Preparation method of super soft stainless steel pipe
Ultra-soft stainless steel pipes are prepared through processes such as vacuum induction melting and multi-pass hot rolling, which solves the problems of high hardness and short service life of stainless steel pipes, achieves low hardness and high corrosion resistance, extends service life and reduces costs.
Patent Information
- Application Number
- CN202410248917.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-05
AI Technical Summary
Due to their high hardness, existing stainless steel pipes are difficult to deform and process, and have a short service life. They are prone to cracks in large deformation areas, affecting the performance and safety of refrigeration equipment.
Ultra-soft stainless steel pipes are prepared using vacuum induction melting + vacuum consumable remelting. Through processes such as multi-pass hot rolling, pickling, cold rolling, laser welding, drawing and graded annealing, the material composition and structure are controlled to reduce hardness and Tensile strength, improved deformation ability and corrosion resistance.
It achieves low hardness and low tensile strength of ultra-soft stainless steel pipes, reduces strain-induced martensite, extends service life, reduces material costs, and improves corrosion resistance and mechanical properties.
Smart Images

Figure CN118162499B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of supersoft stainless steel, in particular to a method for preparing a supersoft stainless steel pipe. Background Art
[0002] Statistics from the Chinese Society of Refrigeration show that my country's air-conditioning products account for more than 80% of global production, refrigerators and freezers account for up to 50%, and automotive air-conditioning accounts for more than 30%. Evaporators and condensers are important components of refrigeration equipment such as air conditioners and refrigerators, and their performance directly affects the entire refrigeration system.
[0003] Copper tubes are widely used in the refrigeration industry due to their good processing performance and thermal conductivity. However, copper tubes have poor high pressure resistance and long-term use will affect the refrigeration effect; they are prone to corrosion, leading to refrigerant leakage and endangering personal safety; copper prices fluctuate greatly and the cost is high.
[0004] Stainless steel is cheap and has good pressure resistance. Using stainless steel to make evaporators and condensers can significantly reduce production costs. However, common stainless steel materials have high strength and hardness, low toughness, are not easy to bend and have a short service life. Summary of the invention
[0005] The purpose of the invention is to overcome the shortcomings of stainless steel, such as high hardness, difficulty in deformation processing, easy cracking in large deformation areas and low service life, and provide a method for preparing an ultra-soft stainless steel tube.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing an ultra-soft stainless steel tube comprises the following steps:
[0008] Step 1, smelting:
[0009] The components used to make the ultra-soft stainless steel tube are weighed according to mass percentage and melted by "vacuum induction melting + vacuum consumable remelting";
[0010] Step 2, continuous casting and rolling:
[0011] The molten steel is poured into a continuous casting machine to form a slab, and then hot-rolled in a soaking furnace for multiple passes to obtain a steel plate;
[0012] Hot rolling can break up the coarse grains in the casting state, heal cracks, eliminate casting defects, and improve the plasticity and mechanical properties of the metal;
[0013] Step 3, pickling:
[0014] The steel plate is placed in a pickling solution for pickling;
[0015] The pickling solution is sulfuric acid + nitric acid, the sulfate ion concentration in the pickling solution is 150g / L-350g / L, the nitrate ion concentration in the pickling solution is 30g / L-50g / L, and the temperature of the pickling solution is controlled at 75℃-85℃;
[0016] Step 4, cold rolling:
[0017] Cold rolling the pickled steel plate to obtain a steel plate;
[0018] The hardness and tensile strength of the invention are low, large rolling deformation will not produce large work hardening, and the forming cost can be saved.
[0019] Step 5, cutting:
[0020] Use a splitter to split the steel plates into steel coils;
[0021] Step 6, Bending:
[0022] Passing each steel coil through a multi-stage forming roller to form the steel coil into a pipe;
[0023] Step 7, Soldering:
[0024] The butt joints of the pipes are welded by a laser welding machine to obtain round pipes;
[0025] The angle between the laser beam and the welding direction is 45°, the welding speed is 5mm / s, the beam spot is 1mm, the arc starting current is 80-100A, and the arc ending current is 130-150A; the arc starting current should not be too high to prevent the pipe from being welded through.
[0026] The laser welding in the present invention adopts inert gas protection, which can reduce the generation of inclusions such as ferrous oxide and silicon dioxide and improve welding stability; the heat affected zone after welding is narrow and the impact on the structure is small; by adjusting the laser welding current and welding speed, the generation of pores can be reduced.
[0027] Step 8, pulling:
[0028] The round tube is subjected to high-frequency induction heating by a puller, and pressure is applied to the round tube for pulling, so that the diameter of the round tube is reduced and the thickness of the tube wall is thinned;
[0029] Heating the round tube can improve the deformation capacity of the round tube and reduce residual stress.
[0030] Step 9, heat treatment:
[0031] Put several round tubes into a hydrogen + argon protective atmosphere furnace for annealing. The first stage annealing temperature is 960℃-1000℃, and the insulation time is 8min-12min; the second stage annealing temperature is 1080℃-1120℃, and the insulation time is 3min-5min. Then, each round tube is water-cooled.
[0032] The present invention adopts a drawing + graded annealing process. Drawing can adjust the weld structure and improve the weld performance. The first-stage annealing can recrystallize the ultra-soft stainless steel tube structure, eliminate the coarse grains that occur during laser welding and the grain deformation during the drawing process, and improve the performance of the ultra-soft stainless steel tube. The second-stage annealing can make the grains grow, control the grain size, and reduce the strength and hardness of the material.
[0033] Preferably, the supersoft stainless steel tube is composed of carbon C, nitrogen N, silicon Si, manganese Mn, chromium Cr, nickel Ni, molybdenum Mo, copper Cu, titanium Ti, niobium Nb, vanadium V and iron Fe; the mass percentages of the components in the supersoft stainless steel tube are as follows: C: 0.005%-0.02%, N: 0.05%-0.2%, Si: 0.01%-0.1%, Mn: 1%-7%, Cr: 16%-20%, Ni: 8%-14%, Mo: 0.5%-3.0%, Cu: 1%-6%, Ti: 0.005%-0.015%, Nb: 0.01%-0.25%, V: 0.03%-0.3%, and the balance is iron;
[0034] Among them, Ni equivalent Ni in super soft stainless steel pipe eq ≥26.5;
[0035] Ni eq =Ni+12.93C+1.11Mn+0.72Cr-0.27Si+0.53Cu+
[0036] 7.55N-0.24Ti+0.19Nb+0.9V+0.88Mo;
[0037] The stacking fault formability index SFI in ultra-soft stainless steel tubes is ≥30;
[0038] SFI=2.2Ni+6Cu-1.1Cr-13Si-1.2Mn+32.
[0039] The carbon atoms of the present invention significantly increase the tensile strength and wear resistance of steel through solid solution strengthening. Too much carbon atoms is not suitable, because too much carbon atoms will easily form carbide inclusions at the grain boundaries, resulting in chromium-poor areas, causing severe grain boundary corrosion and reducing the corrosion resistance of the material.
[0040] The nitrogen element of the present invention can improve the stability of austenite, expand the phase region of austenite, reduce the precipitation of intermetallic compounds in steel, reduce the diffusion coefficient of chromium and hinder the nucleation and growth of carbides at grain boundaries.
[0041] The silicon of the present invention acts as a deoxidizer during smelting of austenitic stainless steel and plays a role in controlling the oxygen content.
[0042] The manganese of the present invention is an element that stabilizes austenite, and manganese can be added to steel to improve its hardenability, reduce material costs, increase Ni equivalent, and reduce yield strength and work hardening degree.
[0043] The chromium of the present invention can form a dense Cr layer on the surface of stainless steel. 2 O 3 , enhance the corrosion resistance of steel without affecting the mechanical properties of steel.
[0044] The nickel of the present invention is an element that stabilizes austenite and can also increase the phase region of austenite. The nickel element can reduce the martensitic transformation temperature, and the steel can be made without undergoing martensitic transformation at a lower temperature. The nickel element significantly reduces the cold forming hardening tendency of austenitic stainless steel, ensuring the excellent toughness, cutting performance and weldability of the steel. In addition, nickel also makes austenitic stainless steel non-magnetic, expanding its scope of use.
[0045] The copper of the present invention can expand the austenite phase region, change the Ni equivalent and stacking fault energy, inhibit the austenite stainless steel from inducing martensitic phase transformation, and thus play a softening role. Copper can form metal deposition at the corrosion site to inhibit anode dissolution, reduce chloride ion erosion, and improve corrosion resistance.
[0046] The molybdenum of the present invention is soluble in the matrix and can improve the corrosion resistance and pitting corrosion resistance equivalent number of the material, so that the steel can show better performance in terms of pitting corrosion resistance, crevice corrosion resistance and the like.
[0047] Ni Equivalent eq (Ni equivalent indicates the tendency to form martensite during cooling or deformation) It is calculated based on the intensity of austenitization of austenite elements (such as nickel, carbon, manganese, etc.) contained in the structure and converted into the sum of several nickel equivalents.
[0048] The stacking fault formability index SFI is ≥ 30 (optimally above 35), where SFI refers to the tendency of dislocations to form between adjacent layers in the crystal structure.
[0049] The present invention uses the stacking fault formability index SFI to predict the possibility of stacking faults. When the stacking fault formability index SFI is less than 30, a large number of stacking faults are generated in the matrix, which inhibits the diffusion of dislocations and improves the hardness of austenitic stainless steel.
[0050] Ti and Nb can easily combine with carbon to form carbides, and their ability to combine with C is higher than that of Cr.
[0051] Vanadium can improve the corrosion resistance of austenitic stainless steel and enhance thermal stability.
[0052] The present invention uses an original Ni equivalent formula to control the Ni equivalent. When the ultra-soft stainless steel is deformed, the content of strain-induced martensite is guaranteed, crack initiation at large deformation locations is reduced, and the service life of the ultra-soft stainless steel is increased.
[0053] Preferably, the puller comprises an inner mold rod, an outer mold tube arranged outside the inner mold rod, a high-frequency induction coil arranged on the right side of the inner mold rod and the outer mold tube, and a support tube arranged in the high-frequency induction coil; the aperture of the right part of the outer mold tube is larger than the aperture of the left part of the outer mold tube, and the cross-sectional size of the inner mold rod is adapted to the aperture of the outer mold tube;
[0054] The outer layer of the support tube is made of stainless steel material, and the inner layer of the support tube is made of corundum material.
[0055] Step 8 is replaced by the following steps:
[0056] The staff passes the round tube into the support tube from right to left, and makes the high-frequency induction coil work to perform high-frequency induction heating on the round tube; the round tube continues to move to the left, so that the round tube enters the gap between the inner mold and the outer mold, and the inner mold and the outer mold pull the round tube to reduce the diameter of the round tube and thin the tube wall.
[0057] Preferably, the protective atmosphere furnace comprises a heating chamber and a cooling chamber located on the right side of the heating chamber; a feeding port is provided at the top of the heating chamber, a feeding port sealing cover is provided on the feeding port, a discharging port is provided at the top of the cooling chamber, a discharging port sealing cover is provided on the discharging port; a temperature and pressure sensor and a plurality of heating elements are provided on the heating chamber; the furnace also comprises a hydrogen cylinder, an argon cylinder and a booster pump connected to the heating chamber, the hydrogen cylinder is connected to the booster pump through a first connecting pipe, the argon cylinder is connected to the booster pump through a second connecting pipe, a first solenoid valve and a second solenoid valve are provided on the first connecting pipe and the second connecting pipe respectively; the furnace also comprises a vacuum pump and a waste gas bin connected to the heating chamber, the vacuum pump is connected to the waste gas bin through a third connecting pipe, and a third solenoid valve is provided on the third connecting pipe;
[0058] It also includes a water inlet pump connected to the cooling chamber and a water tank located below the cooling chamber. The water tank is connected to the cooling chamber through a water inlet pipe and a water outlet pipe respectively. The water inlet pump is located on the water inlet pipe. A fourth solenoid valve is also provided on the water inlet pipe. A fifth solenoid valve is provided on the water outlet pipe. The controller is electrically connected to the temperature and pressure sensor, each heating element, a booster pump, a first solenoid valve, a second solenoid valve, a vacuum pump, a third solenoid valve, a water inlet pump, a fourth solenoid valve and a fifth solenoid valve respectively.
[0059] The present invention adopts double vacuum melting, which can reduce oxide inclusions generated during melting and improve the stability of material properties.
[0060] Preferably, step 9 is replaced by the following steps:
[0061] Open the feeding port, put several round tubes into the heating chamber, and cover the feeding port sealing cover; the controller controls the third solenoid valve to open, start the vacuum pump, evacuate the heating chamber, and pump the gas in the heating chamber into the waste gas bin, observe the pressure data detected by the temperature and pressure sensor, and when the air pressure in the heating chamber reaches 1×10 -3 MPa, the vacuum pump is controlled to stop working and the third solenoid valve is closed;
[0062] The controller controls the second solenoid valve to open, controls the booster pump to work, and fills the heating chamber with argon gas. When the gas pressure in the heating chamber reaches 0.1 MPa, the controller controls the second solenoid valve to close, and the booster pump stops working.
[0063] The controller controls the first solenoid valve to open, controls the booster pump to work, and fills hydrogen into the heating chamber. When the gas pressure in the heating chamber reaches 0.3 MPa, the controller controls the first solenoid valve to close, and the booster pump stops working.
[0064] Control each heating element to heat the heating chamber, the first stage annealing temperature is 960℃-1000℃, and the insulation time is 8min-12min; the second stage annealing temperature is 1080℃-1120℃, and the insulation time is 3min-5min; control each heating element to stop working;
[0065] The staff opens the sealing cover of the feeding port and the sealing cover of the discharging port, uses tools to take out each round tube from the heating chamber, puts each round tube into the cooling chamber, and closes the sealing cover of the feeding port and the sealing cover of the discharging port;
[0066] The fourth solenoid valve is controlled to open by the controller, and the water pump starts to work to pump the cooling water in the water tank into the cooling chamber, and the fourth solenoid valve and the water pump are closed;
[0067] After the round tubes have been water-cooled in the cooling chamber for two minutes, the fifth solenoid valve is controlled to open, and the cooling water in the cooling chamber automatically flows back to the water tank. The discharge port is opened, and the staff takes out the round tubes in the cooling chamber.
[0068] The hydrogen+argon annealing adopted in the present invention can reduce the generation of oxide inclusions, improve the stability of the material and improve the mechanical properties.
[0069] Preferably, the splitting machine includes a steel coil for winding the steel plate, a fixed shaft and a rotating shaft located on the right side of the steel coil and parallel to the steel coil and arranged up and down, and a coiling shaft located on the right side of the fixed shaft for winding the split steel coil; it also includes several groups of leveling shafts located between the steel coil and the fixed shaft, and the fixed shaft is provided with several longitudinally distributed splitting knives; step 5 is replaced by the following steps:
[0070] The staff winds the steel plate onto the steel reel, and uses tools to pull the right edge of the steel plate stretched from the steel reel through the upper and lower leveling shafts of each group of leveling shafts. Each group of leveling shafts flattens the curled steel plate; the steel plate passes between the fixed shaft and the rotating shaft, and the rotating shaft drives the steel plate to move to the right. The splitting knife splits the steel plate into 50mm-70mm steel coils of the same width, and the staff winds the steel coils onto the rotating coiling shaft.
[0071] Preferably, the following steps are included between step 7 and step 8:
[0072] X-rays are used to inspect the welded round tubes to detect cracks, weld bumps, pores and slag inclusions; when defects exist in the round tubes, the round tubes are judged as unqualified; and the unqualified round tubes are treated as scrap.
[0073] Preferably, the following steps are also included between step 8 and step 9:
[0074] X-rays are used to detect the thickness of the round tube. When the error between the detected thickness and the theoretical thickness exceeds 5%, the thickness of the round tube is determined to be unqualified and the unqualified round tube is treated as waste.
[0075] Therefore, the present invention has the following beneficial effects: low tensile strength and hardness, almost no strain-induced martensite, easy deformation, low crack initiation rate, and not easy to break when bent. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 is a flow chart of the present invention;
[0077] Figure 2 It is a structural schematic diagram of the protective atmosphere furnace of the present invention;
[0078] Figure 3 It is a structural schematic diagram of the splitting machine of the present invention;
[0079] Figure 4 It is a structural schematic diagram of the puller of the present invention;
[0080] Figure 5 It is a schematic diagram of a heat treatment process of the present invention;
[0081] Figure 6It is a schematic diagram of wall thickness and pressure of Examples 1 to 4 of the present invention. DETAILED DESCRIPTION
[0082] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0083] Example 1
[0084] like Figure 1-Figure 4 The embodiment shown is a method for preparing an ultra-soft stainless steel tube, comprising the following steps:
[0085] Step 1, smelting:
[0086] The components used to make the ultra-soft stainless steel tube are weighed according to the mass percentage, and melted by "vacuum induction melting + vacuum consumable remelting", with the temperature rising at 350℃ / h, melting at 1600℃-1650℃, and keeping the temperature for 30-40min;
[0087] The super-soft stainless steel pipe is composed of carbon C, nitrogen N, silicon Si, manganese Mn, chromium Cr, nickel Ni, molybdenum Mo, copper Cu, titanium Ti, niobium Nb, vanadium V and iron Fe; the mass percentages of the components in the super-soft stainless steel pipe are as follows: C: 0.005%, N: 0.05%, Si: 0.01%, Mn: 6.8%, Cr: 19.7%, Ni: 8.1%, Cu: 5.8%, Mo: 0.62%, Ti: 0.005%, Nb: 0.01%, V: 0.03%, and the balance is iron;
[0088] Among them, Ni equivalent Ni in super soft stainless steel pipe eq ≥26.5.
[0089] Ni eq =Ni+12.93C+1.11Mn+0.72Cr-0.27Si+0.53Cu+
[0090] 7.55N-0.24Ti+0.19Nb+0.9V+0.88Mo;
[0091] The stacking fault formability index SFI in ultra-soft stainless steel tubes is ≥30;
[0092] SFI=2.2Ni+6Cu-1.1Cr-13Si-1.2Mn+32;
[0093] Step 2, continuous casting and rolling:
[0094] The molten steel is poured into a continuous casting machine to form a 3cm thick slab, which is then kept in a soaking furnace at 1150°C for 4 minutes and then hot rolled in multiple passes to finally form a 5mm-10mm thick steel plate.
[0095] Hot rolling can break up the coarse grains in the casting state, heal cracks, eliminate casting defects, and improve the plasticity and mechanical properties of the metal;
[0096] Step 3, pickling:
[0097] Put the steel plate into the pickling solution and pickle for 25s-30s;
[0098] The pickling solution is sulfuric acid + nitric acid, the sulfate ion concentration in the pickling solution is 250g / L, the nitrate ion concentration in the pickling solution is 40g / L, and the temperature of the pickling solution is controlled at 75℃-85℃;
[0099] Step 4, cold rolling:
[0100] The pickled steel plate is cold rolled to obtain a steel plate with a final thickness of 0.6 mm; wherein the reduction rate each time is 25%-30%;
[0101] Step 5, cutting:
[0102] The splitting machine includes a steel coil 1 for winding steel plates, a fixed shaft 2 and a rotating shaft 3 located on the right side of the steel coil and arranged vertically and parallel to the steel coil, and a coiling shaft 4 located on the right side of the fixed shaft for winding the split steel coil; and also includes three groups of leveling shafts 5 located between the steel coil and the fixed shaft, and five longitudinally distributed splitting knives 21 are provided on the fixed shaft;
[0103] The staff winds the steel plate onto the steel reel, and uses tools to pull the right edge of the steel plate stretched from the steel reel through the upper and lower leveling shafts of each group of leveling shafts. Each group of leveling shafts flattens the curled steel plate; the steel plate passes between the fixed shaft and the rotating shaft, and the rotating shaft drives the steel plate to move to the right. The splitting knife splits the steel plate into steel coils with a width of 60 mm, and the staff winds the steel coils onto the rotating coiling shaft.
[0104] Step 6, Bending:
[0105] Passing each steel coil through a multi-stage forming roller to form the steel coil into a pipe;
[0106] Step 7, Soldering:
[0107] The butt joints of the pipes are welded by a laser welding machine to obtain round pipes. The angle between the laser beam and the welding direction is 45°, the welding speed is 5mm / s, the beam spot is 1mm, the arc starting current is 90A, and the arc ending current is 140A. The arc starting current should not be too high to prevent the pipes from being welded through.
[0108] X-rays are used to inspect the welded round tubes to detect cracks, weld bumps, pores and slag inclusions; when defects exist in the round tubes, the round tubes are judged as unqualified; and the unqualified round tubes are treated as scrap.
[0109] Step 8, pulling:
[0110] The puller includes an inner mold rod 61, an outer mold tube 62 arranged outside the inner mold rod, a high-frequency induction coil 63 arranged on the right side of the inner mold rod and the outer mold tube, and a support tube 64 arranged in the high-frequency induction coil; the aperture of the right part of the outer mold tube is larger than the aperture of the left part of the outer mold tube, and the cross-sectional size of the inner mold rod is adapted to the aperture of the outer mold tube;
[0111] The staff passes the round tube into the support tube from right to left, and makes the high-frequency induction coil work to perform high-frequency induction heating on the round tube, so that the round tube is kept at 600℃ for 30s to improve the deformation capacity and reduce the residual stress; the round tube continues to move to the left and enters the gap between the inner die and the outer die. The inner die and the outer die pull the round tube to reduce the diameter of the round tube and thin the wall thickness.
[0112] X-rays are used to detect the thickness of the round tube. When the error between the detected thickness and the theoretical thickness exceeds 5%, the thickness of the round tube is determined to be unqualified and the unqualified round tube is treated as waste.
[0113] Step 9, heat treatment:
[0114] The protective atmosphere furnace includes a heating chamber 71 and a cooling chamber 72 located on the right side of the heating chamber; a feeding port is provided at the top of the heating chamber, and a feeding port sealing cover 711 is provided on the feeding port; a discharging port is provided at the top of the cooling chamber, and a discharging port sealing cover 721 is provided on the discharging port; a temperature and pressure sensor 712 and a plurality of heating elements 713 are provided on the heating chamber; the furnace also includes a hydrogen bottle 715, an argon bottle 716 and a booster pump 714 connected to the heating chamber, the hydrogen bottle is connected to the booster pump through a first connecting pipe, the argon bottle is connected to the booster pump through a second connecting pipe, and a first solenoid valve 717 and a second solenoid valve 718 are provided on the first connecting pipe and the second connecting pipe, respectively; the furnace also includes a vacuum pump 701 and a waste gas bin 702 connected to the heating chamber, the vacuum pump is connected to the waste gas bin through a third connecting pipe, and a third solenoid valve 703 is provided on the third connecting pipe;
[0115] It also includes a water inlet pump 722 connected to the cooling chamber and a water tank 723 located below the cooling chamber. The water tank is connected to the cooling chamber through a water inlet pipe and a water outlet pipe respectively. The water inlet pump is located on the water inlet pipe. A fourth solenoid valve 724 is also provided on the water inlet pipe. A fifth solenoid valve 725 is provided on the water outlet pipe. The controller is electrically connected to the temperature and pressure sensor, each heating element, a pressure pump, a first solenoid valve, a second solenoid valve, a vacuum pump, a third solenoid valve, a water inlet pump, a fourth solenoid valve and a fifth solenoid valve respectively.
[0116] Open the feeding port, put multiple round tubes into the heating chamber, and cover the feeding port sealing cover; the controller controls the third solenoid valve to open, start the vacuum pump, evacuate the heating chamber, and pump the gas in the heating chamber into the waste gas bin, observe the pressure data detected by the temperature and pressure sensor, and when the air pressure in the heating chamber reaches 1×10 -3 MPa, the vacuum pump is controlled to stop working and the third solenoid valve is closed;
[0117] The controller controls the second solenoid valve to open, controls the booster pump to work, and fills the heating chamber with argon gas. When the gas pressure in the heating chamber reaches 0.1 MPa, the controller controls the second solenoid valve to close, and the booster pump stops working.
[0118] The controller controls the first solenoid valve to open, controls the booster pump to work, and fills hydrogen into the heating chamber. When the gas pressure in the heating chamber reaches 0.3 MPa, the controller controls the first solenoid valve to close, and the booster pump stops working.
[0119] like Figure 5 As shown, each heating element is controlled to heat the heating chamber, the first stage annealing temperature is 980°C, and the temperature is kept for 10 minutes; the second stage annealing temperature is 1100°C, and the temperature is kept for 5 minutes; each heating element is controlled to stop working;
[0120] The staff opens the sealing cover of the feeding port and the sealing cover of the discharging port, uses tools to take out each round tube from the heating chamber, puts each round tube into the cooling chamber, and closes the sealing cover of the feeding port and the sealing cover of the discharging port;
[0121] The fourth solenoid valve is controlled to open by the controller, and the water pump starts to work to pump the cooling water in the water tank into the cooling chamber, and the fourth solenoid valve and the water pump are closed;
[0122] After the round tubes have been water-cooled in the cooling chamber for two minutes, the fifth solenoid valve is controlled to open, and the cooling water in the cooling chamber automatically flows back to the water tank. The discharge port is opened, and the staff takes out the round tubes in the cooling chamber.
[0123] Example 2
[0124] In Example 2, the mass percentages of the components in the ultra-soft stainless steel tube are as follows: C: 0.02%, N: 0.2%, Si: 0.1%, Mn: 1.5%, Cr: 17.4%, Ni: 13.8%, Mo: 2.9%, Cu: 1.3%, Ti: 0.015%, Nb: 0.25%, V: 0.3%, and the balance is iron; the other structures and method parts of Example 2 are the same as those of Example 1.
[0125] Example 3
[0126] In Example 3, the mass percentages of the components in the ultra-soft stainless steel tube are as follows: C: 0.01%, N: 0.1%, Si: 0.08%, Mn: 4.6%, Cr: 17.6%, Ni: 11.3%, Cu: 2.4%, Ti: 0.006%, Nb: 0.02%, V: 0.2%, Mo: 2.1%, and the balance is iron; the other structures and methods of Example 3 are the same as those of Example 1.
[0127] Example 4
[0128] In Example 4, the mass percentages of the components in the ultra-soft stainless steel tube are as follows: C: 0.01%, N: 0.08%, Si: 0.08%, Mn: 5.2%, Cr: 16.3%, Ni: 12.7%, Cu: 2.1%, Ti: 0.01%, Nb: 0.2%, Mo: 0.9%, V: 0.1%, and the balance is iron; the other structures and method parts of Example 4 are the same as those of Example 1.
[0129] The ultra-soft stainless steel tubes prepared in Examples 1 to 4 were tested for mechanical properties and pressure resistance, and the results were as follows: Figure 6 And the following Table 1:
[0130] Table 1
[0131]
[0132] It can be seen from Table 1 that the tensile strength of the obtained ultra-soft stainless steel pipes is all lower than 480 MPa, the yield strength is lower than 170 MPa, and the Vickers hardness is lower than 140 MPa. Compared with ordinary austenitic stainless steel, the strength and hardness of the present invention are lower, and the strain-induced martensite content generated during the deformation process is less.
[0133] Depend on Figure 6 It can be seen that as the wall thickness of the ultra-soft stainless steel pipe increases, the pressure it withstands is also gradually increasing. When the wall thickness reaches 0.7mm, the pressure it withstands can reach 50MPa.
[0134] Therefore, the ultra-soft stainless steel pipe of the present invention can adjust the weld structure, control the grain size, and improve the performance of the ultra-soft stainless steel pipe by adopting graded annealing.
[0135] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an ultra-soft stainless steel tube, Its characteristics are: The steps include: Step 1, smelting: The components used to make the ultra-soft stainless steel tube are weighed according to mass percentage and melted by "vacuum induction melting + vacuum consumable remelting"; Step 2, continuous casting and rolling: The molten steel is poured into a continuous casting machine to form a slab, and then hot-rolled in a soaking furnace for multiple passes to obtain a steel plate; Step 3, pickling: The steel plate is placed in a pickling solution for pickling; Step 4, cold rolling: Cold rolling the pickled steel plate to obtain a steel plate; Step 5, cutting: Using a splitter to split a steel plate (01) into steel coils (02); Step 6, Bending: Passing each steel coil through a multi-stage forming roller to form the steel coil into a pipe; Step 7, Soldering: The butt joints of the pipes are welded by a laser welding machine to obtain round pipes; Step 8, pulling: The round tube is subjected to high-frequency induction heating by a puller, and pressure is applied to the round tube for pulling, so that the diameter of the round tube is reduced and the thickness of the tube wall is thinned; Step 9, heat treatment: Put a number of round tubes into a hydrogen + argon protective atmosphere furnace for annealing, the first stage annealing temperature is 960 ℃ -1000 ℃, keep warm for 8min-12min; the second stage annealing temperature is 1080 ℃ -1120 ℃, keep warm for 3min-5min, then, each round tube is water-cooled; the super soft stainless steel tube is composed of carbon C, nitrogen N, silicon Si, manganese Mn, chromium Cr, nickel Ni, molybdenum M o, copper Cu, titanium Ti, niobium Nb, vanadium V and iron Fe; the mass percentages of the components in the ultra-soft stainless steel tube are as follows: C: 0.005%-0.02%, N: 0.05%-0.2%, Si: 0.01%-0.1%, Mn: 1%-7%, Cr: 16%-20%, Ni: 8%-14%, Mo: 0.5%-3.0%, Cu: 1%-6%, Ti: 0.005%-0.015%, Nb: 0.01%-0.25%, V: 0.03%-0.3%, and the balance is iron; <h2 style=";text-align:left;direction:ltr">Ni<h2 style=";text-align:left;direction:ltr"> eq <h2 style=";text-align:left;direction:ltr"> =Ni+12.93C+1.11Mn+0.72Cr-0.27Si+0.53Cu+ 7.55N-0.24Ti+0.19Nb+0.9V+0.88Mo; Among them, Ni eq is the Ni equivalent in the supersoft stainless steel tube; The stacking fault formability index SFI in ultra-soft stainless steel tubes is ≥30; SFI=2.2Ni+6Cu-1.1Cr-13Si-1.2Mn+32; The protective atmosphere furnace comprises a heating chamber (71) and a cooling chamber (72) located on the right side of the heating chamber; a feeding port is provided at the top of the heating chamber, a feeding port sealing cover (711) is provided on the feeding port, and a discharge port sealing cover (721) is provided on the top of the cooling chamber; a temperature and pressure sensor (712) and a plurality of heating elements (713) are provided on the heating chamber; the furnace also comprises a hydrogen bottle (715), an argon bottle (716) and a pressure pump (714) connected to the heating chamber, the hydrogen bottle is connected to the pressure pump through a first connecting pipe, the argon bottle is connected to the pressure pump through a second connecting pipe, and a first solenoid valve (717) and a second solenoid valve (718) are provided on the first connecting pipe and the second connecting pipe respectively; the furnace also comprises a vacuum pump (701) and a waste gas bin (702) connected to the heating chamber, the vacuum pump is connected to the waste gas bin through a third connecting pipe, and a third solenoid valve (703) is provided on the third connecting pipe; It also includes a water inlet pump (722) connected to the cooling chamber and a water tank (723) located below the cooling chamber, the water tank being connected to the cooling chamber via a water inlet pipe and a water outlet pipe respectively, the water inlet pump being located on the water inlet pipe, a fourth solenoid valve (724) being further provided on the water inlet pipe, and a fifth solenoid valve (725) being provided on the water outlet pipe; the controller being electrically connected to the temperature and pressure sensor, each heating element, the booster pump, the first solenoid valve, the second solenoid valve, the vacuum pump, the third solenoid valve, the water inlet pump, the fourth solenoid valve and the fifth solenoid valve respectively; Step 9 is specifically as follows: Open the feeding port, put several round tubes into the heating chamber, and cover the feeding port sealing cover; the controller controls the third solenoid valve to open, start the vacuum pump, evacuate the heating chamber, and pump the gas in the heating chamber into the waste gas bin, observe the pressure data detected by the temperature and pressure sensor, and when the air pressure in the heating chamber reaches 1×10 -3 MPa, the vacuum pump is controlled to stop working and the third solenoid valve is closed; The controller controls the second solenoid valve to open, controls the booster pump to work, and fills the heating chamber with argon gas. When the gas pressure in the heating chamber reaches 0.1 MPa, the controller controls the second solenoid valve to close, and the booster pump stops working. The controller controls the first solenoid valve to open, controls the booster pump to work, and fills hydrogen into the heating chamber. When the gas pressure in the heating chamber reaches 0.3 MPa, the controller controls the first solenoid valve to close, and the booster pump stops working. Control each heating element to heat the heating chamber, the first stage annealing temperature is 960℃-1000℃, and the heat preservation is 8min-12min; the second stage annealing temperature is 1080℃-1120℃, and the heat preservation is 3min-5min; control each heating element to stop working; The staff opens the sealing cover of the feeding port and the sealing cover of the discharging port, uses tools to take out each round tube from the heating chamber, puts each round tube into the cooling chamber, and closes the sealing cover of the feeding port and the sealing cover of the discharging port; The fourth solenoid valve is opened by the controller, and the water inlet pump starts to work to pump the cooling water in the water tank into the cooling chamber, and the fourth solenoid valve and the water inlet pump are closed; After the round tubes have been water-cooled in the cooling chamber for two minutes, the fifth solenoid valve is controlled to open, and the cooling water in the cooling chamber automatically flows back to the water tank. The sealing cover of the discharge port is opened, and the staff takes out the round tubes in the cooling chamber.
2. The method for preparing the ultra-soft stainless steel tube according to claim 1, Its characteristics are: The puller comprises an inner mold rod (61), an outer mold tube (62) arranged outside the inner mold rod, a high-frequency induction coil (63) arranged on the right side of the inner mold rod and the outer mold tube, and a support tube (64) arranged inside the high-frequency induction coil; the aperture of the right part of the outer mold tube is larger than the aperture of the left part of the outer mold tube, and the cross-sectional size of the inner mold rod is adapted to the aperture of the outer mold tube; Step 8 is specifically as follows: The staff passes the round tube into the support tube from right to left, and makes the high-frequency induction coil work to perform high-frequency induction heating on the round tube; the round tube continues to move to the left, so that the round tube enters the gap between the inner mold and the outer mold, and the inner mold and the outer mold pull the round tube to reduce the diameter of the round tube and thin the tube wall.
3. The method for preparing the ultra-soft stainless steel tube according to claim 1, Its characteristics are: The splitting machine comprises a steel coil (1) for winding steel plates, a fixed shaft (2) and a rotating shaft (3) located on the right side of the steel coil and parallel to the steel coil and arranged up and down, and a plate rolling shaft (4) located on the right side of the fixed shaft for winding the split steel coil; and also comprises a plurality of leveling shafts (5) located between the steel coil and the fixed shaft, and a plurality of longitudinally distributed splitting knives (21) are provided on the fixed shaft.
4. The method for preparing the ultra-soft stainless steel tube according to claim 1, Its characteristics are: The following steps are also included between step 7 and step 8: X-rays are used to inspect the welded round tubes to detect cracks, weld bumps, pores and slag inclusions; when defects exist in the round tubes, the round tubes are judged as unqualified; and the unqualified round tubes are treated as scrap.
5. The method for preparing the ultra-soft stainless steel tube according to claim 1, 2, 3 or 4, Its characteristics are: The following steps are also included between step 8 and step 9: X-rays are used to detect the thickness of the round tube. When the error between the detected thickness and the theoretical thickness exceeds 5%, the thickness of the round tube is determined to be unqualified and the unqualified round tube is treated as waste.