A kind of wormwood and hyaluronic acid modified plant-based fiber and preparation method thereof
Through modified cellulose and electrospinning technology, the problem of poor affinity between mugwort extract and hyaluronic acid on plant-based fibers is solved, stable loading and sustained release of active ingredients are achieved, and the functionality and stability of the fiber are improved. Improves the fiber's moisturizing and antibacterial properties.
Patent Information
- Application Number
- CN202410401678.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-04-03
AI Technical Summary
In the existing technology, mugwort extract and hyaluronic acid have poor affinity when applied on plant-based fibers, resulting in the waste of active ingredients and reduced efficacy, and it is difficult to fully exert the stability and moisturizing effects.
By preparing modified cellulose, combining surface modification treatment with acetic anhydride and anhydrous pyridine, and treating mugwort crude fiber with alkaline and acidic solutions, mugwort extract is prepared, and compounded with hyaluronic acid through electrospinning technology. Form modified plant-based fiber, improve the affinity of fiber with mugwort and hyaluronic acid, and achieve stable loading and sustained release of active ingredients.
It improves the utilization and stability of active ingredients, enhances the functionality of the fiber, reduces the elution rate, and improves the toughness and moisturizing ability of the fiber, while maintaining the natural characteristics and antibacterial properties of the fiber.
Smart Images

Figure BDA0004775834960000181
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fiber manufacturing, and in particular to a plant-based fiber modified with wormwood and hyaluronic acid and a preparation method thereof. Background Art
[0002] Hyaluronic acid, scientifically known as "hyaluronic acid" (HA for short), is an acidic mucopolysaccharide. HA used in industrial production usually exists in the form of sodium salt, namely sodium hyaluronic acid. Hyaluronic acid is widely present in the interstitial matrix of vertebrate tissue cells. Its structure is a linear high-molecular mucopolysaccharide substance composed of D-glucuronic acid and N-acetylglucosamine as disaccharide units repeatedly cross-linked through β-(1,4) glycosidic bonds and β-(1,3) glycosidic bonds. The amount of the two monosaccharides in the molecule is 1:1, and the relative molecular mass ranges from thousands to millions of Daltons. Hyaluronic acid has excellent moisturizing function. Hyaluronic acid with a smaller molecular weight penetrates the surface of the skin, can provide nutritional supplements to the skin, nourish and delay skin aging. Hyaluronic acid is a high-molecular polymer, and it also has the effects of lubrication, regulating physiological functions, and eliminating static electricity.
[0003] With the development of modern science and technology and the enhancement of people's health awareness, natural plant-based materials are gaining more and more attention due to their green, environmentally friendly and sustainable characteristics. The application of plant-based fibers in textiles, medical and health care, cosmetics and other fields is increasing, especially in functional products with specific biological activities.
[0004] As a herb with rich medical and health value, the extract of mugwort contains rich bioactive ingredients, such as volatile oils and flavonoids, which have good antibacterial, anti-inflammatory and skin repair effects. As a natural moisturizing factor, the application of hyaluronic acid in fiber modification will help improve the moisturizing properties and biocompatibility of fibers, thereby meeting the market demand for high-quality, healthy and environmentally friendly textiles.
[0005] However, there are some technical difficulties in directly applying wormwood extract and hyaluronic acid to plant-based fibers. First, the physical and chemical properties of wormwood extract and hyaluronic acid have poor affinity with plant-based fibers and are easily eluted during use, resulting in waste of active ingredients and rapid decline in efficacy. Second, the stability of wormwood extract and the long-term moisturizing effect of hyaluronic acid are difficult to fully exert on untreated plant-based fibers.
[0006] In order to solve the above problems, it is necessary to develop a plant-based fiber modified with mugwort and hyaluronic acid and a preparation method thereof to achieve stable loading and sustained release of active ingredients while maintaining the natural properties of the fiber and enhancing its functionality. Summary of the invention
[0007] The purpose of the present invention is to provide a plant-based fiber modified with mugwort and hyaluronic acid and a preparation method thereof. The present invention can not only improve the utilization rate and stability of the active ingredients, but also enhance the functionality of the plant-based fiber, providing a new idea and method for the development and application of natural plant-based functional materials.
[0008] On the one hand, the present invention provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.1-0.12): (0.2-0.26): (0.4-0.6).
[0009] Furthermore, the preparation method of the modified cellulose comprises: ultrasonically dispersing pine pulp and flax pulp in anhydrous pyridine to obtain a pine pulp and flax pulp suspension, adding acetic anhydride and anhydrous pyridine and stirring, and dialyzing and freeze-drying to obtain the modified cellulose.
[0010] Furthermore, the usage ratio of the pine pulp and flax pulp, anhydrous pyridine and acetic anhydride is (2-3) g: (2-3) g: (100-125) mL: (30-40) mL.
[0011] Furthermore, the preparation method of the modified cellulose comprises: weighing 5-6 g of pine pulp and flax pulp, ultrasonicating in 78-100 mL of anhydrous pyridine for 15-20 min to obtain a suspension of pine pulp and flax pulp, adding 30-40 mL of acetic anhydride and 22-25 mL of anhydrous pyridine, stirring at 80-90° C. for 7-9 h, and obtaining modified cellulose through dialysis and freeze drying.
[0012] Furthermore, the preparation method of the wormwood extract includes: dispersing the wormwood crude fiber in an alkaline solution, washing after heating to obtain alkali-treated fibers, then adding them into an acidic solution and stirring for reaction, collecting the upper suspension by centrifugation after the reaction is completed, obtaining a cellulose suspension after ultrasonic dialysis, and freeze-drying to obtain the wormwood extract.
[0013] Furthermore, the alkaline solution is a 4-6% NaOH solution, and the acidic solution is a 62-66% sulfuric acid solution.
[0014] Furthermore, the usage ratio of the wormwood crude fiber to the alkaline solution is (8-12) g: (100-200) mL; the usage ratio of the alkali-treated fiber to the acidic solution is (4-6) g: (80-120) mL.
[0015] Furthermore, the centrifugal separation step includes: centrifuging at 2500-3500 r / min for 8-12 min, removing the supernatant, adding 40-60 mL of distilled water to wash the precipitate, centrifuging at 8500-9500 r / min for 8-12 min, removing the supernatant, and repeating 3-5 times.
[0016] Furthermore, the preparation method of the wormwood extract comprises: weighing 9-11g of wormwood crude fiber and dispersing it in a 4-6% NaOH solution, heating the suspension at 75-85°C for 0.5-1.5h, washing the fiber with deionized water for multiple times until the pH value of the washing liquid reaches neutral, and drying to constant weight under vacuum conditions; at a temperature of 40-50°C, weighing 4-6g of the treated fiber and adding it to 90-110mL of a 62-66% sulfuric acid solution, stirring it magnetically for 1-3h, and then fully hydrating it; The mixture was centrifuged at 2500-3500 r / min for 8-12 min, and the supernatant was removed. 40-60 mL of distilled water was added to wash the precipitate, and the mixture was centrifuged at 8500-9500 r / min for 8-12 min, and the supernatant was removed. The mixture was repeated 3-5 times and the upper suspension was collected. The mixture was ultrasonicated for 15-25 min, and the pH was neutralized by using distilled water at 3-5° C. to obtain a cellulose suspension, which was freeze-dried to obtain an wormwood extract.
[0017] Plant fibers contain a large number of hydroxyl groups and there are strong hydrogen bonds between molecules. Therefore, the strong polarity exhibited by plant fibers is a very important defect that limits the application of plant fibers, and the large amount of water absorption caused by the hydroxyl groups causes the fibers to absorb a large amount of water, causing fiber aging; and the strong polarity causes the fiber surface to exhibit a large surface tension, resulting in poor wettability with resin matrices containing CH bonds, which easily causes interface debonding; therefore, in the present invention, the surfaces of pine pulp and flax pulp are first modified, and then the wormwood extract is prepared in conjunction with the preparation method of the wormwood extract provided by the present invention, and the wormwood extract is acted on the modified cellulose together with hyaluronic acid, which not only improves the two original defects of the plant fiber, but also retains the performance of the plant fiber itself, and increases the functionality of the plant fiber, which is of great significance for expanding its application.
[0018] On the other hand, the present invention also provides a method for preparing plant-based fibers modified with mugwort and hyaluronic acid, the steps comprising: (1) preparing modified cellulose and mugwort extract; (2) preparing plant-based fibers modified with mugwort and hyaluronic acid: stirring distilled water, adding modified cellulose, mugwort extract and hyaluronic acid to obtain a spinning solution, and performing electrospinning to obtain the obtained fiber.
[0019] Furthermore, during the electrospinning, the humidity of the electrospinning box is 28-32%, the spinning voltage is 18-22 KV, the spinning distance is 18-22 cm, the extrusion volume is 0.35-0.37 ml / h, and the receiving roller speed is 90-110 r / min.
[0020] The beneficial effects of the present invention are:
[0021] (1) The modified plant-based fiber of the present invention is configured with different raw materials and components, and uses modified cellulose, wormwood extract and hyaluronic acid as raw materials, thereby solving the problem of poor affinity when wormwood extract and hyaluronic acid are directly applied to the plant-based fiber, achieving stable loading and sustained release of active components in wormwood extract and hyaluronic acid, while maintaining the natural characteristics of the fiber and enhancing its functionality;
[0022] (2) The present invention uses acetic anhydride and anhydrous pyridine to modify the surface of plant-based fiber pine pulp and flax pulp, which can effectively improve the affinity between the fiber and wormwood and hyaluronic acid, and the modified plant-based fiber is compounded with wormwood fiber and hyaluronic acid. The modified plant-based fiber with sustained release functionality is prepared through electrospinning technology, which also effectively improves the stability of the active ingredient and reduces elution during use;
[0023] (3) In the present invention, the wormwood crude fiber is treated with an alkaline solution and an acidic solution in sequence, the upper suspension is collected by centrifugation, a cellulose suspension is obtained after ultrasonic dialysis, and the wormwood extract is obtained by freeze-drying. The obtained extract is used as a nano wormwood cellulose material. This preparation method also improves the problems of strong polarity and water absorption of the original fiber to a certain extent, based on which the elution property of the antibacterial ability of wormwood can be reduced, and the antibacterial performance of the fiber material itself can be maintained;
[0024] (4) Based on the fact that the wormwood and hyaluronic acid modified plant-based fibers prepared by the present invention have a certain water content, the humidity of the electrospinning box is controlled to be 28-32% during electrospinning, and the spinning voltage is 18-22KV, the spinning distance is 18-22cm, the extrusion volume is 0.35-0.37ml / h, and the receiving roller speed is 90-110r / min. This can effectively improve the toughness and moisturizing ability of the fiber, and spinning under such conditions can also effectively improve the antibacterial ability after washing. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] All raw materials not specified in the following examples are commercially available, among which Staphylococcus aureus was purchased from Shanghai Luwei Technology Co., Ltd., and Escherichia coli was purchased from Shanghai Luwei Technology Co., Ltd.
[0027] Example 1
[0028] This embodiment provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0029] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0030] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0031] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% sulfuric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0032] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added, and 0.11 g of modified cellulose, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid were added under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0033] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0034] Example 2
[0035] This embodiment provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.1): (0.2): (0.4); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0036] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0037] (1) Preparation of modified cellulose: 2 g of pine pulp and 3 g of flax pulp were weighed and ultrasonicated in 80 mL of anhydrous pyridine for 15 min to obtain a suspension of pine pulp and flax pulp, 30 mL of acetic anhydride and 22 mL of anhydrous pyridine were added, and the mixture was stirred at 80° C. for 7 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0038] (2) Preparation of mugwort extract: Weigh 9 g of wormwood crude fiber and disperse it in 4% NaOH solution, and stir evenly; heat the suspension at 75°C for 0.5 h, wash the fiber repeatedly with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 4 g of the treated fiber and add 90 mL of 62% sulfuric acid at 40°C, stir magnetically for 1 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 2500 r / min for 8 min, remove the supernatant, add 40 mL of distilled water to wash the precipitate, centrifuge at 8500 r / min for 8 min, remove the supernatant, repeat 3 times, collect the upper suspension, ultrasonicate for 15 min, dialyze with distilled water at 3°C to neutral pH, obtain a cellulose suspension, freeze-dry, and obtain a wormwood extract;
[0039] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.1 g of modified cellulose, 0.2 g of wormwood extract and 0.4 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0040] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0041] Example 3
[0042] This embodiment provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.12): (0.26): (0.6); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0043] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0044] (1) Preparation of modified cellulose: 3 g of pine pulp and 3 g of flax pulp were weighed and ultrasonicated in 100 mL of anhydrous pyridine for 20 min to obtain a suspension of pine pulp and flax pulp, 40 mL of acetic anhydride and 25 mL of anhydrous pyridine were added, and the mixture was stirred at 90° C. for 9 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0045] (2) Preparation of mugwort extract: Weigh 11 g of wormwood crude fiber and disperse it in a 6% NaOH solution, and stir evenly; heat the suspension at 85°C for 1.5 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 6 g of the treated fiber and add 110 mL of 66% sulfuric acid at 50°C, stir magnetically for 2.5 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3500 r / min for 12 min, remove the supernatant, add 60 mL of distilled water to wash the precipitate, centrifuge at 9500 r / min for 12 min, remove the supernatant, repeat 5 times, collect the upper suspension, ultrasonicate for 25 min, dialyze with distilled water at 5°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0046] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.12 g of modified cellulose, 0.26 g of wormwood extract and 0.6 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0047] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0048] Example 4
[0049] This embodiment provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.26): (0.4); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0050] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0051] (1) Preparation of modified cellulose: 3 g of pine pulp and 3 g of flax pulp were weighed and ultrasonicated in 80 mL of anhydrous pyridine for 15 min to obtain a suspension of pine pulp and flax pulp, 40 mL of acetic anhydride and 22 mL of anhydrous pyridine were added, and the mixture was stirred at 80° C. for 9 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0052] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 6% NaOH solution, stir evenly; heat the suspension at 85°C for 1 h, wash the fiber repeatedly with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 6 g of the treated fiber and add 110 mL of 65% sulfuric acid at 50°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3500 r / min for 10 min, remove the supernatant, add 55 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 5 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, freeze-dry, and obtain a wormwood extract;
[0053] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added, and 0.26 g of modified cellulose, 0.26 g of wormwood extract and 0.6 g of hyaluronic acid were added under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0054] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0055] Comparative Example 1
[0056] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include pine pulp and flax pulp, mugwort extract and hyaluronic acid in a weight ratio of (0.05): (0.06): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0057] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0058] (1) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% sulfuric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0059] (2) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.05 g of pine pulp and 0.06 g of flax pulp, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0060] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0061] Comparative Example 2
[0062] This comparative example provides a mugwort modified plant-based fiber, the raw materials comprising modified cellulose and mugwort extract in a weight ratio of (0.11): (0.23);
[0063] The method for preparing the wormwood modified plant-based fiber comprises the following steps:
[0064] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0065] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% sulfuric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0066] (3) Preparation of modified wormwood plant-based fiber: 10 g of distilled water was added with 0.11 g of modified cellulose and 0.23 g of wormwood extract under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood modified plant-based fiber was obtained after electrospinning;
[0067] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0068] Comparative Example 3
[0069] This comparative example provides a hyaluronic acid modified plant-based fiber, the raw materials include modified cellulose and hyaluronic acid in a weight ratio of (0.11): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0070] The method for preparing the hyaluronic acid-modified plant-based fiber comprises the following steps:
[0071] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0072] (2) Preparation of hyaluronic acid modified plant-based fibers: 0.11 g of modified cellulose and 0.5 g of hyaluronic acid were added to 10 g of distilled water under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0073] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0074] Comparative Example 4
[0075] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort powder and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0076] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0077] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0078] (2) Artemisia argyi powder was commercially available from China Merchants Health Industry Qichun Co., Ltd.;
[0079] (3) Preparation of plant-based fibers modified with mugwort and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of mugwort powder and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the plant-based fibers modified with mugwort and hyaluronic acid were obtained after electrospinning;
[0080] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0081] Comparative Example 5
[0082] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort essential oil and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0083] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0084] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0085] (2) Artemisia argyi essential oil was commercially available from Shanghai Xinya New Material Technology Co., Ltd.;
[0086] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of wormwood essential oil and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0087] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0088] Comparative Example 6
[0089] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0090] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0091] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0092] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add it to 100 mL of deionized water at 45°C, stir it magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0093] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0094] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0095] Comparative Example 7
[0096] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0097] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0098] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0099] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in deionized water, stir evenly; heat the suspension at 80°C for 1 h, wash the fiber repeatedly with deionized water until the pH value of the washing liquid reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% sulfuric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, sonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, freeze-dry, and obtain a wormwood extract;
[0100] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0101] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0102] Comparative Example 8
[0103] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0104] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0105] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0106] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% nitric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0107] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0108] During electrospinning, the humidity of the electrospinning box was 30%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0109] Comparative Example 9
[0110] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0111] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0112] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0113] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% sulfuric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0114] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0115] During electrospinning, the humidity of the electrospinning box was 20%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0116] Comparative Example 10
[0117] This comparative example provides a plant-based fiber modified with mugwort and hyaluronic acid, wherein the raw materials include modified cellulose, mugwort extract and hyaluronic acid in a weight ratio of (0.11): (0.23): (0.5); the average molecular weight of the hyaluronic acid is 50,000 Daltons;
[0118] The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps:
[0119] (1) Preparation of modified cellulose: 2.5 g of pine pulp and 2.5 g of flax pulp were weighed and ultrasonicated in 90 mL of anhydrous pyridine for 17 min to obtain a suspension of pine pulp and flax pulp, 35 mL of acetic anhydride and 24 mL of anhydrous pyridine were added, and the mixture was stirred at 85° C. for 8 h. The modified cellulose was obtained after dialysis and freeze-drying;
[0120] (2) Preparation of mugwort extract: Weigh 10 g of wormwood crude fiber and disperse it in 5% NaOH solution, and stir evenly; heat the suspension at 80°C for 1 h, repeatedly wash the fiber with deionized water until the pH value of the washing solution reaches neutral, and dry it in a vacuum to constant weight; weigh 5 g of the treated fiber and add 100 mL of 64% sulfuric acid at 45°C, stir magnetically for 2 h to fully hydrolyze, and add 10 times the volume of distilled water to terminate the reaction; centrifuge at 3000 r / min for 10 min, remove the supernatant, add 50 mL of distilled water to wash the precipitate, centrifuge at 9000 r / min for 10 min, remove the supernatant, repeat 4 times, collect the upper suspension, ultrasonicate for 20 min, dialyze with distilled water at 4°C to a neutral pH, obtain a cellulose suspension, and freeze-dry to obtain a wormwood extract;
[0121] (3) Preparation of plant-based fibers modified with wormwood and hyaluronic acid: 10 g of distilled water was added with 0.11 g of modified cellulose, 0.23 g of wormwood extract and 0.5 g of hyaluronic acid under stirring conditions of a water bath magnetic stirrer at 70° C. to obtain a spinning solution, and the wormwood and hyaluronic acid modified plant-based fibers were obtained after electrospinning;
[0122] During electrospinning, the humidity of the electrospinning box was 40%, the spinning voltage was 20 KV, the spinning distance was 20 cm, the extrusion volume was 0.36 ml / h, and the speed of the receiving roller was 100 r / min.
[0123] Test Example: The properties of the wormwood and hyaluronic acid modified plant-based fibers prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-10 were explored, and the prepared wormwood and hyaluronic acid modified plant-based fibers were tested as follows:
[0124] Mechanical properties test: The test method is based on GB / T 14344. No less than 30 test specimens are tested and the average test value is taken.
[0125] Hygroscopicity: Take 10g of each sample to be tested and place it in a drying oven at 80°C to dry to constant weight. Record the weight of each sample after drying, recorded as W0. Place each dried sample in an environment with a temperature of 37°C and a relative humidity of 90% for 8h, and measure the weight of each sample after moisture absorption, recorded as W1. Moisture absorption rate (%) = (W1-W0) / W0×100;
[0126] Antibacterial performance test: According to the method in GB / T20944.3-2008, the inhibition rate of each wormwood and hyaluronic acid modified plant-based fiber on Staphylococcus aureus and Escherichia coli was tested, and the inhibition rate on Staphylococcus aureus and Escherichia coli was tested after washing 100 times.
[0127] The test results are shown in Table 1 below:
[0128] Table 1
[0129]
[0130] The dry breaking strength reflects the ability of the fiber to withstand external forces in a dry state. The larger the value, the less likely the fiber is to break when subjected to external forces, and has better tensile resistance. The dry breaking elongation describes the maximum elongation that the fiber can reach before breaking, reflecting the flexibility and ductility of the fiber. The wormwood and hyaluronic acid modified plant-based fibers containing wormwood active ingredients prepared in the aforementioned embodiments have a dry breaking strength of 11.6-12.1cN / tex, a dry breaking elongation of 64-71%, a moisture absorption rate of 39-43%, and an antibacterial rate of up to 99.8%. After 100 washes, the antibacterial rate is not less than 85%, and the antibacterial performance and antibacterial retention performance are excellent.
[0131] Finally, it should be noted that the above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A plant-based fiber modified with wormwood and hyaluronic acid, characterized in that: The raw materials include modified cellulose, wormwood extract and hyaluronic acid in a weight ratio of (0.1-0.12): (0.2-0.26): (0.4-0.6); The preparation method of the modified cellulose comprises: ultrasonically dispersing pine pulp and flax pulp in anhydrous pyridine to obtain a suspension, adding acetic anhydride and anhydrous pyridine, stirring, dialyzing, and freeze-drying to obtain the modified cellulose; The usage ratio of the pine pulp, flax pulp, anhydrous pyridine and acetic anhydride is (2-3) g: (2-3) g: (100-125) mL: (30-40) mL; The preparation method of the wormwood extract comprises: dispersing wormwood crude fiber in an alkaline solution, washing after heating to obtain alkali-treated fiber, then adding it into an acidic solution for stirring and reacting, collecting the upper suspension by centrifugation after the reaction is completed, obtaining a cellulose suspension after ultrasonic dialysis, and freeze-drying to obtain the wormwood extract; The alkaline solution is a 5% NaOH solution, and the acidic solution is a 64% sulfuric acid solution; The usage ratio of the crude wormwood fiber to the alkaline solution is (8-12) g: (100-200) mL; the usage ratio of the alkali-treated fiber to the acidic solution is (4-6) g: (80-120) mL; The method for preparing the wormwood and hyaluronic acid modified plant-based fiber comprises the following steps: preparing modified cellulose and wormwood extract; Preparation of plant-based fibers modified with wormwood and hyaluronic acid: stirring distilled water, adding modified cellulose, wormwood extract and hyaluronic acid to obtain a spinning solution, and performing electrostatic spinning to obtain the obtained fiber; During the electrospinning, the humidity of the electrospinning box is 28-32%, the spinning voltage is 18-22 KV, the spinning distance is 18-22 cm, the extrusion volume is 0.35-0.37 ml / h, and the receiving roller speed is 90-110 r / min.
2. The plant-based fiber modified with wormwood and hyaluronic acid according to claim 1, characterized in that: The centrifugal separation step includes: centrifuging at 2500-3500 r / min for 8-12 min, removing the supernatant, adding 40-60 mL of distilled water to wash the precipitate, centrifuging at 8500-9500 r / min for 8-12 min, removing the supernatant, and repeating 3-5 times.