, ensuring a relatively sufficient crystallization process. This, in turn, ensures a relatively stable pore structure in the prepared membrane, which is more conducive to forming a suitable membrane pore structure. As one of the important conditions of the process steps of this invention, the die extrusion temperature is controlled at 165-180℃ during melt extrusion. This is because the hydrophobic additive is a non-crystalline substance with a relatively low glass transition temperature. Controlling the die extrusion temperature to be relatively low allows for more uniform mixing between the hydrophobic additive and the PP material, resulting in relatively suitable fluidity after extrusion, which is beneficial for obtaining an ideal membrane structure. If the die extrusion temperature is too high, it may affect the fluidity of the hydrophobic additive and the uniformity of mixing with PP, thus failing to obtain a hollow fiber membrane structure with relatively hydrophobic and uniform inner and outer surfaces.
[0078] Furthermore, by controlling the die's aspect ratio to 2-8, the macromolecular chains in the molten mixture undergo orientation under shear force during flow. The PP material in the mixture readily forms crystal nuclei, resulting in a suitable degree of crystallinity in the final membrane filaments. This leads to a more stable pore structure and higher tensile strength and elongation at break in the prepared membrane. Simultaneously, the use of inert gas as the core liquid during melt extrusion ensures a relatively uniform thickness in the formed degassed membrane.
[0079] In this process, the present invention controls the extrusion screw to be a special single screw, controls the compression ratio of the feeding section to be 1.05-1.4, and controls the compression ratio of the mixing section to be 1.4-2.7. It should be noted that the "compression ratio" in the present invention refers to the inlet screw groove depth / outlet screw groove depth of the section. Generally, a higher compression ratio results in a greater average tensile stress exerted on the melt by the screw, leading to stronger plastic deformation capacity of the melt and thus reducing the stress deformation rate of the molten material during extrusion. Secondly, a higher compression ratio means a smaller screw helical groove volume, increasing the braking and heating effect of the stirring force on the molten material, thereby increasing the temperature of the molten material. This invention, through reasonable control of the compression ratio in the feeding and mixing sections, allows for more uniform mixing of the hydrophobic additive and PP material. Furthermore, the mixing section includes a mixing thread, which allows the screw to exert additional shear force on the molten material, further promoting more uniform mixing between the hydrophobic additive and PP material. The metering section length / screw diameter affects the melting and conveying process of the material. This invention, by controlling the metering section length / screw diameter within the range of 5-12, ensures a suitable residence time of the material within the screw, which is beneficial for the complete melting and mixing of the hydrophobic additive and PP material. This invention, through the rational control of the compression ratio of the feeding section and the mixing section, and the rational selection of the metering section length / screw diameter, combined with the action of the mixing screw, ensures that the hydrophobic additive and PP material can be more evenly distributed during the blending and melting process. As a result, the inner and outer surfaces of the hollow fiber membrane produced have good hydrophobicity, making it suitable for degassing applications such as wastewater ammonia removal and carbon dioxide capture, where the inner and outer surfaces of the hollow fiber membrane need to be in long-term contact with the liquid to be degassed or acidic or alkaline active liquids.
[0080] Based on this, in step S2 of the present invention, the molded product after extrusion through the die head is pre-crystallized in an air section. The temperature and residence time of the air section mainly affect the pore structure and skin structure on the outer surface of the hollow fiber membrane. (When the temperature of the air section is relatively high and the residence time of the air section is relatively long, the outer surface of the degassed membrane also has relatively sufficient time to form crystal nuclei of appropriate size and number. After stretching and pore formation, a certain pore structure is formed on the outer surface. At this time, the thickness of the skin structure will also be relatively small. As the temperature of the air section and the pre-crystallization time decrease, the number of crystal nuclei generated on the outer surface of the hollow fiber membrane gradually decreases, and even crystal nuclei of appropriate size cannot be formed. After stretching and pore formation, a relatively dense membrane pore structure is formed on the outer surface. At this time, the thickness of the skin structure will also be relatively increased.)
[0081] Next, the molded product that has passed through the air section is subjected to air-cooled crystallization. After the pre-crystallization process in the air section, a certain number and size of crystal nuclei are formed inside the molded product. This invention controls the appropriate blowing temperature (30-70℃) and blowing speed (20-80m / min) to form a suitable number and size of crystal nuclei inside the molded product, thereby preparing membrane filaments with ideal membrane structures (that is, by controlling the blowing temperature and blowing speed, and combining the pre-crystallization process in the air section, membrane filaments with different outer surface pore structures can be formed).
[0082] Next, the nascent fibers undergo a first heat setting. As one of the important steps in this invention, a stretching process is performed during the first heat setting, with a stretching elongation of 0.5-2%. By performing a stretching process during the first heat setting and controlling the stretching elongation within the range of 0.5-2%, a certain degree of stretching is achieved within the heat-set semi-finished product. This allows for the formation of a certain number of micro-cracks or pore structures within the heat-set semi-finished product, enabling better stretching of the crystal nuclei and the formation of a more uniform pore structure during the subsequent cold drawing process. If the elongation rate of the first heat setting stretch is too high, it may result in excessive stretching within the heat-set semi-finished product. This could lead to an excessive number and area of microcracks or pore structures, resulting in excessively large pore sizes and porosity in the membrane fibers formed after subsequent cold and hot drawing processes. This could affect the overall durability of the membrane fibers. Conversely, if the elongation rate of the first heat setting stretch is too low, it may prevent the formation of an appropriate number and area of microcracks or pore structures within the heat-set semi-finished product. Consequently, the final membrane fibers may not achieve suitable porosity and pore size.
[0083] It is important to note that the elongation during the first heat-setting stretching process needs to be coordinated with the temperature and time of the first heat-setting. In this invention, the temperature of the first heat-setting is controlled at 80-110℃, and the time is controlled at 20-50 minutes. This is because during the stretching process of the first heat-setting, we hope that the stretching process will result in appropriate stretching within the heat-set semi-finished product to form a certain number and area of tiny cracks or pore structures. However, if the temperature of the first heat-setting is too high or the time is too long, it may lead to the diffusion of the cracks or pore structures formed during the stretching process (too many in number and area). This may result in the pore size of the pore structure formed after the heat-set semi-finished product undergoes cold drawing and hot drawing processes being too large, or the merging of adjacent pore structures, which is undesirable.
[0084] After the first heat setting, the heat-set semi-finished product undergoes a cold drawing process. The main purpose of the cold drawing process is to open up the crystal nuclei inside the heat-set semi-finished product and form a porous structure. This is also one of the more important steps in this invention. This invention performs two cold drawing processes on the heat-set semi-finished product. The ratio of the temperature of the first cold drawing to the temperature of the first heat setting is controlled within the range of 1:(2-5), and the cold drawing rate of both cold drawings is not higher than 20%. The cold drawing rate of the first cold drawing is less than that of the second cold drawing. The elongation of the first cold drawing is 5%-20%, and the elongation of the second cold drawing is 10%-30%. Preferably, the cold drawing rate of the first cold drawing is 5-10% / min, the cold drawing rate of the second cold drawing is 15-20% / min, and the temperature of the second cold drawing is 0-5℃ higher than that of the first cold drawing.
[0085] First, this invention employs a two-stage cold drawing process. This is because after the stretching process in the first heat setting, a certain number of micro-cracks and nascent pore structures will form within the heat-set semi-finished product. By employing a two-stage cold drawing process, this invention enables these micro-cracks and nascent pore structures to be stretched to form pore structures of appropriate size. On the other hand, it also enables the stretching of regions within the heat-set semi-finished product that have a suitable number and size of crystal nuclei (regions that may not have formed micro-cracks or nascent pore structures after the first heat setting stretching process) to form pore structures of appropriate size. This is something that cannot be achieved in a single cold drawing process.
[0086] The first cold drawing process of this invention employs a slow and limited drawing (the first cold drawing rate is controlled at 5-10% / min, and the first cold drawing elongation is 5-20%). It should be noted that "slow drawing" and "fast drawing" here refer to a comparison between the cold drawing rates of the first and second cold drawings, and are not related to the absolute values of the cold drawing rates during the two cold drawings. The cold drawing rates of both cold drawings should not exceed 20% / min. "Slow drawing" and "high drawing" here refer to a comparison between the cold drawing elongation of the first and second cold drawings, and are not related to the absolute values of the cold drawing rates during the two cold drawings. The absolute value of the cold drawing elongation is irrelevant. Furthermore, the ratio of the temperature of the first cold drawing to the temperature of the first heat setting is within the range of 1: (2-5). We found that under such a temperature ratio, combined with the effect of "less drawing" and "slow drawing" in the first cold drawing process, the first cold drawing process can better stretch the micro-cracks and the prototype of the pore structure formed during the first heat setting and stretching process (with a relatively small elongation rate) to form a suitable pore structure. It can also reduce the formation of defective pores to a certain extent (such as the spacing between adjacent pore structures being too close or the occurrence of partial merging).
[0087] After the first cold drawing, the crack or pore structure in the heat-set semi-finished product can be stretched well and form a relatively stable pore structure. However, some areas of the crystal nuclei in the heat-set semi-finished product have not been stretched properly and formed a pore structure. We found that the second cold drawing process, which uses multiple and fast drawing and the second cold drawing temperature is 0-5℃ higher than the first cold drawing temperature, can better open up the crystal nuclei areas that have not been stretched to form a pore structure during the first cold drawing process. This allows for the formation of a more suitable pore structure in these areas, resulting in a final membrane fiber with suitable porosity and pore structure. This leads to a relatively high degassing rate and degassing efficiency, meeting the needs of degassing fields such as wastewater ammonia removal that require rapid gas removal.
[0088] Based on this, the cold drawing rate during both cold drawing processes should not exceed 20%. This may be because pentene-based hydrophobic additives are added in this invention. These additives are usually non-crystalline substances. Compared to PP materials, the addition of pentene-based hydrophobic additives will have a certain impact on the toughness of the heat-set semi-finished product and cause it to decrease. If the cold drawing rate during the two cold drawing processes is too high (above 20%), there may be micro-cracks or pore structure prototypes formed during the first heat-set stretching process, as well as the merging of adjacent pore structures during the process of the crystal nuclei being pulled apart to form pore structures in the heat-set semi-finished product.
[0089] After cold drawing to form a hole, the cold-drawn semi-finished product is then hot-drawn to expand the hole. In this invention, the hot drawing temperature is controlled at 100-120℃, and the hot drawing rate of both hot drawing processes is not higher than 5% / min. The hot drawing rate of the first hot drawing is lower than that of the second hot drawing. Preferably, the hot drawing rate of the first hot drawing is 0.2-0.8% / min, the hot drawing rate of the second hot drawing is 1.5-2%, the elongation of the first hot drawing is 20%-80%, and the elongation of the second hot drawing is 40%-100%.
[0090] Similar to the cold drawing process, this invention also employs a two-stage hot drawing process for stretching. The first hot drawing process involves less and slower stretching, while the second hot drawing process involves more and faster stretching, and the hot drawing rate for both processes cannot exceed 5%. This is because during the cold drawing process to form a porous structure, the formation of the porous structure can be broadly divided into two categories: one is the porous structure formed by cold drawing after the formation of micro-cracks or pore structure prototypes during the first hot-setting stretching process; the other is the porous structure formed by pulling open the difficult-to-stretch crystal nuclei in the hot-setting semi-finished product during the second cold drawing process. If only one hot drawing process is performed, the porous structures in the above two categories may not be able to achieve adequate pore expansion, i.e., a suitable membrane pore structure cannot be formed, which may result in defects such as low porosity and small membrane pores, which is not conducive to the application of membrane fibers in degassing applications such as wastewater ammonia removal that require a fast degassing rate.
[0091] This invention employs a first hot-drawing process with less and slower stretching, followed by a second hot-drawing process with more and faster stretching, all at a suitable hot-drawing temperature (100-120℃). The aim is to first subject the pore structure, formed through micro-cracks or nascent pore structures, to a relatively suitable stretching process, ensuring the relatively stable existence of this pore structure within the hot-drawn semi-finished product. The second hot-drawing process then expands the pore structure formed by the latter, thus reducing the probability of excessively large pore structures or the merging of adjacent pore structures. It should be noted that the cold-drawn elongation rate and the hot-drawn elongation rate in this invention are calculated using an additive method. For example, if the elongation rate of the cold-drawn semi-finished product is 20% after the first hot-drawing process and 40% after the second, then the total hot-drawn elongation rate of the cold-drawn semi-finished product after both processes is 20% + 40% = 60%.
[0092] Finally, a second heat-setting process is performed on the hot-drawn semi-finished product. Preferably, the temperature of the second heat-setting is controlled at 110-140℃, and the time is controlled at 2-5 minutes. Under such heat-setting temperature and time, the residual stress of the stretching and pore-forming stage can be effectively eliminated. At the same time, it can also avoid the impact on the internal pore structure and stability of the membrane fibers due to excessively high second heat-setting temperature. As a result, the final membrane fibers have excellent resistance, high degassing rate and degassing efficiency, and good tensile strength and elongation at break. It is suitable for applications where the inner surface of hollow fiber membranes needs to be in long-term contact with acidic, alkaline and other active liquids for degassing (such as ammonia removal from wastewater and carbon dioxide capture). At the same time, in some degassing applications where water vapor is easily formed and condenses to form a liquid film, it can also effectively inhibit the formation of liquid film and reduce the amount of water vapor lost after condensation.
[0093] Furthermore, the present invention also provides an application of an asymmetric PP hollow fiber porous membrane for degassing, wherein the porous membrane is used in degassing fields such as degassing of ultrapure water and / or deammoniation of wastewater.
[0094] It should be noted that the wastewater claimed in this invention can originate from landfill leachate, industrial wastewater, wastewater from chemical products, etc. The hollow fiber membrane of this invention can be well applied in some fields where the inner surface of the hollow fiber membrane needs to be in long-term contact with active liquids such as acidic and alkaline substances for degassing (such as ammonia removal from wastewater, carbon dioxide capture, etc.), and can also be well applied in some degassing fields where water vapor is easily formed and condenses to form a liquid film (such as ultrapure water degassing, etc.).
[0095] In summary, the present invention has at least one of the following beneficial technical effects: 1. This invention, through the addition of pentene-based hydrophobic additives, enables hollow fiber porous membranes made of PP material to possess better hydrophobicity. This allows the hollow fiber porous membranes to better resist the corrosive effects of active solutions, such as acidic or alkaline solutions, where both the inner and outer surfaces of the hollow fiber membrane need to come into contact with the liquid to be degassed. This gives the hollow fiber porous membranes better long-term durability. At the same time, the hollow fiber porous membranes of this invention can also be well applied in degassing applications where water vapor easily forms and condenses to form a liquid film, significantly reducing the amount of water vapor loss due to condensation.
[0096] 2. By selecting appropriate weight-average molecular weight and proportion of hydrophobic additives and PP materials, the hollow fiber porous membrane prepared in this invention still has a high degree of crystallinity, thereby giving the hollow fiber porous membrane a good degassing rate and high degassing efficiency. In wastewater deammoniation applications, the deammoniation efficiency can reach more than 80%, and the deoxygenation efficiency can reach more than 90%. Attached Figure Description
[0097] The present invention will be further described below with reference to the accompanying drawings: Figure 1 The image shown is a scanning electron microscope image of the inner surface of the hollow fiber porous membrane prepared in Example 1, with a magnification of 20K×. Figure 2 The image shown is a scanning electron microscope image of the outer surface of the hollow fiber porous membrane prepared in Example 1, with a magnification of 50K×. Figure 3 The image shown is a scanning electron microscope image of the inner surface of the hollow fiber porous membrane prepared in Example 2, with a magnification of 5K×. Figure 4 The image shown is a scanning electron microscope (SEM) image of the outer surface of the hollow fiber porous membrane prepared in Example 5, with a magnification of 50K×. Detailed Implementation
[0098] The present invention will be further described in detail below with reference to the embodiments. Unless otherwise specified, the raw materials and equipment used to prepare hollow fiber membranes in the following embodiments can be purchased commercially. Example 1
[0099] A process for preparing an asymmetric PP hollow fiber porous membrane for degassing includes the following steps: S1, spinning, involves blending and melting PP material and hydrophobic additives, then extruding through a die to form a molded product with a hollow inner cavity. The extrusion screw is a special single-screw screw with a feed section compression ratio of 1.2 and a mixing section compression ratio of 2. The mixing section includes a mixing thread, and the metering section length / screw diameter ratio is 9. The die extrusion temperature is 170℃. The melting process includes melting, mixing, and metering steps, with a metering temperature of 180℃ and a die length-to-diameter ratio of 6. The isotacticity of the PP material is not less than 95%, and the melt index of the PP raw material is 5 g / min@(190℃, 5 kg). The weight-average molecular weight of the PP material is 150,000, the molecular weight distribution of the PP material is 7, the weight-average molecular weight of the hydrophobic additive is 50,000, and the hydrophobic additive accounts for 20% of the total polymer mass (referring to the total mass of the hydrophobic additive and the PP material). S2, Pre-crystallization: The molded product is placed in an air section for pre-crystallization, where the temperature of the air section is 50°C and the residence time in the air section is 0.1s. S3, air-cooled crystallization: the molded product obtained in step S2 is cooled by blowing air in an air atmosphere, wherein the blowing temperature is 55℃ and the blowing speed is 40m / min, to obtain nascent fibers. S4, First heat setting: The nascent fibers undergo a first heat setting treatment and a stretching treatment. The first heat setting temperature is 100℃, the first heat setting time is 30 minutes, and the stretching elongation is 0.8%, resulting in a heat-set semi-finished product. S5, Cold drawing to form holes: The heat-set semi-finished product is subjected to two cold drawing processes. The temperature of the first cold drawing is 50℃, the cold drawing rate is 8.5% / min, and the elongation is 15%. The temperature of the second cold drawing is 53℃, the cold drawing rate is 18% / min, and the elongation is 25%, thus obtaining the cold-drawn semi-finished product. S6, Hot drawing and hole expansion: The cold-drawn semi-finished product is subjected to two hot drawing and hole expansion processes. The temperature of the two hot drawing processes is 115℃. The hot drawing rate of the first hot drawing is 0.6% / min and the elongation of the first hot drawing is 60%. The hot drawing rate of the second hot drawing is 1.8% / min and the elongation of the second hot drawing is 80%, thus obtaining the hot-drawn semi-finished product. S7, Secondary heat setting: The hot-drawn semi-finished product undergoes a second heat setting process. The temperature of the second heat setting is 130℃, and the time of the second heat setting is 3.5 minutes, to obtain a hollow fiber porous membrane.
[0100] Examples 2-7
[0101] The difference between Examples 2-7 and Example 1 lies in the different process parameters, as shown in Tables 1-1, 1-2 and 1-3. Comparative Example 1
[0102] The difference between Comparative Example 1 and Example 1 is that no hydrophobic additive was added. Other differences are shown in Tables 1-1, 1-2 and 1-3. Comparative Example 2
[0103] The difference between Comparative Example 2 and Example 1 is that a hydrophobic additive was added, wherein the hydrophobic additive is BASF's silicone resin Silres 80. Other differences are shown in Tables 1-1, 1-2 and 1-3. Comparative Example 3
[0104] The difference between Comparative Example 3 and Example 1 is that the amount of hydrophobic additive added is 50% of the total polymer mass. Other differences are shown in Tables 1-1, 1-2 and 1-3. Comparative Example 4
[0105] The difference between Comparative Example 4 and Example 1 is that the amount of hydrophobic additive added is 1% of the total polymer mass. Other differences are shown in Tables 1-1, 1-2 and 1-3. Comparative Example 5
[0106] The difference between Comparative Example 5 and Example 1 lies in the different process parameters, as shown in Tables 1-1, 1-2 and 1-3.
[0107] The hydrophobic additive used in Examples 1-2 was cis-1,4-polyisoprene rubber; the hydrophobic additive used in Examples 3-4 was styrene-isoprene-styrene block copolymer (SIS); the hydrophobic additive used in Examples 5-7 was Mitsui's Tafmer propylene / pentene copolymer; the hydrophobic additive used in Comparative Example 2 was BASF's silicone resin Silres 80; and the hydrophobic additive used in Comparative Examples 3-5 was cis-1,4-polyisoprene rubber.
[0108] Table 1-1
[0109] Table 1-2
[0110] Table 1-3
[0111] Membrane structure parameter detection The morphology of the PP hollow fiber porous membranes prepared in Examples 1-7 and Comparative Examples 1-5 was characterized using a scanning electron microscope (Hitachi S-5500). The outer surface, inner surface and cross-section of the PP hollow fiber porous membrane were selected as the observation objects. The specific detection and measurement results are shown in Tables 2-1 and 2-2.
[0112] Table 2-1
[0113] Table 2-2
[0114] The skin thickness of Examples 1-4 was measured, and the test results are shown in Tables 2-3.
[0115] Table 2-3
[0116] The pore size and density of the external degassing pores on the outer surface of Examples 5-7 were measured, and the test results are shown in Tables 2-4.
[0117] Table 2-4
[0118] Membrane performance parameter testing 1.1 Tensile strength and elongation at break tests After testing, the tensile strength of the PP hollow fiber porous membranes prepared in Examples 1-7 is not less than 200 CN, and the elongation at break is 50-500%, which means that they all have large tensile strength and elongation at break, and can meet the needs of industrialization.
[0119] 1.2 Ammonia removal efficiency test; 1.3 Oxygen permeation rate test; 1.4 Water evaporation rate test; 1.5 Deoxygenation efficiency test; 1.6 XRD crystallinity test; 1.7 Water contact angle test; 1.8 Roughness test.
[0120] The test results are shown in Table 3. The water evaporation amount refers to the amount of water lost during the degassing process. As the gas is continuously removed, the water in the liquid system will be converted into water vapor due to evaporation and other factors, and then condense along with the gas to be removed as it passes through the hollow fiber porous membrane.
[0121] Table 3
[0122] As can be seen from the above, the hollow fiber porous membranes prepared in Examples 1-7 of this invention, after adding the pentene-based hydrophobic additives of this invention, can significantly improve the hydrophobic properties of the hollow fiber porous membranes, resulting in high internal and external water contact angles. Furthermore, the crystallinity of the hollow fiber porous membranes is almost unaffected by the addition of the pentene-based hydrophobic additives, remaining at a high level. This allows the hollow fiber porous membranes of this invention to be well-suited for applications where the inner surface of the hollow fiber membrane needs to be in long-term contact with reactive liquids such as acids and alkalis for degassing (e.g., wastewater ammonia removal, carbon dioxide capture). When applied to wastewater ammonia removal, the ammonia removal efficiency of the hollow fiber porous membranes of this invention can reach over 80% (with the samples prepared in Examples 5-7 showing particularly good ammonia removal effects), generating significant economic value. In addition, the hollow fiber porous membrane of this invention has a low water evaporation rate, and also possesses high degassing efficiency and a good degassing rate. Therefore, the hollow fiber porous membrane of this invention can be well applied in degassing fields where water vapor easily forms and condenses to form a liquid film (such as ultrapure water degassing). Especially when applied to ultrapure water degassing, it can remove dissolved oxygen from ultrapure water as much as possible while reducing ultrapure water loss, resulting in high production efficiency and high economic value. Finally, the hollow fiber porous membrane of this invention also has good durability. After long-term testing in the wastewater deammoniation process, the ammonia removal efficiency of the hollow fiber porous membrane of this invention remained essentially unchanged after 3 months of use. In contrast, the hollow fiber porous membranes prepared in Comparative Examples 1-5, due to their poor durability, showed a significant decrease in ammonia removal efficiency after 24 hours of testing.
[0123] The hollow fiber porous membranes prepared in Comparative Examples 1-5 all had high water evaporation rates, making them unsuitable for applications such as ultrapure water degassing. Furthermore, the hollow fiber porous membranes prepared in Comparative Examples 1-5 exhibited poor long-term durability, making them unsuitable for degassing applications where the inner surface of some hollow fiber membranes needs to be in long-term contact with reactive liquids such as acids and alkalis for degassing. This also leads to a decrease in the degassing efficiency and degassing rate of the hollow fiber porous membranes, making it difficult to meet the needs of practical applications.
[0124] The preferred embodiments of the present invention have been described in detail above. However, it should be understood that after reading the above teachings, those skilled in the art can make various alterations or modifications to the present invention. These equivalent forms also fall within the scope defined by the appended claims.
Claims
1. An asymmetric PP hollow fiber porous membrane for degassing, comprising a main body, one side of which is an inner surface facing the inner cavity, and the other side is an outer surface; the main body has non-directional tortuous channels; the inner surface has internal degassing pores; the pore area ratio of the outer surface is not greater than 5%, and the pore area ratio of the outer surface is less than that of the inner surface; characterized in that, The average SEM pore size of the internal degassing pores is 30-150 nm, and the pore area ratio of the inner surface is 10%-40%. The overall porosity of the porous membrane is 20%-65%; the thickness of the porous membrane is 30-75 μm. The polymer constituting the porous membrane includes at least a hydrophobic additive and PP, wherein the weight-average molecular weight of the PP is 100,000 to 600,000 and the molecular weight distribution is 2 to 7. The hydrophobic additive contains only carbon and hydrogen elements and is a pentene-based substance; the weight-average molecular weight of the hydrophobic additive is 50,000-200,000. The hydrophobic additives in the polymer constituting the porous membrane account for 5%-30% of the total polymer mass; The porous membrane was prepared by melt stretching. The porous membrane was tested by XRD, and the XRD crystallinity of the porous membrane was 60%-90%.
2. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The infrared absorption spectra of the inner and outer surfaces of the porous membrane were tested using the ATR method, and the hydrophobic additive doping coefficient X of the porous membrane was calculated. X=ABS 720 / ABS 1460 ; where ABS 720 is the absorption intensity of the porous membrane at a wave number of 720 cm -1 nearby. ABS 1460 The porous membrane has an absorption intensity near a wave number of 1460 cm -1 -1. Hydrophobic additive doping factor X 内 = ABS 内表面720 / ABS 内表面1460 ; wherein X 内 ranges from 0.0005 to 0.15; ABS 内表面720 The absorption intensity of the inner surface of the porous membrane at a wave number of 720 cm -1 nearby; ABS 内表面1460 The inner surface of the porous membrane has an absorption intensity in the vicinity of a wave number of 1460 cm -1 -1.
3. The asymmetric PP hollow fiber porous membrane for degassing according to claim 2, characterized in that, The X 内 The value range is 0.001-0.
08.
4. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, Hydrophobic additive doping factor X 外 = ABS 外表面720 / ABS 外表面1460 ; wherein X 外 ranges from 0.001 to 0.3; ABS 外表面720 The absorption intensity of the outer surface of the porous membrane at a wave number of 720 cm -1 nearby; ABS 外表面1460 The porous membrane outer surface has an absorption intensity in the vicinity of a wave number of 1460 cm -1 -1.
5. The asymmetric PP hollow fiber porous membrane for degassing according to claim 4, characterized in that, The X 外 The value range is 0.005-0.
1.
6. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The overall porosity of the porous membrane is 25%-60%, and the thickness of the porous membrane is 40-65 μm.
7. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The porous membrane has a full width at half maximum (FWHM) of 0.2-0.7 near a 2θ angle of 14.1°, and the grain size is not less than 150 angstroms.
8. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The water contact angle of the inner surface is 95°-120°, and the roughness Ra of the inner surface is 20-60μm; and / or the water contact angle of the outer surface is 100°-130°, and the roughness Ra of the outer surface is 15-70μm.
9. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, Some adjacent internal degassing pores are separated by supporting fibers, the average SEM length of the supporting fibers is 50-500nm, and the ratio of the average SEM length of the supporting fibers to the average SEM width of the supporting fibers is 1.5-15:
1. The length direction of the supporting fibers is consistent with the circumferential direction of the porous membrane, and the width direction of the supporting fibers is consistent with the length direction of the porous membrane.
10. The asymmetric PP hollow fiber porous membrane for degassing according to claim 9, characterized in that, The internal degassing pores are stacked to form an internal degassing region. Some adjacent internal degassing regions are separated by dense regions. The average SEM width of the internal degassing region is 80-1200 nm, and the average SEM length of the internal degassing region is at least 1.5 times the average SEM width of the internal degassing region. The length of the internal degassing zone is aligned with the circumferential direction of the porous membrane, while the width of the internal degassing zone is aligned with the length of the porous membrane.
11. The asymmetric PP hollow fiber porous membrane for degassing according to claim 9, characterized in that, The internal degassing pores include a plurality of elliptical air pores. The average major axis of the air pores is 100-600 nm, the ratio of the average major axis of the air pores to the average pore diameter of the air pores is 1.5-10:1, and the ratio of the average pore diameter of the air pores to the average width of the supporting fibers is 1.5-12:
1. The major axis of the pores is aligned with the length of the porous membrane.
12. The asymmetric PP hollow fiber porous membrane for degassing according to claim 10, characterized in that, The average SEM width of the dense region is 60-800nm, and the ratio of the average SEM width of the supporting fiber to the average SEM width of the dense region is 1:4-10. The width of the dense region is aligned with the length of the porous membrane.
13. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The main body comprises a skin layer and a support layer, one side of the support layer is an inner surface, one side of the skin layer is an outer surface, the other side of the skin layer and the other side of the support layer are in continuous fiber transition; the support layer has porous fibers for forming a porous structure, the SEM average diameter of the porous fibers is 30-200 nm, the density of the porous fibers is 10-300 / 1 μm 2 .
14. The asymmetric PP hollow fiber porous membrane for degassing according to claim 13, characterized in that, The average diameter variation gradient of the porous fiber under SEM is 0.1-1.2 nm / μm; The gradient of the average SEM diameter of porous fibers = (average SEM diameter of porous fibers near the inner surface - average SEM diameter of porous fibers far from the inner surface) / thickness of the support layer.
15. The asymmetric PP hollow fiber porous membrane for degassing according to claim 13, characterized in that, The outer surface is a dense surface with a pore area ratio of less than 1%, the skin layer thickness is 0.1-3 μm, and the support layer thickness is at least 29 μm greater than the skin layer thickness.
16. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The outer surface has an external degassing region and an external dense region. The porosity of the external dense region is less than 1%. The external degassing region contains a plurality of external degassing pores. The average SEM pore size of the external degassing pores in the external degassing region is 10-90 nm, and the density of the external degassing pores is 10-80 pores / μm. 2 .
17. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The outer surface has a plurality of uniformly distributed external degassing pores, the SEM average pore diameter of which is 10-90 nm, and the density of which is 1-30 pores / 10 μm. 2 .
18. The asymmetric PP hollow fiber porous membrane for degassing according to claim 1, characterized in that, The ammonia removal efficiency of the porous membrane is at least greater than 80%. The O2 permeation rate of the porous membrane is not less than 30 L / (min·bar·0.1m). 2 ); The water evaporation rate of the porous membrane is no higher than 0.10 ml / m³. 2 / min; The deoxygenation efficiency of the porous membrane is greater than or equal to 90%.
19. The preparation process of an asymmetric PP hollow fiber porous membrane for degassing according to any one of claims 1-18, characterized in that, The process includes the following steps: S1, spinning, involves blending and melting PP material and hydrophobic additives, then extruding through a die to form a molded product with a hollow inner cavity. The extrusion screw is a single screw, with a feed section compression ratio of 1.05-1.4; the mixing section compression ratio is 1.4-2.7, and the mixing section includes a mixing thread; the metering section length / screw diameter is 5-12, and the die extrusion temperature is 165-180℃; the melting process includes melting, mixing, and metering steps, with the metering temperature 10-20℃ higher than the die extrusion temperature; the die length-to-diameter ratio is 2-8; the isotacticity of the PP is not less than 95%; the melt index of the PP raw material is 1~7 g / min@(190℃, 5kg). S2, Pre-crystallization, involves placing the molded product in the air section for pre-crystallization; S3, air-cooled crystallization: the molded product obtained in step S2 is cooled by blowing air in an air atmosphere to obtain nascent fibers; S4, First heat setting, involves heat setting the nascent fibers for the first time and then stretching them. The first heat setting temperature is 80-110℃, and the stretching elongation is 0.5-2%, resulting in a heat-set semi-finished product. S5, cold drawing to form holes: The heat-set semi-finished product is subjected to two cold drawing processes, wherein the ratio of the temperature of the first cold drawing to the temperature of the first heat setting is 1:(2-5), and the cold drawing rate of both cold drawing processes is not higher than 20% / min. The cold drawing rate of the first cold drawing process is less than the cold drawing rate of the second cold drawing process, and a cold-drawn semi-finished product is obtained. The elongation rate of the first cold drawing is 5%-20%, and the elongation rate of the second cold drawing is 10%-30%. S6, hot drawing and hole expansion: The cold-drawn semi-finished product is subjected to two hot drawing and hole expansion processes. The temperature of the two hot drawing processes is 100-120℃, and the hot drawing rate of the two hot drawing processes is not higher than 5% / min. The hot drawing rate of the first hot drawing process is less than the hot drawing rate of the second hot drawing process, so as to obtain the hot-drawn semi-finished product. S7, Secondary heat setting: The hot-drawn semi-finished product undergoes a second heat setting process to obtain a hollow fiber porous membrane.
20. The preparation process of an asymmetric PP hollow fiber porous membrane for degassing according to claim 19, characterized in that, In step S2, the temperature of the air section is 40-70℃, and the residence time of the air section is 0.01-0.1s; In step S3, the blowing temperature is 30-70℃ and the blowing speed is 20-80m / min.
21. The preparation process of an asymmetric PP hollow fiber porous membrane for degassing according to claim 19, characterized in that, In step S4, the first heat setting time is 20-50 minutes; In step S7, the temperature for the second heat setting is 110-140℃, and the time for the second heat setting is 2-5 minutes.
22. The preparation process of an asymmetric PP hollow fiber porous membrane for degassing according to claim 19, characterized in that, In step S5, the cold drawing rate of the first cold drawing is 5-10% / min, the cold drawing rate of the second cold drawing is 15-20% / min, and the temperature of the second cold drawing is 0-5℃ higher than that of the first cold drawing. In step S6, the hot stretching rate of the first hot stretch is 0.2-0.8% / min, the hot stretching rate of the second hot stretch is 1.5-2% / min, the elongation of the first hot stretch is 20%-80%, and the elongation of the second hot stretch is 40%-100%.
23. The application of the asymmetric PP hollow fiber porous membrane for degassing according to any one of claims 1-18, characterized in that, The porous membrane is used for degassing of ultrapure water and / or ammonia removal from wastewater.
Citation Information
Patent Citations
Preparation method for hydrophobic ammonia nitrogen removal film
CN103551046A
A method for preparing an asymmetric polyolefin membrane
CN111346519B
Asymmetric hydrophobic polyolefin hollow fiber membrane, preparation method and application thereof
CN111888946A
Polyolefin hollow fiber membrane for asymmetric degassing as well as preparation method and application of polyolefin hollow fiber membrane
CN115155329A