Reaction equipment and preparation method of poly(p-phenylene terephthalamide)

By using a combination of a micro-mixer and a twin-screw polymerization reactor in the preparation of poly(p-phenylene terephthalamide), the problems of uneven material ratio and temperature control were solved, achieving a highly efficient and stable polymerization reaction and improving product quality.

CN118162079BActive Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211573732.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2026-11-17
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of poly(p-phenylene terephthalamide) suffers from problems such as uneven material ratio, difficulty in local temperature control, and the occurrence of hot spots, resulting in unstable product quality.

Method used

A reaction apparatus is used, comprising a micro mixer, a prepolymer reactor, and a twin-screw polymerization reactor. The micro mixer achieves material mixing within seconds, the prepolymer reactor maintains good material mixing, and the twin-screw polymerization reactor completes the polymerization reaction. The reaction process is rationally designed.

Benefits of technology

It achieves rapid and uniform mixing and efficient polymerization of materials, ensures stable product quality, solves the temperature control problem, improves the specific concentration and logarithmic viscosity of the product, and ensures the smooth progress of the polymerization reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118162079B_ABST
    Figure CN118162079B_ABST
Patent Text Reader

Abstract

This invention relates to the field of polymer preparation, and discloses a reaction apparatus and a method for preparing poly(p-phenylene terephthalamide). The reaction apparatus of this invention includes a micro-mixer, a prepolymerization reactor, and a twin-screw polymerization reactor connected in sequence. The prepolymerization reactor has a double-tube structure, with the inner tube being a hollow tube located on the central axis. A reaction zone is formed between the inner surface of the outer tube and the outer surface of the inner tube. The hollow tube is rotatable and equipped with internal component units, each including two or more fins. When used in the preparation method of poly(p-phenylene terephthalamide), the reaction apparatus of this invention enables rapid mixing of materials within seconds using the micro-mixer. The pre-reaction unit maintains a good mixing state of the materials and achieves preliminary polymerization, increasing the viscosity of the materials. The subsequent twin-screw polymerization reactor completes the polymerization reaction. The reaction process is rationally designed, resulting in high and stable product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer preparation, specifically to a reaction apparatus and a method for preparing poly(p-phenylene terephthalamide). Background Technology

[0002] Poly(p-phenylene terephthalamide) fiber, also known as para-aramid, is a high-tech synthetic fiber and a type of aromatic polyamide fiber. It possesses excellent properties such as high strength, high modulus, high temperature resistance, chemical corrosion resistance, and light weight. Its strength is 5-6 times that of steel wire, its modulus is 2-3 times that of steel wire and glass fiber, its toughness is twice that of steel wire, while its weight is only about 20% of that of steel wire. It has wide applications in aerospace, personal protective equipment, structural materials, and friction sealing materials.

[0003] Currently, the industrial-scale synthesis method for PPTA is the low-temperature solution polycondensation method. This method involves using terephthaloyl chloride and p-phenylenediamine as raw materials under low-temperature conditions in an amide-type aprotic polar solvent system, such as hexamethylphosphoramide, N-methylpyrrolidone, and dimethylacetamide, to polymerize and produce PPTA. p-Phenylenediamine can be dissolved in the solvent system to form a liquid for easy transport. However, terephthaloyl chloride (melting point 78℃) can undergo side reactions with the solvent, leading to substandard specific concentration and logarithmic viscosity of the product. Therefore, it can only be added to the reactor as a solid powder or melt droplet. Adding solid powder results in uneven material distribution in some areas, while melt feeding generates a large amount of heat, which is detrimental to temperature control and also presents the problem of high local concentrations of terephthaloyl chloride. The main challenges in production are controlling the reactor temperature to prevent hot spots and rapidly and efficiently dispersing the materials to achieve the optimal reaction molar ratio. Summary of the Invention

[0004] The purpose of this invention is to provide a reaction apparatus and a method for preparing poly(p-phenylene terephthalamide) using the reaction apparatus. When the reaction apparatus of this invention is used in the preparation method of poly(p-phenylene terephthalamide), it can achieve rapid mixing of materials within seconds using a micro-mixer, maintain a good mixing state of the materials through a pre-reaction unit and achieve preliminary polymerization to increase the viscosity of the materials, and then complete the polymerization reaction through a subsequent twin-screw polymerization reactor. The reaction process is rationally designed, resulting in high and stable product quality.

[0005] To achieve the above objectives, the present invention provides a reaction apparatus comprising a micro mixer, a prepolymer reactor, and a twin-screw polymerization reactor connected in sequence. The prepolymer reactor has a double-layer tube structure, wherein the inner tube is a hollow tube located on the central axis of the tube, and a reaction zone is formed between the inner surface of the outer tube and the outer surface of the inner tube. The hollow tube is rotatable and is provided with an internal component unit, wherein the internal component unit includes two or more fins.

[0006] Preferably, there are multiple internal component units, which are arranged side by side along the length of the hollow tube.

[0007] Preferably, each internal component unit includes two or more fins of different sizes, and the fins of different sizes are arranged alternately at equal intervals on the circumference of the hollow tube.

[0008] Preferably, each internal component unit includes two fins of different sizes, and the two fins of different sizes are arranged alternately at equal intervals on the circumference of the hollow tube.

[0009] Preferably, at least a portion of the fins have holes, and auxiliary strips for increasing material flow disturbance are provided in the holes.

[0010] Preferably, each internal component unit includes two fins of different sizes, which are arranged alternately at equal intervals on the circumference of the hollow tube. The larger fin has holes, and auxiliary strips for increasing material flow disturbance are provided in the holes.

[0011] Preferably, the auxiliary strip is a serrated auxiliary strip.

[0012] Preferably, the number of fins is 4-10.

[0013] Preferably, the micromixer is a microchannel mixer, and the size of the microchannel is 0.2-2 mm.

[0014] Preferably, the reaction apparatus further includes a first material supply unit.

[0015] Preferably, the reaction apparatus further includes a second material supply unit.

[0016] According to a second aspect of the present invention, a method for preparing poly(p-phenylene terephthalamide) is provided, wherein the method uses the reaction apparatus described in the first aspect of the present invention, comprising: sequentially feeding a solution containing a reaction solvent, a chloride and p-phenylene diamine and molten terephthaloyl chloride into the microreactor, the prepolymerization reactor and the twin-screw polymerization reactor for mixing, prepolymerization and polymerization, wherein the chloride is an alkali metal chloride and / or an alkaline earth metal chloride.

[0017] Preferably, the mixing temperature is between -10°C and 40°C, and the material residence time is less than 20 seconds.

[0018] Preferably, the prepolymerization temperature is 5-50°C, and the prepolymerization results in a specific logarithmic viscosity of 1-3 dL / g for the material.

[0019] Preferably, the polymerization temperature is 10-80℃, and the prepolymerization results in a specific logarithmic viscosity of the material of 6 dL / g or higher.

[0020] Preferably, the chloride is one or more of calcium chloride, lithium chloride, and magnesium chloride.

[0021] Preferably, the reaction solvent is one or more of N-methylpyrrolidone, N-ethylpyrrolidone, dimethylformamide, dimethylacetamide, dimethylpropionamide, and diethylacetamide.

[0022] Preferably, the weight ratio of the reaction solvent to the chloride is 1:(0.03-0.1).

[0023] Preferably, the concentration of p-phenylenediamine in the solution containing the reaction solvent, chloride and p-phenylenediamine is 0.2-0.5 mol / L.

[0024] Preferably, the molar ratio of p-phenylenediamine to terephthaloyl chloride is 1:(1-1.1).

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] (1) The continuous feeding of materials is achieved by using melt feeding without introducing third-party solvents or changing the existing process route.

[0027] (2) The material is rapidly mixed in seconds by a micro mixer, the material is kept in a good mixed state by a pre-reaction unit and the material is initially polymerized to increase the viscosity of the material, and the polymerization reaction is completed by a subsequent polymerization reactor. The reaction process is reasonably designed and the product quality is high and stable. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of the preparation method of poly(p-phenylene terephthalamide).

[0029] Figure 2 This is a schematic diagram showing the fin structure of the pre-reactor.

[0030] Figure 3 This is a schematic diagram showing the fin structure of the pre-reactor.

[0031] Figure 4 This is a schematic diagram illustrating the structure of a prepolymer reactor.

[0032] Explanation of reference numerals in the attached figures

[0033] 1-First material supply unit, 2-Second material supply unit, 3-First material supply pump, 4-Second material supply pump, 5-Micro mixer, 6-Prepolymer reactor, 7-Twin-screw polymerization reactor Detailed Implementation

[0034] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0035] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium, or internal communication between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0036] Figure 1 This is a schematic diagram of the preparation method of poly(p-phenylene terephthalamide); Figure 2 This is a schematic diagram showing the fin structure of the pre-reactor; Figure 3 This is a schematic diagram showing the fin structure of the pre-reactor; Figure 4 This is a schematic diagram illustrating the structure of a prepolymer reactor. (Example:) Figure 1-4 As shown, the reaction equipment provided by the present invention includes a micro mixer 5, a prepolymer reactor 6 and a twin-screw polymerization reactor 7 connected in sequence. The prepolymer reactor 6 has a double-layer tube structure. The inner tube is a hollow tube located on the central axis of the tube. The inner surface of the outer tube and the outer surface of the inner tube form a reaction zone. The hollow tube is rotatable and is provided with an internal component unit. The internal component unit includes two or more fins.

[0037] In this invention, the internal component unit can be one or more. Preferably, the internal component unit is multiple and arranged in parallel along the length of the hollow tube.

[0038] In the reaction apparatus of the present invention, the length of the prepolymer reactor 6 can be appropriately configured according to the heat and mass transfer requirements of the material. In a specific embodiment, the inner diameter of the outer tube of the prepolymer reactor 6 can be 1-40 cm; preferably, the inner diameter of the outer tube of the prepolymer reactor 6 is 5-20 cm. Furthermore, in a specific embodiment, the length of the prepolymer reactor 6 can be 0.1-30 m; preferably, the length of the prepolymer reactor 6 is 0.5-10 m.

[0039] In the prepolymer reactor 6, when multiple internal component units are arranged side by side along the length of the hollow tube, the spacing between two adjacent internal component units can be 0-5m, preferably 0.1-3m, more preferably 0.1-2m, further preferably 0.1-1m, and even more preferably 0.1-0.5m.

[0040] In this invention, preferably, each internal component unit includes two or more fins of different sizes, and the fins of different sizes are arranged alternately at equal intervals on the circumference of the hollow tube. Preferably, there can be 2 to 5 types of fins of different sizes, for example, 2, 3, 4 or 5 types. Among these, 2 types are particularly preferred, that is, preferably each internal component unit includes 2 types of fins of different sizes, and the fins of the two types of fins of different sizes are arranged alternately at equal intervals on the circumference of the hollow tube.

[0041] In this invention, preferably, at least a portion of the fins have holes, and auxiliary strips for increasing material flow disturbance are disposed within these holes. Because at least a portion of the fins have holes, and auxiliary strips for increasing material flow disturbance are disposed within these holes, the effect of further improving material flow disturbance is achieved.

[0042] Preferably, the auxiliary strip is one or more of a serrated auxiliary strip, a trapezoidal strip, and an irregularly shaped auxiliary strip; more preferably, the auxiliary strip is a serrated auxiliary strip.

[0043] In a particularly preferred embodiment of the invention, the auxiliary strip is an auxiliary strip with serrations on one side.

[0044] In another particularly preferred embodiment of the present invention, the auxiliary strip is an auxiliary strip with serrations on both sides, and the serrations are in the same direction.

[0045] In another particularly preferred embodiment of the invention, the auxiliary strip is an auxiliary strip with serrations on both sides, and the serrations are in opposite directions.

[0046] The preferred number of fins is 4-10, more preferably 6-8, and particularly preferably 6. Specific examples include 4, 5, 6, 7, 8, 9, or 10 fins.

[0047] In a particularly preferred embodiment of the invention, such as Figure 2 and Figure 3 As shown, each internal component unit includes two fins of different sizes. The two fins of different sizes are arranged alternately at equal intervals on the circumference of the hollow tube. The larger fins have holes, and auxiliary strips for increasing material flow disturbance are provided in the holes. The auxiliary strips are serrated auxiliary strips.

[0048] In the reaction apparatus, the hollow tube is used to be filled with a heat exchange medium and to exchange heat with the reactants.

[0049] According to the present invention, preferably, the micromixer is a microchannel mixer, wherein the inner diameter of the microchannel is 0.2-2 mm. Such a micromixer can be a micro-slit dispersion structure, a heart-shaped, umbrella-shaped, or other shaped microchannel reactor plate. The aforementioned micromixer can be commercially available, for example, from Corning Reactor Technologies Co., Ltd., Shandong Haomai Group, Hangzhou Shenshi Energy Saving Technology Co., Ltd., Shandong Weijing Chemical Technology Co., Ltd., Shandong Jinde New Materials Co., Ltd., etc.

[0050] In this invention, the twin-screw polymerization reactor is a device commonly used in the art, which has two screws that can mesh with each other, and can be commercially available.

[0051] According to the present invention, preferably, the reaction apparatus further includes a first material supply unit, which may be, for example, a mixing vessel. In the method for preparing poly(p-phenylene terephthalamide), the first material supply unit is used to prepare a solution containing a reaction solvent, a chloride, and p-phenylene diamine.

[0052] According to the present invention, preferably, the reaction apparatus further includes a second material supply unit, which may be, for example, a storage tank with a heating means. In the method for preparing poly(p-phenylene terephthalamide), the second material supply unit is used to store molten terephthaloyl chloride. To store the molten terephthaloyl chloride, the temperature of the second material supply unit may be greater than or equal to 78°C.

[0053] In this invention, the heating means can be any means that can heat the storage tank, and can be any heating means commonly used in the art, such as a heating jacket.

[0054] According to the present invention, preferably, the reaction apparatus further includes a first material supply pump 3 for feeding the material in the first material supply unit into the microreactor 5.

[0055] According to the present invention, preferably, the reaction apparatus further includes a second material supply pump 4 for feeding the material in the second material supply unit into the microreactor 5.

[0056] According to the present invention, preferably, the reaction apparatus further includes a motor connected to the hollow tube for driving the hollow tube to rotate.

[0057] According to a second aspect of the present invention, a method for preparing poly(p-phenylene terephthalamide) is provided, wherein the method uses the reaction apparatus described in the first aspect of the present invention, comprising: sequentially feeding a solution containing a reaction solvent, a chloride and p-phenylene diamine and molten terephthaloyl chloride into the microreactor 5, the prepolymerization reactor 6 and the twin-screw polymerization reactor 7 for mixing, prepolymerization and polymerization, wherein the chloride is an alkali metal chloride and / or an alkaline earth metal chloride.

[0058] Preferably, the mixing temperature is -10℃ to 40℃, and the material residence time is less than 20 seconds; more preferably, the mixing temperature is -10℃ to 20℃, and the material residence time is 1 to 10 seconds.

[0059] Specific examples of the above-mentioned mixed temperatures include: -10℃, -8℃, -6℃, -4℃, -2℃, 0℃, 2℃, 4℃, 6℃, 8℃, 10℃, 12℃, 14℃, 16℃, 18℃, 20℃, 22℃, 24℃, 26℃, 28℃, 30℃, 32℃, 34℃, 36℃, 38℃, 40℃, etc., as well as the range formed by any two of these values.

[0060] Specific examples of the aforementioned material residence time include: 1 second, 2 seconds, 3 seconds, 4 seconds, 5 seconds, 6 seconds, 7 seconds, 8 seconds, 9 seconds, 10 seconds, 11 seconds, 12 seconds, 13 seconds, 14 seconds, 15 seconds, 16 seconds, 17 seconds, 18 seconds, 19 seconds, 20 seconds, etc., as well as the range formed by any two of these values.

[0061] Preferably, the prepolymerization temperature is 5-50°C, and the prepolymerization results in a specific logarithmic viscosity of 1-3 dL / g; more preferably, the prepolymerization temperature is 5-30°C, and the prepolymerization results in a specific logarithmic viscosity of 1-2 dL / g.

[0062] Specific examples of the prepolymerization temperatures mentioned above include: 5℃, 6℃, 8℃, 10℃, 12℃, 14℃, 16℃, 18℃, 20℃, 22℃, 24℃, 26℃, 28℃, 30℃, 32℃, 34℃, 36℃, 38℃, 40℃, 42℃, 44℃, 46℃, 48℃, 50℃, and the range formed by any two of these values.

[0063] Specific examples of specific logarithmic viscosity include: 1 dL / g, 1.2 dL / g, 1.4 dL / g, 1.6 dL / g, 1.8 dL / g, 2 dL / g, 2.2 dL / g, 2.4 dL / g, 2.6 dL / g, 2.8 dL / g, 3 dL / g, and the range formed by any two of these values.

[0064] In this invention, during the prepolymerization process, the rotation speed of the hollow tube can be 50-1000 rpm; preferably, the rotation speed of the hollow tube is 100-800 rpm; more preferably, the rotation speed of the hollow tube is 200-600 rpm; and even more preferably, the rotation speed of the hollow tube is 300-500 rpm.

[0065] In this invention, preferably, the polymerization temperature is 30-70°C, more preferably, the polymerization temperature is 40-70°C, and the prepolymerization results in a specific logarithmic viscosity of the material of 6 dL / g or higher, for example, 7 dL / g, 8 dL / g, 9 dL / g, 10 dL / g, etc., and any range of any two of these values.

[0066] Examples of the polymerization temperatures mentioned above include: 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, and any range of any two of these values.

[0067] In this invention, preferably, the chloride is one or more of calcium chloride, lithium chloride and magnesium chloride; more preferably, the chloride is calcium chloride.

[0068] In this invention, preferably, the reaction solvent is one or more of N-methylpyrrolidone, N-ethylpyrrolidone, dimethylformamide, dimethylacetamide, dimethylpropionamide, and diethylacetamide; more preferably, the reaction solvent is N-methylpyrrolidone and / or N-ethylpyrrolidone.

[0069] In this invention, preferably, the weight ratio of the reaction solvent to the chloride is 1:(0.03-0.1); more preferably, the weight ratio of the reaction solvent to the chloride is 1:(0.05-0.5); even more preferably, the weight ratio of the reaction solvent to the chloride is 1:(0.05-0.1).

[0070] In this invention, preferably, the concentration of p-phenylenediamine in the solution containing the reaction solvent, chloride, and p-phenylenediamine is 0.2-0.5 mol / L; more preferably, the concentration of p-phenylenediamine in the solution containing the reaction solvent, chloride, and p-phenylenediamine is 0.3-0.4 mol / L.

[0071] In this invention, preferably, the molar ratio of p-phenylenediamine to terephthaloyl chloride is 1:(1-1.1); more preferably, the molar ratio of p-phenylenediamine to terephthaloyl chloride is 1:(1-1.05).

[0072] In one specific embodiment of the present invention, such as Figure 1 As shown, the reaction equipment includes a first material supply unit 1, a second material supply unit 2, a first material supply pump 3, a second material supply pump 4, a micro mixer 5, a prepolymerization reactor 6, and a twin-screw polymerization reactor 7. The first material stream is pumped through the first material supply unit 1 and via the first material supply pump 3, and the second material stream is pumped through the second material supply unit 2 and via the second material supply pump 4. The two material streams enter the micro reactor 5, the prepolymerization reactor 6, and the twin-screw polymerization reactor 7 in sequence for mixing, prepolymerization, and polymerization.

[0073] The present invention will be described in detail below through embodiments, but the present invention is not limited to the following embodiments.

[0074] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.

[0075] Example 1

[0076] This embodiment is in Figure 1 The reaction is carried out in the shown reaction apparatus, which includes a first material supply unit 1 (batching vessel), a second material supply unit 2 (high-temperature storage tank), a first material supply pump 3, a second material supply pump 4, a micro mixer 5, a prepolymerization reactor 6, and a twin-screw polymerization reactor 7. The first material stream is pumped through the first material supply unit 1 and via the first material supply pump 3, and the second material stream is pumped through the second material supply unit 2 and via the second material supply pump 4. The two material streams enter the micro reactor 5, the prepolymerization reactor 6, and the twin-screw polymerization reactor 7 in sequence for mixing, prepolymerization, and polymerization.

[0077] The prepolymer reactor has the following structure: the inner diameter of the outer tube is 6 cm, and the length of the prepolymer reactor 6 is 2 m. Within the prepolymer reactor 6, internal component units are arranged side-by-side along the length of the hollow tube, with a spacing of 0.15 m between adjacent internal component units. Each internal component unit includes two different fin sizes, which are alternately arranged at equal intervals on the circumference of the hollow tube. The larger fins have holes, and auxiliary strips for increasing material flow disturbance are installed within these holes. These auxiliary strips are serrated on one side. Furthermore, the rotational speed of the prepolymer reactor during prepolymerization is 300 rpm.

[0078] The specific steps are as follows:

[0079] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.5dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.8dL / g.

[0080] Example 2

[0081] This embodiment is carried out in the same reaction apparatus as in Example 1, and the specific steps are as follows:

[0082] Weighed N-ethylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.2dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.1dL / g.

[0083] Example 3

[0084] This embodiment is carried out in the same reaction apparatus as in Example 1, and the specific steps are as follows:

[0085] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.1. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.3dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.1dL / g.

[0086] Example 4

[0087] This embodiment is carried out in the same reaction apparatus as in Example 1, and the specific steps are as follows:

[0088] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, maintaining a molar ratio of 1:1.05 for p-phenylenediamine to terephthaloyl chloride. The micro-mixer was a T-type micro-mixer (0.5 mm inner diameter), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.2dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.7dL / g.

[0089] Example 5

[0090] This embodiment is carried out in the same reaction apparatus as in Example 1, and the specific steps are as follows:

[0091] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (p-phenylenediamine) was added at a concentration of 0.3 mol / L. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet-type micro-mixer (holding capacity 250 ml), with a controlled temperature of 10°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.6dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.2dL / g.

[0092] Example 6

[0093] This embodiment is carried out in the same reaction apparatus as in Example 1, and the specific steps are as follows:

[0094] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 30°C and the material residence time is 10 seconds. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.9 dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60°C and the total reaction time is 15 minutes. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.3 dL / g.

[0095] Example 7

[0096] This embodiment is in Figure 1The reaction is carried out in the shown reaction apparatus, which includes a first material supply unit 1 (batching vessel), a second material supply unit 2 (high-temperature storage tank), a first material supply pump 3, a second material supply pump 4, a micro mixer 5, a prepolymerization reactor 6, and a twin-screw polymerization reactor 7. The first material stream is pumped through the first material supply unit 1 and via the first material supply pump 3, and the second material stream is pumped through the second material supply unit 2 and via the second material supply pump 4. The two material streams enter the micro reactor 5, the prepolymerization reactor 6, and the twin-screw polymerization reactor 7 in sequence for mixing, prepolymerization, and polymerization.

[0097] The prepolymer reactor has the following structure: the inner diameter of the outer tube is 16 cm, and the length of the prepolymer reactor 6 is 4 m. Within the prepolymer reactor 6, internal component units are arranged side-by-side along the length of the hollow tube, with a spacing of 0.15 m between adjacent internal component units. Each internal component unit includes two different sized fins, which are alternately arranged at equal intervals on the circumference of the hollow tube. The larger fins have holes, and auxiliary strips with serrations are installed within these holes to increase material flow disturbance. Furthermore, the rotational speed of the prepolymer reactor during prepolymerization is 300 rpm.

[0098] The specific steps are as follows:

[0099] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.4dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.4dL / g.

[0100] Example 8

[0101] This embodiment is in Figure 1The reaction is carried out in the shown reaction apparatus, which includes a first material supply unit 1 (batching vessel), a second material supply unit 2 (high-temperature storage tank), a first material supply pump 3, a second material supply pump 4, a micro mixer 5, a prepolymerization reactor 6, and a twin-screw polymerization reactor 7. The first material stream is pumped through the first material supply unit 1 and via the first material supply pump 3, and the second material stream is pumped through the second material supply unit 2 and via the second material supply pump 4. The two material streams enter the micro reactor 5, the prepolymerization reactor 6, and the twin-screw polymerization reactor 7 in sequence for mixing, prepolymerization, and polymerization.

[0102] The prepolymer reactor has the following structure: the inner diameter of the outer tube is 6 cm, and the length of the prepolymer reactor 6 is 2 m. Within the prepolymer reactor 6, internal component units are arranged side-by-side along the length of the hollow tube, with a spacing of 0.15 m between adjacent internal component units. Each internal component unit includes two different sized fins, which are alternately arranged at equal intervals on the circumference of the hollow tube. The larger fins have holes, and auxiliary strips for increasing material flow disturbance are installed within these holes. These auxiliary strips are serrated on both sides, with the serrations aligned in the same direction. Furthermore, the rotational speed of the prepolymer reactor during prepolymerization is 300 rpm.

[0103] The specific steps are as follows:

[0104] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.7dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 6.5dL / g.

[0105] Example 9

[0106] This embodiment is in Figure 1The reaction is carried out in the shown reaction apparatus, which includes a first material supply unit 1 (batching vessel), a second material supply unit 2 (high-temperature storage tank), a first material supply pump 3, a second material supply pump 4, a micro mixer 5, a prepolymerization reactor 6, and a twin-screw polymerization reactor 7. The first material stream is pumped through the first material supply unit 1 and via the first material supply pump 3, and the second material stream is pumped through the second material supply unit 2 and via the second material supply pump 4. The two material streams enter the micro reactor 5, the prepolymerization reactor 6, and the twin-screw polymerization reactor 7 in sequence for mixing, prepolymerization, and polymerization.

[0107] The prepolymer reactor has the following structure: the inner diameter of the outer tube is 6 cm, and the length of the prepolymer reactor 6 is 2 m. Within the prepolymer reactor 6, internal component units are arranged side-by-side along the length of the hollow tube, with a spacing of 0.15 m between adjacent internal component units. Each internal component unit includes two different sized fins, which are alternately arranged at equal intervals on the circumference of the hollow tube. The larger fins have holes, and auxiliary strips for increasing material flow disturbance are installed within these holes. These auxiliary strips are serrated on both sides with opposite serration directions. Furthermore, the rotational speed of the prepolymer reactor during prepolymerization is 500 rpm.

[0108] The specific steps are as follows:

[0109] Weighed N-methylpyrrolidone and calcium chloride were added to the mixing vessel at a mass ratio of 1:0.05. After the calcium chloride dissolved, p-phenylenediamine (0.3 mol / L) was added. Terephthaloyl chloride was placed in a high-temperature storage tank and heated to 85°C to dissolve. The two materials were then fed to a micro-mixer via a first material supply pump 3 and a second material supply pump 4, with a molar ratio of p-phenylenediamine to terephthaloyl chloride of 1:1.05. The micro-mixer was a heart-shaped sheet mixer (250 ml capacity), with a controlled temperature of 5°C and a material residence time of 2 seconds. The material flows to the prepolymer reactor, where the temperature is controlled at 10℃ and the material residence time is 10s. The specific logarithmic viscosity at the outlet of the prepolymer reactor reaches 1.9dL / g. Finally, it enters the twin-screw polymerization reactor, where the temperature is controlled at 60℃ and the total reaction time is 15min. The product is washed with water to remove the solvent and dried to obtain poly(p-phenylene terephthalamide) powder with a specific logarithmic viscosity of 7.1dL / g.

[0110] Comparative Example 1

[0111] The method was carried out according to Example 1, except that the prepolymer reactor was an empty tube. The specific concentration logarithmic viscosity of the product was 4.1 dL / g.

[0112] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing poly(p-phenylene terephthalamide), characterized in that, The reaction equipment used in this method includes a micro-mixer, a prepolymer reactor, and a twin-screw polymerization reactor connected in sequence. The prepolymer reactor has a double-tube structure, with the inner tube being a hollow tube located on the central axis. A reaction zone is formed between the inner surface of the outer tube and the outer surface of the inner tube. The hollow tube is rotatable and equipped with internal component units. Each internal component unit includes two fins of different sizes, which are arranged alternately at equal intervals on the circumference of the hollow tube. The larger fins have holes, and auxiliary strips for increasing disturbance are provided in the holes. These auxiliary strips are serrated. The internal component units are multiple and arranged along the length of the hollow tube; The method includes: sequentially feeding a solution containing a reaction solvent, a chloride, and p-phenylenediamine, and molten terephthaloyl chloride into the micromixer, the prepolymer reactor, and the twin-screw polymerization reactor for mixing, prepolymerization, and polymerization, wherein the chloride is an alkali metal chloride and / or an alkaline earth metal chloride.

2. The method according to claim 1, wherein, Each internal component unit has 4-10 fins.

3. The method according to claim 1, wherein, The micro mixer is a microchannel mixer, and the inner diameter of the microchannel is 0.2-2 mm.

4. The method according to claim 1, wherein, The reaction apparatus also includes a first material supply unit.

5. The method according to claim 1, wherein, The reaction equipment also includes a second material supply unit.

6. The method according to claim 1, wherein, The mixing temperature is between -10°C and 40°C, and the material residence time is less than 20 seconds.

7. The method according to claim 1, wherein, The prepolymerization temperature is 5-50℃, and the prepolymerization results in a specific logarithmic viscosity of 1-3 dL / g.

8. The method according to claim 1, wherein, The polymerization temperature is 10-80℃, and the polymerization results in a specific logarithmic viscosity of the material of 6 dL / g or higher.

9. The method according to claim 1, wherein, The chloride is one or more of calcium chloride, lithium chloride, and magnesium chloride.

10. The method according to claim 1, wherein, The reaction solvent is one or more of N-methylpyrrolidone, N-ethylpyrrolidone, dimethylformamide, dimethylacetamide, dimethylpropionamide, and diethylacetamide.

11. The method according to claim 1, wherein, The weight ratio of the reaction solvent to the chloride is 1:0.03-0.

1.

12. The method according to claim 1, wherein, The concentration of p-phenylenediamine in the solution containing the reaction solvent, chloride, and p-phenylenediamine is 0.2-0.5 mol / L.

13. The method according to claim 1, wherein, The molar ratio of p-phenylenediamine to terephthaloyl chloride is 1:1-1.1.

Citation Information

Patent Citations

  • Method for continuously preparing poly-p-phenylene terephthalamide resin

    CN104119526A

  • Micro-reaction system and micro-reaction method for preparing para / meta-aramid

    CN104667846A

  • Tubular reaction kettle for polymer synthesis

    CN209451852U