A lithium difluorophosphate production process and preparation system

By adopting the technology of gradually accelerating the start-up of centrifuges and auxiliary parts in the preparation of lithium difluorophosphate, the problems of low purity and excessive stress on the centrifuge caused by the irregular movement of lithium fluoride in the traditional centrifugal process are solved, and high The purity and low cost of lithium difluorophosphate preparation extend centrifuge life.

CN118164467BActive Publication Date: 2024-10-18JIANGSU CHUANGKE NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410565919.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-10-18
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

During the preparation process of lithium difluorophosphate, the traditional centrifugal process causes lithium fluoride to move irregularly in the centrifuge, resulting in smaller particle size, impurities entering the solution, reducing purity, and excessive force on the centrifuge, affecting its service life.

Method used

Start the centrifuge with gradual acceleration and set the auxiliary parts so that the lithium difluorophosphate mixture spreads evenly along the inner wall of the centrifuge. The lithium fluoride and lithium difluorophosphate solutions are separated through the centrifugation process of repeated speed reduction and speed increase, and the lithium difluorophosphate solution is carbonized. tower and stirred crystallization tank for further purification.

Benefits of technology

It improves the purity of lithium difluorophosphate, reduces the preparation cost, extends the service life of the centrifuge, realizes full utilization of resources, and has simple process, convenient operation, low energy consumption, low product acidity, high purity and high yield. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118164467B_ABST
    Figure CN118164467B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation technology, and specifically relates to a lithium difluorophosphate production process and a preparation system thereof. The lithium difluorophosphate production process comprises: carbonizing lithium carbonate to prepare high-purity lithium carbonate; preparing a first mixed solution by using ethylene glycol dimethyl ether and lithium hexafluorophosphate, adding ultrapure water and heating to a reaction temperature; preparing a lithium difluorophosphate mixture by using the high-purity lithium carbonate and the first mixed solution; and concentrating to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether to extract lithium difluorophosphate crystals. The invention can improve the purity of the lithium difluorophosphate solution extracted from the lithium difluorophosphate mixture, realize full utilization of resources, reduce the preparation cost of lithium difluorophosphate, realize improved service life of a centrifuge, and has the advantages of simple process, convenient operation, short reaction time and low energy consumption, can avoid the defects of moisture absorption, agglomeration and pollution caused by powder, and can make the final product low in acidity, high in purity and high in yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation technology, and specifically relates to a lithium difluorophosphate production process and a preparation system thereof. Background Art

[0002] The electrolyte is a part of the lithium-ion battery, which transports ions between the positive and negative electrodes to conduct current. The performance of the electrolyte affects the performance of the lithium-ion battery. Lithium difluorophosphate is used to prepare the electrolyte. In terms of electrolyte modification, lithium difluorophosphate plays a role in increasing the discharge rate of the battery and reducing the internal resistance of the battery.

[0003] However, in the process of preparing lithium difluorophosphate, lithium fluoride and lithium difluorophosphate solution need to be separated from the lithium difluorophosphate mixture, and the centrifuge is directly started at full speed in the traditional centrifugal process, such as Figure 1 As shown, the lithium fluoride in the lithium difluorophosphate mixture is inconsistent in weight, shape, force direction, etc., and the centrifugal force is very large when the centrifuge is started at full speed, which causes the lithium fluoride in the lithium difluorophosphate mixture to move irregularly in the centrifuge, causing collisions between lithium fluorides, and the particle size of lithium fluoride becomes smaller and flows out of the centrifuge with the lithium difluorophosphate solution, that is, the lithium difluorophosphate solution contains impurities, and the purity of the lithium difluorophosphate finally prepared becomes low, which in turn affects the performance of the electrolyte and the performance of the lithium-ion battery, and the large particle size of lithium fluoride will also block the sieve hole of the centrifuge, affecting the outflow of the lithium difluorophosphate solution, there is a waste of resources, and the preparation cost of lithium difluorophosphate is increased. In addition, the centrifuge needs instantaneous high torque to start at full speed directly, which causes the centrifuge to heat up and the stress it is subjected to is also very large, affecting the service life of the centrifuge.

[0004] Therefore, it is urgent to develop a new lithium difluorophosphate production process and preparation system to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide a lithium difluorophosphate production process and a preparation system thereof.

[0006] In order to solve the above technical problems, the present invention provides a lithium difluorophosphate production process, which comprises: carbonizing lithium carbonate to prepare high-purity lithium carbonate; preparing a first mixed solution by using ethylene glycol dimethyl ether and lithium hexafluorophosphate, adding ultrapure water to the first mixed solution and heating it to a reaction temperature; preparing a lithium difluorophosphate mixture by reacting the high-purity lithium carbonate with the first mixed solution; arranging an auxiliary part in a centrifuge, putting the lithium difluorophosphate mixture into the centrifuge, gradually accelerating and starting the centrifuge so that the lithium difluorophosphate mixture is spread on the inner wall of the centrifuge under the guidance of the auxiliary part and under the centrifugal action, separating lithium fluoride and lithium difluorophosphate solution in the lithium difluorophosphate mixture by speeding up the centrifuge, and circulating the process of first slowing down, then speeding up, and then slowing down the centrifuge at least twice; concentrating the lithium difluorophosphate solution to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether to extract lithium difluorophosphate crystals.

[0007] Specifically, the drum of the centrifuge is arranged horizontally, and the auxiliary component is arranged horizontally in the drum and is located above the bottom of the drum.

[0008] Specifically, the centrifuge is started with gradual acceleration, so that the lithium difluorophosphate mixture is spread circumferentially on the inner wall of the drum under the guidance of the auxiliary parts and under the centrifugal action; after the centrifuge separates the lithium fluoride and the lithium difluorophosphate solution in the lithium difluorophosphate mixture for the first time, the centrifuge is decelerated to make the lithium difluorophosphate mixture spread circumferentially on the inner wall of the drum fall toward the bottom of the drum, so that the auxiliary parts remix the lithium difluorophosphate mixture, and then the centrifuge is accelerated to redistribute the lithium difluorophosphate mixture to be spread circumferentially on the inner wall of the drum until the lithium difluorophosphate solution flows out of the drum.

[0009] Specifically, high-purity lithium carbonate is prepared by placing lithium carbonate in a carbonization tower and adding carbon dioxide for carbonization treatment.

[0010] Specifically, the amount of ultrapure water added is 0.01% to 0.5% of the total mass of the high-purity lithium carbonate and the first mixed solution.

[0011] Specifically, a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is placed in a stirred crystallization tank for stirred crystallization, and the temperature drop gradient during crystallization is controlled.

[0012] Specifically, the time from 10°C to 0°C in the temperature reduction gradient is 5 h, and the stirring speed is 20 rpm to 40 rpm; the time from 0°C to -30°C in the temperature reduction gradient is 15 h, and the stirring speed is 60 rpm to 80 rpm.

[0013] Specifically, a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is stirred and crystallized to form crystals, and the crystals are taken out by natural sedimentation, and the crystals are dried by a screw belt dryer to extract lithium difluorophosphate crystals.

[0014] Specifically, the high-purity lithium carbonate is screened so that the particle size of the high-purity lithium carbonate is no greater than 1000 mesh.

[0015] Specifically, lithium hexafluorophosphate is dissolved in ethylene glycol dimethyl ether solution, and the concentration of lithium hexafluorophosphate in the first mixed solution is 0.2 to 1.5 mol / L, the dissolution temperature is 0 to 30° C., and the addition time of lithium hexafluorophosphate is 1 to 2 hours.

[0016] Specifically, the lithium difluorophosphate crystals are screened so that the particle size of the lithium difluorophosphate crystals is 10-325 mesh.

[0017] On the other hand, the present invention provides a preparation system using the above-mentioned lithium difluorophosphate production process, which comprises: a carbonization tower, a centrifuge, a stirring crystallization tank and a spiral belt dryer; lithium carbonate is placed in the carbonization tower and carbon dioxide is added for carbonization treatment to prepare high-purity lithium carbonate; a first mixed solution is prepared by using ethylene glycol dimethyl ether and lithium hexafluorophosphate, ultrapure water is added to the first mixed solution and the solution is heated to a reaction temperature; a lithium difluorophosphate mixture is prepared by reacting high-purity lithium carbonate with the first mixed solution; the lithium difluorophosphate solution is extracted by a centrifuge; the lithium difluorophosphate solution is concentrated to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether, and the saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is placed in a stirring crystallization tank for stirring crystallization, and lithium difluorophosphate crystals are extracted by a spiral belt dryer.

[0018] The invention has the beneficial effects that, by gradually accelerating the centrifuge during the centrifugation process and cooperating with auxiliary parts, the lithium difluorophosphate mixture accumulated at the bottom of the centrifuge can be evenly spread along the inner wall, and the lithium fluoride in the lithium difluorophosphate mixture can be prevented from colliding at the moment of starting the centrifuge, thereby improving the purity of the lithium difluorophosphate solution extracted from the lithium difluorophosphate mixture, thereby improving the purity of the lithium difluorophosphate, and improving the performance of the electrolyte and the performance of the lithium ion battery. At the same time, by repeatedly mixing the lithium difluorophosphate mixture and re-separating the lithium fluoride and the lithium difluorophosphate solution, the lithium difluorophosphate solution in the lithium difluorophosphate mixture can be extracted to the maximum extent, and the resources can be fully utilized, and the preparation cost of lithium difluorophosphate can be reduced. At the same time, the centrifuge is driven to work by gradually accelerating and decelerating to meet the optimal working conditions of the centrifuge, and the service life of the centrifuge is improved. The invention has the advantages of simple process, convenient operation, short reaction time, and low energy consumption, and can avoid the defects of moisture absorption, agglomeration, and pollution caused by the powder, and can make the final product low in acidity, high in purity, and high in yield.

[0019] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practicing the present invention.

[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 It is a schematic diagram of a centrifugal process in the prior art;

[0023] Figure 2 It is a flow chart of the lithium difluorophosphate production process of the present invention;

[0024] Figure 3 It is a schematic diagram of placing a lithium difluorophosphate mixture into a centrifuge in the lithium difluorophosphate production process of the present invention;

[0025] Figure 4 It is a schematic diagram of the centrifuge in the lithium difluorophosphate production process of the present invention when it is working.

[0026] In the figure:

[0027] 1. Roller; 2. Lithium difluorophosphate mixture; 3. Lithium fluoride; 4. Auxiliary parts. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Embodiment 1, in this embodiment, as Figures 2 to 4As shown, this embodiment provides a lithium difluorophosphate production process, which includes: carbonizing lithium carbonate to prepare high-purity lithium carbonate; preparing a first mixed solution by ethylene glycol dimethyl ether and lithium hexafluorophosphate, adding ultrapure water to the first mixed solution and heating it to a reaction temperature; preparing a lithium difluorophosphate mixture 2 by reacting the high-purity lithium carbonate with the first mixed solution; arranging an auxiliary part 4 in a centrifuge, placing the lithium difluorophosphate mixture 2 into the centrifuge, gradually accelerating the centrifuge to spread the lithium difluorophosphate mixture 2 on the inner wall of the centrifuge under the guidance of the auxiliary part 4 and under the centrifugal action, separating the lithium fluoride 3 in the lithium difluorophosphate mixture 2 from the lithium difluorophosphate solution by speeding up the centrifuge, and circulating the centrifuge to first slow down, then speed up, and then slow down at least twice; concentrating the lithium difluorophosphate solution to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether to extract lithium difluorophosphate crystals.

[0030] Specifically, the reaction temperature is 40-80°C.

[0031] In this embodiment, the lithium difluorophosphate mixture 2 accumulated at the bottom of the centrifuge can be evenly spread along the inner wall by gradually accelerating the centrifuge and cooperating with the auxiliary part 4 during the centrifugation process, thereby avoiding the collision of lithium fluoride 3 in the lithium difluorophosphate mixture 2 at the moment of starting the centrifuge, thereby improving the purity of the lithium difluorophosphate solution extracted from the lithium difluorophosphate mixture 2, thereby improving the purity of lithium difluorophosphate, and improving the performance of the electrolyte and the performance of the lithium ion battery. At the same time, by repeatedly mixing the lithium difluorophosphate mixture 2 and re-separating the lithium fluoride 3 and the lithium difluorophosphate solution, the lithium difluorophosphate solution in the lithium difluorophosphate mixture 2 can be extracted to the maximum extent, resources can be fully utilized, and the preparation cost of lithium difluorophosphate can be reduced. At the same time, gradually accelerating and decelerating the centrifuge to work meets the optimal working conditions of the centrifuge, thereby improving the service life of the centrifuge, and has the advantages of simple process, convenient operation, short reaction time, and low energy consumption. It can avoid the defects of moisture absorption, agglomeration, and pollution caused by the powder, and can make the final product low in acidity, high in purity, and high in yield.

[0032] Specifically, the existing preparation methods of lithium difluorophosphate have the problems of long reaction time, low reaction yield, low product purity, etc. The product obtained by the current preparation methods of lithium difluorophosphate is basically lithium difluorophosphate powder, but the powder is easy to absorb moisture, agglomerate and generate dust pollution, and it is easy to have difficulty in feeding and generate a lot of heat in the downstream electrolyte preparation process, and it is more likely to cause decomposition, and its application scope is severely limited. Most of the existing technologies use ester solvents such as dimethyl carbonate, diethyl carbonate, ethyl acetate, etc. as solvents to prepare lithium difluorophosphate, but lithium difluorophosphate is insoluble in the above ester solvents, so it is necessary to use ethylene glycol dimethyl ether for dissolution and separation in the later stage. At the same time, the ester solvent contacts the raw material lithium hexafluorophosphate during the reaction, and the phosphorus pentafluoride decomposed will turn into light yellow or even brown, thereby affecting the product color and subsequent application of the product. In this embodiment, each material is purified to reduce the content of impurities in the ether solvent, and when lithium hexafluorophosphate is added, the temperature is controlled at 0-30°C and the concentration is controlled at 0.2-1.5 mol / L, which can prevent the lithium hexafluorophosphate from being decomposed due to excessively high temperature when it meets the ether solvent, and excessively high or low concentration will reduce the final yield. Ultrapure water is used as a catalyst, which is not only easy to obtain, but also promotes rapid reaction and reduces the reaction time to 1-2 hours. It does not need to introduce other impurities and does not produce pollutants. At the same time, it reduces the reaction temperature and improves production efficiency. In addition, adding too much water will react with lithium hexafluorophosphate to result in low product yield and high acidity. If the amount of water added is too little, it will not have a catalytic effect and the reaction time will be long. The invention controls the amount of ultrapure water added to be 0.01% to 0.5% of the total mass of the reactants, so that the final product has low acidity, high purity and high yield. The weight ratio of high-purity lithium carbonate to lithium hexafluorophosphate is limited to (0.98 to 1.07):1, so as to avoid incomplete reaction and improve the purity of lithium difluorophosphate. Ethylene glycol dimethyl ether is used as a solvent, which has a low boiling point, is easy to volatilize and is easy to dry. It can not only dissolve the raw material lithium hexafluorophosphate, but also dissolve the product lithium difluorophosphate. There is no need to add solvent for centrifugation and concentration after the reaction is completed, so as to avoid secondary separation and simplify the process. The temperature-drop gradient crystallization method can be used to obtain regular lithium difluorophosphate elliptical crystals, which have less insoluble matter and high product quality. At the same time, the specific surface area is small, the application of the crystals in the electrolyte is stable, the dissolution heat is reduced, and the crystals are not easy to decompose, which greatly broadens the scope of application.

[0033] In this embodiment, the drum 1 of the centrifuge is horizontally arranged, and the auxiliary component 4 is horizontally arranged in the drum 1 and located above the bottom of the drum 1 .

[0034] Specifically, the auxiliary member 4 is arranged in a columnar shape and is fixed to the housing of the centrifuge, so that the drum 1 rotates while the auxiliary member 4 does not rotate, and the drum 1 rotates relative to the auxiliary member 4, so that the auxiliary member 4 plays a guiding and mixing role.

[0035] In this embodiment, the centrifuge is started with gradual acceleration, so that the lithium difluorophosphate mixture 2 is spread circumferentially on the inner wall of the drum 1 under the guidance of the auxiliary member 4 and the centrifugal action; after the centrifuge separates the lithium fluoride 3 and the lithium difluorophosphate solution in the lithium difluorophosphate mixture 2 for the first time, the centrifuge is decelerated to make the lithium difluorophosphate mixture 2 spread circumferentially on the inner wall of the drum 1 fall toward the bottom of the drum 1, so that the auxiliary member 4 remixes the lithium difluorophosphate mixture 2, and then the centrifuge is accelerated to redistribute the lithium difluorophosphate mixture 2 to be spread circumferentially on the inner wall of the drum 1, until the lithium difluorophosphate solution flows out of the drum 1.

[0036] Specifically, all the lithium difluorophosphate mixture 2 is placed in the drum 1, so that the lithium difluorophosphate mixture 2 is piled at the bottom of the drum 1, and the centrifuge is driven to accelerate slowly and stably rotate at a low speed. At this time, the lithium difluorophosphate mixture 2 can stick to the inner wall of the drum 1 under the action of centrifugal force, and gradually cover the inner wall of the drum 1 circumferentially. At this time, the centrifuge is driven to gradually speed up to separate the lithium fluoride 3 and the lithium difluorophosphate solution in the lithium difluorophosphate mixture 2, that is, the lithium difluorophosphate solution flows out of the drum 1, and the centrifuge can be accelerated to the highest speed. When the lithium difluorophosphate solution no longer flows out of the drum 1, it means that the lithium fluoride 3 has blocked the sieve holes of the drum 1 at this time. Then the centrifuge is driven to gradually decelerate, so that the lithium difluorophosphate mixture 2 attached to the inner wall of the drum 1 falls toward the bottom of the drum 1, and the lithium difluorophosphate mixture 2 is diverted by the auxiliary component 4 during the falling process. The auxiliary component 4 plays the role of remixing the lithium difluorophosphate mixture 2. At this time, the centrifuge is driven to gradually accelerate, and the lithium difluorophosphate mixture 2 located at the bottom of the drum 1 climbs up the inner wall of the drum 1 again. In the process of the lithium difluorophosphate mixture 2 climbing up the inner wall of the drum 1, the auxiliary component 4 can stir the lithium difluorophosphate mixture 2 to achieve redistribution of the lithium difluorophosphate mixture 2 and spread it circumferentially on the inner wall of the drum 1. When the centrifuge is accelerated to a certain speed, the lithium fluoride 3 and the lithium difluorophosphate solution in the lithium difluorophosphate mixture 2 are separated again. The residual lithium difluorophosphate solution in the lithium difluorophosphate mixture 2 can be drained from the drum 1 to purify the lithium difluorophosphate mixture 2. The process of decelerating and speeding up the centrifuge is repeated again to ensure that all the lithium difluorophosphate solution in the lithium difluorophosphate mixture 2 flows out of the drum 1, so as to achieve full utilization of resources.

[0037] In this embodiment, high-purity lithium carbonate is prepared by placing lithium carbonate in a carbonization tower and adding carbon dioxide for carbonization treatment.

[0038] Specifically, industrial-grade lithium carbonate is placed in a carbonization tower, carbon dioxide is added thereto for carbonization treatment, impurities insoluble in carbon dioxide are removed, and then dried and crushed to produce high-purity lithium carbonate.

[0039] Specifically, lithium hexafluorophosphate is slowly added to the purified ethylene glycol dimethyl ether to dissolve the lithium hexafluorophosphate, thereby obtaining an ethylene glycol dimethyl ether solution of lithium hexafluorophosphate.

[0040] In this embodiment, the amount of ultrapure water added is 0.01% to 0.5% of the total mass of the high-purity lithium carbonate and the first mixed solution.

[0041] Specifically, the ultrapure water is added dropwise.

[0042] In this embodiment, a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is placed in a stirring crystallization tank for stirring crystallization, and the temperature drop gradient during crystallization is controlled.

[0043] In this embodiment, the time from 10°C to 0°C in the cooling gradient is 5 h, and the stirring speed is 20 rpm to 40 rpm; the time from 0°C to -30°C in the cooling gradient is 15 h, and the stirring speed is 60 rpm to 80 rpm.

[0044] In this embodiment, a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is stirred and crystallized to form crystals, and the crystals are taken out by natural sedimentation, and the crystals are dried by a screw belt dryer to extract lithium difluorophosphate crystals.

[0045] In this embodiment, the high-purity lithium carbonate is screened so that the particle size of the high-purity lithium carbonate is no greater than 1000 mesh.

[0046] In this embodiment, lithium hexafluorophosphate is dissolved in ethylene glycol dimethyl ether solution, and the concentration of lithium hexafluorophosphate in the first mixed solution is 0.2 to 1.5 mol / L, the dissolution temperature is 0 to 30° C., and the addition time of lithium hexafluorophosphate is 1 to 2 hours.

[0047] In this embodiment, the lithium difluorophosphate crystals are screened so that the particle size of the lithium difluorophosphate crystals is 10-325 mesh.

[0048] Test case 1, industrial-grade lithium carbonate is placed in a carbonization tower, carbon dioxide is added thereto for carbonization treatment, impurities insoluble in carbon dioxide are removed, and then dried and crushed to obtain high-purity lithium carbonate with a particle size of less than 1000 mesh; 152g of lithium hexafluorophosphate is slowly added to 1000mL of purified ethylene glycol dimethyl ether, with a concentration of 1mol / L and a temperature of 0°C, and the addition is completed within 1 hour; 0.3g of ultrapure water is added to the obtained completely dissolved solution, and after the ultrapure water is added, the temperature is raised to 60°C; 148g of high-purity lithium carbonate is added to the obtained solution, and the reaction is carried out for 1 hour to obtain crude lithium difluorophosphate; the obtained crude lithium difluorophosphate is centrifuged by a centrifuge to separate the insoluble lithium fluoride 3 and the lithium difluorophosphate solution; the separated difluorophosphate The lithium acid solution is concentrated to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether, and then enters a stirred crystallization tank for crystallization while stirring, and the cooling gradient during crystallization is controlled. The time from 10°C to 0°C is 5h, and the stirring speed is controlled to 30rpm. The time from 0°C to -30°C is 15h, and the stirring speed is controlled to 70rpm. The stirred crystallization forms regular elliptical crystals, and the mother liquor obtained in the crystallization process can be recycled. After the crystallization is completed, the crystals are released by natural sedimentation and directly transferred to a spiral belt dryer for drying to obtain regular lithium difluorophosphate crystals. The lithium difluorophosphate obtained in this test case 1 is white in color, has a purity of 99.9%, a yield of 99%, a moisture content of 80ppm, an acidity of 50ppm, and a particle size of 18-100 meshes.

[0049] Test case 2, industrial-grade lithium carbonate is placed in a carbonization tower, carbon dioxide is added thereto for carbonization treatment, impurities insoluble in carbon dioxide are removed, and then dried and crushed to obtain high-purity lithium carbonate with a particle size of less than 1000 mesh; 30.4g of lithium hexafluorophosphate is slowly added to 1000mL of ethylene glycol dimethyl ether after purification, the concentration is controlled to be 0.2mol / L, the temperature is 15°C, and the addition is completed within 1.5h; 0.006g of ultrapure water is added to the obtained completely dissolved solution, and after the ultrapure water is added, the temperature is raised to 80°C; 30.4g of high-purity lithium carbonate is added to the obtained solution according to proportion, and the reaction is carried out for 1.5h to obtain crude lithium difluorophosphate; the obtained crude lithium difluorophosphate is centrifuged by a centrifuge to separate the insoluble lithium fluoride 3 and the lithium difluorophosphate solution; The obtained lithium difluorophosphate solution after centrifugation is concentrated to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether, and then enters a stirred crystallization tank for crystallization while stirring, and the cooling gradient during crystallization is controlled. The time from 10°C to 0°C is 5h, and the stirring speed is controlled to be 20rpm. The time from 0°C to -30°C is 15h, and the stirring speed is controlled to be 60rpm. The stirred crystallization forms regular elliptical crystals, and the mother liquor obtained during the crystallization process can be recycled. After the crystallization is completed, the crystals are released by natural sedimentation and directly transferred to a spiral belt dryer for drying to obtain regular lithium difluorophosphate crystals. The lithium difluorophosphate obtained in this test case 2 is white in color, has a purity of 99.9%, a yield of 99%, a moisture content of 50ppm, an acidity of 45ppm, and a particle size of 18-100 mesh.

[0050] Test case 3, industrial-grade lithium carbonate is placed in a carbonization tower, carbon dioxide is added thereto for carbonization treatment, impurities insoluble in carbon dioxide are removed, and then dried and crushed to obtain high-purity lithium carbonate with a particle size of less than 1000 mesh; 228g of lithium hexafluorophosphate is slowly added to 1000mL of ethylene glycol dimethyl ether after purification, the concentration is controlled to be 1.5mol / L, the temperature is 30°C, and the addition is completed within 2h; 2.15g of ultrapure water is added to the obtained completely dissolved solution, and after the ultrapure water is added, the temperature is raised to 40°C; 222g of high-purity lithium carbonate is added to the obtained solution according to proportion, and the reaction is carried out for 2h to obtain crude lithium difluorophosphate; the obtained crude lithium difluorophosphate is centrifuged The insoluble lithium fluoride 3 and lithium difluorophosphate solution are separated by centrifugation; the obtained lithium difluorophosphate solution is concentrated to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether, and then enters a stirred crystallization tank for crystallization while stirring, and the temperature gradient during crystallization is controlled, 10℃~0℃ time is 5h, the stirring speed is controlled to 40rpm, 0℃~-30℃ time is 15h, the stirring speed is controlled to 80rpm, and the stirred crystallization forms regular elliptical crystals. The mother liquor obtained during the crystallization process can be recycled; after the crystallization is completed, the crystals are released by natural sedimentation and directly transferred to a spiral belt dryer for drying to obtain regular lithium difluorophosphate crystals. The lithium difluorophosphate obtained in this test case 3 is white in color, with a purity of 99.9%, a yield of 98.5%, a moisture content of 100ppm, an acidity of 41ppm, and a particle size of 18~100 mesh.

[0051] Comparative Example 1 is different from Experimental Case 1 in that ethylene glycol dimethyl ether is replaced with tetrahydrofuran. The obtained lithium difluorophosphate is light yellow in color, has a purity of 98.5%, a yield of 90%, a moisture content of 85 ppm, an acidity of 60 ppm, and a particle size of 18-100 mesh.

[0052] Comparative Example 2 is different from Experimental Case 1 in that ethylene glycol dimethyl ether is replaced with dimethyl carbonate. The obtained lithium difluorophosphate is light yellow in color, has a purity of 98.7%, a yield of 87%, a moisture content of 90 ppm, an acidity of 65 ppm, and a particle size of 18-100 mesh.

[0053] Comparative Example 3 is different from Experimental Example 1 in that ultrapure water is not added. The obtained lithium difluorophosphate is white in color, has a purity of 99%, a yield of 40%, a moisture content of 60 ppm, an acidity of 50 ppm, and a particle size of 18-100 mesh.

[0054] Comparative Example 4 is different from Experimental Case 1 in that the amount of ultrapure water added is changed to 0.005%. The obtained lithium difluorophosphate is white in color, has a purity of 99%, a yield of 50%, a moisture content of 60 ppm, an acidity of 45 ppm, and a particle size of 18-100 mesh.

[0055] Comparative Example 5 is different from Experimental Case 1 in that the amount of ultrapure water added is changed to 1.0%. The obtained lithium difluorophosphate is white in color, has a purity of 95%, a yield of 70%, a moisture content of 500 ppm, an acidity of 350 ppm, and a particle size of 18-100 mesh.

[0056] It can be seen from the performance parameters of the lithium difluorophosphate obtained in each embodiment and each comparative example that an ester solvent is added as a solvent during the preparation process, and the solvent will participate in the reaction, causing the color of the lithium difluorophosphate to turn yellow. However, when ethylene glycol dimethyl ether is added as a solvent, there is no need to add a solvent for centrifugation, concentration, etc. after the reaction is completed, thereby avoiding secondary separation, which is beneficial to improving the purity and yield of the product. Insufficient addition of pure water or no addition of water during the preparation process will result in a low yield of lithium difluorophosphate, and excessive pure water will result in a low yield and purity of lithium difluorophosphate (lithium hexafluorophosphate decomposes too quickly), and high acidity and moisture.

[0057] Example 2. On the basis of Example 1, this example provides a preparation system using the lithium difluorophosphate production process provided in Example 1, which includes: a carbonization tower, a centrifuge, a stirred crystallization tank and a spiral belt dryer; high-purity lithium carbonate is prepared by placing lithium carbonate in a carbonization tower and adding carbon dioxide for carbonization treatment; a first mixed solution is prepared by using ethylene glycol dimethyl ether and lithium hexafluorophosphate, and ultrapure water is added to the first mixed solution and heated to the reaction temperature; a lithium difluorophosphate mixture 2 is prepared by reacting high-purity lithium carbonate with the first mixed solution; a lithium difluorophosphate solution is extracted by a centrifuge; the lithium difluorophosphate solution is concentrated to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether, and the saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is placed in a stirred crystallization tank for stirred crystallization, and lithium difluorophosphate crystals are extracted by a spiral belt dryer.

[0058] In summary, the present invention can make the lithium difluorophosphate mixture accumulated at the bottom of the centrifuge be evenly spread along the inner wall by gradually accelerating the centrifuge and cooperating with auxiliary parts during the centrifugation process, so as to avoid the collision of lithium fluoride in the lithium difluorophosphate mixture at the moment of starting the centrifuge, thereby improving the purity of the lithium difluorophosphate solution extracted from the lithium difluorophosphate mixture, thereby improving the purity of the lithium difluorophosphate, and improving the performance of the electrolyte and the performance of the lithium ion battery. At the same time, by repeatedly mixing the lithium difluorophosphate mixture and re-separating the lithium fluoride and the lithium difluorophosphate solution, the lithium difluorophosphate solution in the lithium difluorophosphate mixture can be extracted to the maximum extent, so as to achieve full utilization of resources and reduce the preparation cost of lithium difluorophosphate. At the same time, the centrifuge is driven to work by gradually accelerating and decelerating to meet the optimal working conditions of the centrifuge, so as to improve the service life of the centrifuge, and has the advantages of simple process, convenient operation, short reaction time and low energy consumption, and can avoid the defects of moisture absorption, agglomeration and pollution caused by the powder, so that the final product can have low acidity, high purity and high yield.

[0059] The various devices selected in this application (components whose specific structures are not described) are all universal standard parts or components known to those skilled in the art, and their structures and principles can be known to those skilled in the art through technical manuals or conventional experimental methods.

[0060] In the description of the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0061] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0062] In the several embodiments provided in the present application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. The device embodiments described above are merely schematic. For example, the division of the units is only a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some communication interfaces, and the indirect coupling or communication connection of devices or units can be electrical, mechanical or other forms.

[0063] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.

[0064] In addition, each functional unit in each embodiment of the present invention may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit.

[0065] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A process for producing lithium difluorophosphate, It is characterized in that include: Carrying out carbonization treatment on lithium carbonate to prepare high-purity lithium carbonate; Prepare a first mixed solution by using ethylene glycol dimethyl ether and lithium hexafluorophosphate, add ultrapure water into the first mixed solution and heat it to a reaction temperature; Prepare a lithium difluorophosphate mixture by reacting high-purity lithium carbonate with the first mixed solution; An auxiliary part is arranged in a centrifuge, a lithium difluorophosphate mixture is placed in the centrifuge, and the centrifuge is started with gradual acceleration, so that the lithium difluorophosphate mixture is spread on the inner wall of the centrifuge under the guidance of the auxiliary part and under the centrifugal action, lithium fluoride and lithium difluorophosphate solution in the lithium difluorophosphate mixture are separated by speeding up the centrifuge, and the centrifuge is cycled through a process of first slowing down, then speeding up, and then slowing down again at least twice; Concentrating the lithium difluorophosphate solution to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether to extract lithium difluorophosphate crystals; The amount of ultrapure water added is 0.01% to 0.5% of the total mass of the high-purity lithium carbonate and the first mixed solution; The drum of the centrifuge is arranged horizontally, and the auxiliary parts are arranged horizontally in the drum and above the bottom of the drum; The centrifuge is started at a gradually accelerated speed, so that the lithium difluorophosphate mixture is spread circumferentially on the inner wall of the drum under the guidance of the auxiliary member and the centrifugal action; After the centrifuge separates lithium fluoride and lithium difluorophosphate solution in the lithium difluorophosphate mixture for the first time, the centrifuge is decelerated to make the lithium difluorophosphate mixture spread circumferentially on the inner wall of the drum fall toward the bottom of the drum, so that the auxiliary component remixes the lithium difluorophosphate mixture, and then the centrifuge is accelerated to redistribute the lithium difluorophosphate mixture to spread circumferentially on the inner wall of the drum until the lithium difluorophosphate solution flows out of the drum; The auxiliary part is arranged in a columnar shape and is fixed to the shell of the centrifuge, so that the drum can rotate relative to the auxiliary part.

2. The lithium difluorophosphate production process according to claim 1, It is characterized in that High-purity lithium carbonate is prepared by placing lithium carbonate in a carbonization tower and adding carbon dioxide for carbonization treatment.

3. The lithium difluorophosphate production process according to claim 1, It is characterized in that A saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is placed in a stirred crystallization tank for stirred crystallization, and the temperature drop gradient during crystallization is controlled.

4. The lithium difluorophosphate production process as claimed in claim 3, It is characterized in that The time from 10°C to 0°C in the temperature reduction gradient is 5 h, and the stirring speed is 20 rpm to 40 rpm; The time from 0°C to -30°C in the temperature drop gradient was 15 h, and the stirring speed was 60 rpm to 80 rpm.

5. The lithium difluorophosphate production process as claimed in claim 3, It is characterized in that The saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is stirred and crystallized to form crystals, and the crystals are taken out by natural sedimentation, and the crystals are dried by a screw belt dryer to extract lithium difluorophosphate crystals.

6. The lithium difluorophosphate production process according to claim 1, It is characterized in that The high-purity lithium carbonate is screened so that the particle size of the high-purity lithium carbonate is no greater than 1000 mesh.

7. The lithium difluorophosphate production process according to claim 1, It is characterized in that Lithium hexafluorophosphate is dissolved in ethylene glycol dimethyl ether solution, and the concentration of lithium hexafluorophosphate in the first mixed solution is 0.2 to 1.5 mol / L, the dissolution temperature is 0 to 30° C., and the addition time of lithium hexafluorophosphate is 1 to 2 hours.

8. The lithium difluorophosphate production process according to claim 1, It is characterized in that The lithium difluorophosphate crystals are screened so that the particle size of the lithium difluorophosphate crystals is 10-325 mesh.

9. A preparation system using the lithium difluorophosphate production process according to any one of claims 1 to 8, It is characterized in that include: Carbonization tower, centrifuge, stirred crystallization tank and spiral ribbon dryer; The high-purity lithium carbonate is prepared by placing lithium carbonate in a carbonization tower and adding carbon dioxide for carbonization treatment; Prepare a first mixed solution by using ethylene glycol dimethyl ether and lithium hexafluorophosphate, add ultrapure water into the first mixed solution and heat it to a reaction temperature; Prepare a lithium difluorophosphate mixture by reacting high-purity lithium carbonate with the first mixed solution; Extract the lithium difluorophosphate solution by centrifuge; The lithium difluorophosphate solution is concentrated to a saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether, and the saturated solution of lithium difluorophosphate / ethylene glycol dimethyl ether is placed in a stirred crystallization tank for stirred crystallization, and lithium difluorophosphate crystals are extracted by a screw belt dryer.

Citation Information

Patent Citations

  • Preparation method of difluorophosphoric acid alkali metal salt

    CN105236368A

  • Preparation method of lithium difluorophosphate

    CN106829910A