A kind of preparation device and preparation method of nano silver
Through a DC power supply and a partitioned device, nanosilver is directly generated in the polyol solution in the anode tank, which solves the problems of lengthy process and large pollution in the traditional method, and achieves efficient and environmentally friendly nanosilver preparation, and the nanosilver particles are The diameter and shape meet the standards.
Patent Information
- Application Number
- CN202410378379.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-29
AI Technical Summary
In the traditional preparation method of silver nanoparticles, silver nitrate is required as an intermediate product, resulting in a lengthy process, high pollution, and increased energy consumption.
Using a DC power supply and partitioned design, the polyol solution is electrolyzed between the dissolution zone and the reduction zone of the anode tank to directly generate nano-silver, avoiding the intermediate step of silver nitrate, and is optimized through anion exchange mechanism and heating and cooling mechanism. reaction conditions.
It achieves the direct and environmentally friendly preparation of nanosilver, and the generated by-product is hydrogen, which reduces pollution, improves production efficiency, and ensures that the particle size and morphology of nanosilver meet standards.
Smart Images

Figure CN118147705B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metal material preparation, and in particular to a nanosilver preparation device and method. Background Art
[0002] Silver has excellent electrical and thermal conductivity, anti-oxidation and antibacterial properties. Nanosilver materials are widely used in various fields. In the photovoltaic and electronic fields, nanosilver materials are used as conductive silver pastes and conductive components in transparent electrodes; in the medical field, nanosilver has been proven to have a strong inactivation effect on Escherichia coli and Staphylococcus aureus; in the field of fuel cells, nanosilver has excellent catalytic activity in oxygen reduction reactions, making it a promising alternative to platinum as a cheap catalyst for fuel cells.
[0003] At present, nanosilver can be prepared by spray pyrolysis, solvent thermal method, chemical reduction, sol-gel method and other methods. Most of these methods use silver nitrate as an intermediate product (raw material of nanosilver), such as Figure 7 The traditional preparation method shown uses pure silver as raw material and uses silver nitrate as an intermediate product to prepare nanosilver. In the traditional preparation method, pure silver is dissolved in concentrated nitric acid to obtain a silver nitrate solution, and nitrogen oxide pollution will be generated in this process; the silver nitrate solution is crystallized by heating to obtain silver nitrate crystals; the nitrate crystals are then chemically reduced or spray pyrolyzed to obtain nanosilver. This traditional process has the problems of lengthy process and high pollution. In fact, in the traditional process, both the starting point (pure silver) and the end point (nanosilver) are metallic silver, but because silver nitrate (compound) is required as an intermediate product, silver and silver ions need to undergo multiple dissolution and deposition processes, which is the direct cause of the increase in process and energy consumption. Summary of the invention
[0004] The embodiment of the present application provides a nanosilver preparation device and preparation method, which can directly prepare nanosilver, the particle size and morphology of the prepared nanosilver meet the standards, and can also produce usable by-products.
[0005] In a first aspect, an embodiment of the present application provides a device for preparing nanosilver, comprising:
[0006] A direct current power supply, wherein the positive electrode of the direct current power supply is connected to pure silver to form an anode, and the negative electrode of the direct current power supply is connected to metal to form a cathode; an anode tank, wherein a polyol solution is arranged in the anode tank; the anode tank comprises a dissolution zone and a reduction zone along its length direction, wherein at least part of the anode is arranged in the dissolution zone, and the reduction zone is used to generate nanosilver; a cathode tank, wherein a cathode liquid is arranged in the cathode tank, and at least part of the cathode is arranged in the cathode tank; an anion exchange mechanism, which is connected between the dissolution zone and the cathode tank of the anode tank, and the anion exchange mechanism can block the flow of cations between the dissolution zone and the cathode tank; a cooling mechanism, which is at least partially wrapped on the periphery of the dissolution zone; and a heating mechanism, which is at least partially wrapped on the periphery of the reduction zone.
[0007] In a second aspect, an embodiment of the present application provides a method for preparing nanosilver, using a nanosilver preparation device, the preparation method comprising: starting a cooling mechanism and a heating mechanism, applying a current of a predetermined value between an anode and a cathode, and performing constant current electrolysis; hydrogen is precipitated on the surface of the cathode, and the anode loses electrons to generate silver ions that enter a polyol solution; the silver ions reach a reduction zone of an anode tank through diffusion, and the silver ions in the reduction zone react with the polyol solution heated by the heating mechanism to generate nanosilver.
[0008] The nano silver preparation device and preparation method of the present application have at least the following beneficial effects:
[0009] The preparation device of the present application can directly prepare nanosilver without using silver nitrate as an intermediate product, and the by-product generated during the reaction is hydrogen, which is more environmentally friendly than traditional methods. The by-product hydrogen can bring certain additional economic benefits and can effectively solve the technical problems existing in traditional processes. On the one hand, the anode liquid of the present application is configured as a polyol solution, which can gently reduce silver ions, prevent the excessive growth of silver crystal nuclei during the violent reduction process, and ensure that the particle size and morphology of the generated nanosilver meet the standards. On the other hand, the anode tank is zoned, and the top dissolution zone and the bottom reduction zone are respectively provided with cooling mechanisms and heating mechanisms, so that the polyol solution in the anode tank forms different temperature ranges, and realizes the innovative preparation method of nanosilver of "pure silver top dissolution, polyol bottom reduction" in the anode tank. At the same time, the top dissolution zone is designed as a low-temperature zone, which can avoid damage to the anion exchange mechanism and other structures in the dissolution zone (such as filter membrane) due to high temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0011] Figure 1 Schematic diagram of the structure of the nanosilver preparation device in the embodiment of the present application;
[0012] Figure 2 It is a schematic diagram of the structure of the anode tank in the embodiment of the present application;
[0013] Figure 3 It is a schematic diagram of the structure of the cathode tank in the embodiment of the present application;
[0014] Figure 4 is a schematic diagram of an anion exchange mechanism in an embodiment of the present application;
[0015] Figure 5is a schematic diagram of an anode tank and a cooling mechanism in an embodiment of the present application;
[0016] Figure 6 is a scanning electron microscope image of nanosilver prepared by the preparation method in the embodiment of the present application;
[0017] Figure 7 This is a flow chart of the preparation of nanosilver in the traditional technology;
[0018] Description of the reference numerals is as follows:
[0019] 1. DC power supply; 11. anode; 12. cathode;
[0020] 2. anode tank; 21. polyol solution; 22. dissolution zone; 23. reduction zone; 24. filter membrane; 25. anode fixing member; 26. first communication port;
[0021] 3. cathode tank; 31. cathode liquid; 32. air guide tube; 33. hydrogen; 34. second communication port; 35. cathode fixing member;
[0022] 4. anion exchange mechanism; 41. anion exchange membrane; 42. gasket; 43. waterproof ring;
[0023] 5. Cooling mechanism; 51. Cooling water tank; 52. Cooling water tank; 53. First circulation pipe; 54. Second circulation pipe; 55. Pump unit; 56. Flow regulator; 57. Anode tank clamping mechanism; 58. Cooling liquid;
[0024] 6. Heating mechanism; 61. Heating pot body; 62. Magnetic stirring bar; 63. Oil; 64. Insulation cotton;
[0025] 7. Nanosilver. DETAILED DESCRIPTION
[0026] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only intended to explain the present application, rather than to limit the present application. For those skilled in the art, the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application.
[0027] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.
[0028] like Figures 1 to 5 As shown, the embodiment of the present application discloses a nanosilver preparation device, including a DC power supply 1, an anode tank 2, a cathode tank 3, an anion exchange mechanism 4, a cooling mechanism 5 and a heating mechanism 6, which are specifically as follows:
[0029] 1. If Figure 1 As shown, the positive electrode of the DC power supply 1 is connected to pure silver to form an anode 11. The pure silver can be in the form of sheets, rods, powder, etc., as long as it can be stably connected to the positive electrode of the power supply. "Pure silver" can refer to silver with a content of 99.9% to 99.99% or 925 pure silver with a content of 92.5%. The "pure silver" here can also be selected as silver with other contents according to actual conditions.
[0030] Among them, the end of the anode 11 is arranged in the anode tank 2, and the end of the anode 11 is wrapped with a filter membrane 24. The end of the anode 11 and the filter membrane 24 are both located in the anode tank 2 and are both located below the liquid surface of the polyol solution 21. When the pure silver anode 11 is dissolved, a certain amount of anode mud will be generated. By wrapping the filter membrane 24 on the end of the pure silver anode 11, the prepared anode mud can be collected to prevent the anode mud from mixing into the nanosilver.
[0031] The negative pole of the DC power supply 1 is connected to a metal (the type of metal is selected according to actual conditions) to form a cathode 12. The cathode 12 is arranged in a cathode slot 3. A cathode liquid 31 is arranged in the cathode slot 3. At least part of the cathode 12 is inserted below the liquid surface of the cathode liquid 31.
[0032] 2. Anode tank 2, such as Figure 1 and Figure 2 As shown, a polyol solution 21 is provided in the anode tank 2. Preferably, the polyol is one of ethylene glycol, propylene glycol and diethylene glycol.
[0033] It should be noted that the reducing ability of polyols is weak at room temperature, but its reducing ability increases with increasing temperature. According to relevant research, polyols can reduce silver ions to nanosilver at 100-200°C, and at the same time they themselves are oxidized to substances such as aldehydes, aldehydes, formic acid and carbon dioxide. There are two reasons why polyol can generate nanosilver 7 instead of micron-sized silver powder when reducing silver ions: 1) polyol has weak reducing ability for silver ions. Compared with strong reducing agents for silver ions such as hydrazine hydrate, ascorbic acid, sodium hypophosphite, etc., polyol can reduce silver ions gently, thus preventing the excessive growth of silver crystal nuclei during the violent reduction process; 2) polyol solution 21 is an organic system, and the diffusion rate of metal ions in it is relatively slow (compared with aqueous solution system). During the formation of nanosilver, silver ions near the silver crystal nucleus diffuse to the vicinity of the crystal nucleus to make it grow. In the organic system, due to the slow diffusion rate of ions, the growth rate of the crystal nucleus is relatively slow, and nanometer-sized particles are finally formed. On the contrary, in the aqueous solution system, the diffusion rate of ions is relatively fast, the growth rate of the crystal nucleus is relatively large, and it is difficult to form nanometer-sized particles.
[0034] The anode tank 2 is vertically arranged, and the anode tank 2 is a tubular structure with a certain length. In the embodiment of the present application, the anode tank 2 is divided into a dissolution zone 22 and a reduction zone 23 connected to each other in the longitudinal direction thereof, and the dissolution zone 22 and the reduction zone 23 are both filled with a polyol solution 21. Among them, the upper port of the dissolution zone 22 is configured as an insertion port of the anode 11, and an anode fixing member 25 (refer to the prior art) is arranged at the insertion port position, and the anode fixing member 25 is used to install and stabilize the anode 11. The anode fixing member 25 and the anode tank 2 need to be sealed, and a frosted glass stopper, a rubber stopper, etc. are installed at the corresponding position, so that the entire anode tank 2 can be formed into a closed state to prevent the anode liquid from overflowing or the coolant 58 from flowing into the anode tank 2.
[0035] The dissolution zone 22 of the anode tank 2 is provided with a first communication port 26 , which is in communication with the anion exchange mechanism 4 . Similarly, the first communication port 26 and the anion exchange mechanism 4 need to be sealed to ensure that the anode tank 2 is in a sealed state.
[0036] In the embodiment of the present application, the anode tank 2 is partitioned to form different temperature ranges of the polyol solution 21 in the anode tank 2, so as to realize the partitioned reaction preparation method of "pure silver dissolving at the top and polyol reducing at the bottom" in the anode tank 2. It should be noted that if the partition design is not performed, two problems may occur: 1) the temperature at the top of the anode tank 2 is too high, and the anion exchange mechanism 4 and the filter membrane 24 in the dissolution zone 22 are damaged due to the high temperature; 2) the temperature of the reduction zone 23 at the bottom of the anode tank 2 is too low, and the reducing ability of the polyol is not enhanced, so nanosilver cannot be prepared at the bottom.
[0037] Preferably, the length ratio of the dissolution zone 22 to the reduction zone 23 is 1:2-4, for example 1:2 or 1:3. The length ratio is designed to leave more reduction zones 23 to ensure reduction efficiency.
[0038] Further preferably, in order to match some special working conditions, the total length of the anode tank 2 of the embodiment of the present application is 40 cm to 120 cm. Compared with the length of the anode tank 2 in the traditional laboratory, the length of the anode tank 2 in the embodiment of the present application is longer, which can facilitate the formation of different temperature ranges for the polyol solution 21. When the length of the anode tank 2 is too short, it is difficult to form differentiated temperature ranges at the top and bottom of the anode tank 2. On the other hand, when the length of the anode tank 2 is too long, the manufacturing cost of the device increases, and it is difficult to carry out loading and unloading.
[0039] 3. Cathode tank 3, such as Figure 1 and Figure 3 As shown, a cathode liquid 31 is provided in the cathode tank 3, and the cathode liquid 31 includes an aqueous solution containing an electrolyte; the purpose of adding the electrolyte is to increase the conductivity of the aqueous solution so that a hydrogen evolution reaction occurs at the metal cathode 12 to generate hydrogen 33. When chloride salts (such as sodium chloride) and sulfate salts (such as sodium sulfate) are used as electrolytes, chloride ions and sulfate ions will enter the anode liquid from the cathode liquid 31 through the anion exchange mechanism 4, and react with silver ions to generate silver chloride and silver sulfate, thereby failing to successfully prepare nanosilver. Therefore, the electrolyte type is preferably one of nitrate, acetate and aminosulfonate.
[0040] A second connecting port 34 is provided at the middle position of the cathode slot 3, and the second connecting port 34 is connected to the anion exchange mechanism 4. A cathode fixing member 35 (the prior art can be referred to) is provided at the upper opening position of the cathode slot 3, and the cathode fixing member 35 is used to install and stabilize the cathode 12. Sealing treatment is required between the cathode fixing member 35 and the cathode slot 3, and between the second connecting port 34 and the anion exchange mechanism 4, so that the entire cathode slot 3 can be formed in a closed state to prevent the cathode liquid 31 from overflowing or the coolant 58 from flowing into the cathode slot 3. The hydrogen 33 generated by the cathode 12 is discharged through the air duct 32.
[0041] One end of the air duct 32 is inserted into the cathode tank 3, specifically above the liquid surface of the cathode liquid 31, and the other end of the air duct 32 is connected to an external structure (for example, connected to an external collection tank, etc.). The hydrogen 33 is discharged through the air duct 32 and collected for subsequent use, which can enhance the added value of the device.
[0042] 4. Anion exchange mechanism 4, such as Figure 1 and Figure 4As shown, the anion exchange mechanism 4 is disposed between the first communication port 26 of the anode tank 2 and the second communication port 34 of the cathode tank 3, and is connected to the first communication port 26 and the second communication port 34 respectively. The function of the anion exchange mechanism 4 is to block the flow of cations (such as silver ions) and allow the flow of anions (such as nitrate ions, acetate ions, etc.). After power is turned on, the pure silver (anode 11) loses electrons and dissolves, and the generated silver ions enter the anode liquid (polyol solution 21). Since the anode tank 2 and the cathode tank 3 are separated by the anion exchange mechanism 4, the silver ions in the anode liquid cannot enter the cathode liquid 31, and the silver ions in the anode liquid can then be transferred from the dissolution area 22 at the top of the anode tank 2 to the reduction area 23 at the bottom through diffusion and precipitation.
[0043] The anion exchange mechanism 4 includes an anion exchange membrane 41, a gasket group and a waterproof rubber ring group; the gasket group includes two gaskets 42; the waterproof rubber ring group includes two waterproof rings 43; the anion exchange membrane 41 is used to block cations and allow anions to pass; the two gaskets 42 are stacked on both sides of the anion exchange membrane 41 to form a sandwich structure; the two waterproof rings 43 are respectively arranged in a one-to-one correspondence with the two gaskets 42, and the waterproof ring 43 is laminated on the side of the gasket 42 away from the anion exchange membrane 41. More preferably, the anion exchange membrane 41, the gasket 42 and the waterproof ring 43 are coaxially arranged.
[0044] Among them, the diameter D1 of the anion exchange membrane 41 is larger than the inner diameter D2 of the gasket 42 and smaller than the outer diameter D3 of the gasket 42. If the diameter D1 of the anion exchange membrane 41 is smaller than the inner diameter D2 of the gasket 42, the anion exchange membrane 41 cannot effectively block the ion exchange between the anode liquid and the cathode liquid 31. When the diameter D1 of the anion exchange membrane 41 is larger than the outer diameter D3 of the gasket 42, the anion exchange membrane 41 and the gasket assembly cannot be clamped.
[0045] The inner diameter D4 of the waterproof ring 43 is larger than the inner diameter D2 of the gasket 42 and smaller than the outer diameter D3 of the gasket 42. If the inner diameter D4 of the waterproof ring 43 is smaller than the inner diameter D2 of the gasket 42, the ion exchange area is blocked by the waterproof ring 43 and the effective exchange area is reduced. When the inner diameter D4 of the waterproof ring 43 is larger than the outer diameter D3 of the gasket 42, a closed structure cannot be formed and the external coolant 58 may flow into the anode liquid and the cathode liquid 31.
[0046] The first communication port 26 of the anode tank 2 is communicated with the inner hole of the waterproof ring 43 on one side, and the second communication port 34 of the cathode tank 3 is communicated with the inner hole of the waterproof ring 43 on the other side.
[0047] It should be noted that if the anion exchange mechanism 4 is not designed, the silver ions dissolved in the anode 11 will not be blocked, and the silver ions will follow the direction of the current into the cathode slot 3, and metallic silver crystals will precipitate on the surface of the copper sheet of the cathode 12, which will eventually make it impossible to prepare nanosilver.
[0048] 5. Cooling mechanism 5, such as Figure 1 and Figure 5 As shown, the cooling mechanism 5 in the embodiment of the present application is at least partially wrapped around the outer periphery of the dissolution zone 22. Further preferably, at least a portion of the cathode slot 3 is also wrapped by the cooling mechanism 5, and the dissolution zone 22 of the anode slot 2 and the cathode slot 3 are cooled by the cooling mechanism 5.
[0049] The cooling mechanism 5 includes a cooling water tank 51, a cooling water tank 52, a first circulation pipe 53, a second circulation pipe 54, a pump unit 55, a flow regulator 56 and an anode tank clamping mechanism 57;
[0050] The cooling water tank 51 is located above the cooling water tank 52, and a coolant 58 is provided in the cooling water tank 51;
[0051] The inner bottom surface of the cooling water tank 52 is vertically provided with a mounting hole, and the anode tank 2 is vertically penetrated with the mounting hole. An anode tank clamping mechanism 57 is provided between the outer periphery of the anode tank 2 (specifically the dissolution zone 22) and the inner peripheral wall of the mounting hole. The anode tank clamping mechanism 57 can realize the stable mounting of the anode tank 2 on the cooling water tank 52. If the anode tank 2 needs to be removed, the anode tank clamping mechanism 57 only needs to be removed. The specific form of the anode tank clamping mechanism 57 is not limited, as long as it can meet the function of fixing the anode tank 2 and preventing the cooling water from leaking when the coolant 58 circulates, and when the coolant 58 stops, it is convenient to remove the anode tank 2. In the embodiment of the present application, the anode tank clamping mechanism 57 can be a rubber ring or a combination of a rubber ring and a clamp. The rubber ring is inserted between the anode tank 2 and the inner peripheral wall of the mounting hole. If it is not stable enough, the anode tank 2 is clamped by the clamp and the rubber ring is squeezed so that the rubber ring fills the gap between the anode tank 2 and the mounting hole.
[0052] Among them, at least part of the dissolution zone 22 of the anode tank 2 is located in the cooling water tank 52, and at least part of the cathode tank 3 and the anion exchange mechanism 4 are also located in the cooling water tank 52. The coolant 58 in the cooling water tank 52 can wrap the dissolution zone 22, the anion exchange mechanism 4 and at least part of the cathode tank 3 in the cooling water tank 52, and take away the heat through the coolant 58.
[0053] The upper end of the first circulation pipe 53 is connected to the bottom of the cooling water tank 52, and the lower end of the first circulation pipe 53 is connected to the pump unit 55 in the cooling water tank 51. The pump unit 55 includes a water pump, and the output port of the water pump is connected to the lower end of the first circulation pipe 53. The coolant 58 is driven to circulate through the pump unit 55. The flow regulator 56 is arranged on the first circulation pipe 53, and the flow regulator 56 can adjust the flow of the coolant 58.
[0054] The upper end of the second circulation pipe 54 is connected to the bottom of the cooling water tank 52 , and the lower end of the second circulation pipe 54 is connected to the cooling water tank 51 .
[0055] In the embodiment of the present application, a circulation loop is formed between the cooling water tank 51, the cooling water tank 52, the first circulation pipe 53, the second circulation pipe 54 and the pump unit 55, and the coolant 58 can circulate in the circulation loop. In addition, the cooling mechanism 5 can also refer to the mechanism in the prior art that can achieve the temperature reduction function.
[0056] 6. Heating mechanism 6, such as Figure 1 As shown, the heating mechanism 6 is at least partially wrapped around the outer periphery of the reduction zone 23, and the reduction zone 23 is heated by the heating mechanism 6, wherein the heating mechanism 6 can wrap all the outer surfaces of the reduction zone 23, and of course, it can also only wrap one-third or one-half of the outer surface of the reduction zone 23. The embodiment of the present application illustrates that the heating mechanism 6 wraps about one-third of the outer surface of the reduction zone 23.
[0057] In the embodiment of the present application, the heating mechanism 6 is configured as a magnetic stirring heating pot (e.g., an oil bath type heating pot); the specific structure of the magnetic stirring heating pot can refer to the prior art. Here is a brief description, the magnetic stirring heating pot includes a heating pot body 61 and a magnetic stirring rod 62, the interior of the heating pot body 61 is provided with a heat conducting medium, the heat conducting medium can be an oil 63, the reduction zone 23 at the bottom of the anode tank 2 is inserted into the oil 63 of the heating pot body 61, the oil 63 is heated by the heat generated by the heating pot body 61, the oil 63 conducts the heat to the reduction zone 23 for heating, and the wrapped reduction zone 23 is insulated by providing a heat insulation cotton 64; the magnetic stirring rod 62 is provided at the bottom of the reduction zone 23, and the magnetic stirring rod 62 is used to stir the anode liquid (polyol solution), thereby improving the polyol reducibility at the bottom of the anode tank 2.
[0058] The present application also discloses a method for preparing nanosilver, which is prepared by using the nanosilver preparation device. The method comprises:
[0059] Step S1: adding a polyol solution 21 (e.g., ethylene glycol solution) as an anolyte to the anode tank 2, adding a sodium nitrate aqueous solution as a cathode liquid 31 to the cathode tank 3, and using a filter membrane 24 to wrap the portion of the anode 11 immersed in the anolyte, the filter membrane 24 can collect the anode mud generated during the preparation process;
[0060] Step S2: Turn on the heating mechanism 6 to heat the oil 63 to 150 degrees Celsius, and use the magnetic stirrer 62 to stir the anolyte, and at the same time turn on the pump unit 55 of the cooling mechanism 5 to drive the coolant 58 to circulate;
[0061] Step S3: starting the DC power supply 1, applying a current of a predetermined value (e.g., 50 mA) between the anode 11 and the cathode 12, and performing constant current electrolysis;
[0062] Hydrogen 33 is precipitated on the copper sheet surface of the cathode 12, and the anode 11 (pure silver) loses electrons to generate silver ions that enter the anode liquid; the silver ions reach the reduction zone 23 at the bottom of the anode tank 2 by diffusion, and the silver ions react with the polyol solution 21 heated by the heating mechanism 6 to generate nanosilver 7. The prepared nanosilver is as follows Figure 6 shown.
[0063] The above is only a specific implementation of the present application. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working processes of the systems, modules and units described above can refer to the corresponding processes in the aforementioned method embodiments, and will not be repeated here. It should be understood that the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in this application, and these modifications or replacements should be included in the protection scope of this application.
Claims
1. A device for preparing nano silver, characterized in that: include: A direct current power source (1), wherein the positive electrode of the direct current power source (1) is connected to pure silver to form an anode (11), and the negative electrode of the direct current power source (1) is connected to a metal to form a cathode (12); An anode tank (2), wherein a polyol solution (21) is arranged in the anode tank (2); the anode tank (2) comprises a dissolution zone (22) and a reduction zone (23) along its length direction, at least part of the anode (11) is arranged in the dissolution zone (22), and the reduction zone (23) is used to generate nanosilver (7); A cathode tank (3), wherein a cathode liquid (31) is arranged in the cathode tank (3), and at least a part of the cathode (12) is arranged in the cathode tank (3); An anion exchange mechanism (4) is connected between the dissolution zone (22) of the anode tank (2) and the cathode tank (3), and the anion exchange mechanism (4) can block the flow of cations between the dissolution zone (22) and the cathode tank (3); A cooling mechanism (5) at least partially wraps around the outer periphery of the dissolving zone (22); The heating mechanism (6) is at least partially wrapped around the outer periphery of the reduction zone (23).
2. The nano silver preparation device according to claim 1, characterized in that: The polyol solution (21) is any one of ethylene glycol, propylene glycol and diethylene glycol.
3. The nano silver preparation device according to claim 2 is characterized in that: The ratio of the length of the dissolution zone (22) to the length of the reduction zone (23) is 1:2-4.
4. The nano silver preparation device according to claim 1, characterized in that: The end of the anode (11) is wrapped with a filter membrane (24), and the end of the anode (11) and the filter membrane (24) are both located below the liquid surface of the polyol solution (21).
5. The nano silver preparation device according to claim 1, characterized in that: The cathode liquid (31) comprises an aqueous solution containing an electrolyte; the electrolyte is one of nitrate, acetate and aminosulfonate.
6. The nano silver preparation device according to claim 1, characterized in that: One end of an air guide tube (32) is inserted into the cathode tank (3), and the other end of the air guide tube (32) is communicated with an external structure.
7. The nanosilver preparation device according to any one of claims 1 to 6, characterized in that: The anion exchange mechanism (4) comprises an anion exchange membrane (41), a gasket group and a waterproof rubber ring group; the gasket group comprises two gaskets (42) respectively stacked on both sides of the anion exchange membrane (41); the waterproof rubber ring group comprises a waterproof ring (43) corresponding to the gasket (42) one by one, and the waterproof ring (43) is stacked on the side of the gasket (42) away from the anion exchange membrane (41); The diameter of the anion exchange membrane (41) is larger than the inner diameter of the gasket (42) and smaller than the outer diameter of the gasket (42), and the inner diameter of the waterproof ring (43) is larger than the inner diameter of the gasket (42) and smaller than the outer diameter of the gasket (42).
8. The nanosilver preparation device according to any one of claims 1 to 6, characterized in that: The cooling mechanism (5) comprises a cooling water tank (51), a cooling water tank (52), a first circulation pipe (53), a second circulation pipe (54), a pump unit (55), a flow regulator (56) and an anode tank clamping mechanism (57); Both ends of the first circulation pipe (53) and the second circulation pipe (54) are respectively connected to the cooling water tank (51) and the cooling water tank (52), forming a circulation loop for circulating the cooling liquid (58); the pump unit (55) is connected to the circulation loop and is used to drive the cooling liquid (58) to flow; the flow regulator (56) is arranged on the circulation loop, and along the flow direction of the cooling liquid (58), the flow regulator (56) is located at the rear end of the pump unit (55) to control the output flow of the pump unit (55); the anode tank clamping mechanism (57) is used to install the anode tank (2) on the cooling water tank (52); The dissolution zone (22), cathode tank (3) and anion exchange mechanism (4) of the anode tank (2) are all located in a cooling water tank (52), and the cooling liquid (58) in the cooling water tank (52) can contact the dissolution zone (22), cathode tank (3) and anion exchange mechanism (4).
9. The nanosilver preparation device according to any one of claims 1 to 6, characterized in that: The heating mechanism (6) is configured as a magnetic stirring heating pot; the magnetic stirring heating pot comprises a heating pot body (61) wrapped around the outer periphery of the reduction zone (23) and a magnetic stirring bar (62) arranged at the bottom of the reduction zone (23).
10. A method for preparing nano silver, characterized in that: The nano silver preparation device according to any one of claims 1 to 9 is used, and the preparation method comprises: The cooling mechanism (5) and the heating mechanism (6) are started, and a current of a predetermined value is applied between the anode (11) and the cathode (12) to perform constant current electrolysis; hydrogen (33) is precipitated on the surface of the cathode (12), and the anode (11) loses electrons to generate silver ions which enter the polyol solution (21); the silver ions reach the reduction zone (23) of the anode tank (2) through diffusion, and the silver ions in the reduction zone (23) react with the polyol solution (21) heated by the heating mechanism (6) to generate nano silver (7).