A single-phase europium titanate, its preparation method, and its application in the preparation of glass-ceramic solidified bodies.
Europium titanate powder was prepared by reacting Eu2O3 and TiO2 with KCl-NaCl molten salt, and then composited with borosilicate glass. This solved the problem of high energy consumption in the synthesis of lanthanide titanate ceramics and achieved efficient and energy-saving solidification of radioactive waste.
Patent Information
- Application Number
- CN202410271325.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing methods for synthesizing lanthanide titanate ceramics require long reaction times, high temperatures and pressures, and high energy consumption. Furthermore, traditional methods are difficult to effectively immobilize radioactive lanthanide oxides.
Using Eu2O3 and TiO2 as raw materials, mixed with KCl and NaCl as molten salt, and reacted at 1000℃ for 4h in air atmosphere, a single-phase europium titanate powder was prepared. This powder was then mixed with borosilicate glass powder and sintered at 1200℃ to prepare a glass-ceramic solidified body.
High-purity europium titanate was synthesized at lower temperatures, reducing energy consumption. By fixing lanthanide elements in the crystal lattice, chemical durability and leaching resistance were improved, making it suitable for the stable storage of radioactive waste.
Smart Images

Figure CN118164525B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a single-phase europium titanate, its preparation method, and its application in the preparation of glass-ceramic solidified bodies, belonging to the technical field of molten salt method for preparing inorganic non-metallic materials. Background Technology
[0002] Nuclear energy has garnered widespread attention for addressing the global energy crisis due to its high energy density, relatively low cost, and zero greenhouse gas emissions. Currently, dry reprocessing of spent fuel based on high-temperature molten salt electrolysis technology is commonly used for treating and recovering mixed oxide spent fuels due to its advantages such as simple process, low hazard, and no high emissions of organic waste liquid. However, the waste salt produced after repeated electrolytic reduction and refining contains a large amount of radioactive lanthanide oxides that are difficult to recover. Therefore, the targeted development of solidified forms capable of effectively immobilizing radioactive lanthanide oxides is crucial for the long-term storage of highly radioactive waste in geological environments.
[0003] Borosilicate glass-ceramic composites containing lanthanide titanates (Ln₂Ti₂O₇) have proven to be potential candidates for solidifying radioactive lanthanides. In these composites, the ceramic matrix can immobilize the lanthanides within its crystal structure to achieve a high loading rate. Furthermore, the glass matrix provides an additional protective layer to enhance chemical durability. However, conventional lanthanide titanate ceramics prepared by solid-state sintering (1400 °C) using oxides as reactants typically require long reaction times, high temperatures and pressures, and high energy consumption. Therefore, it is essential to provide a simple, energy-efficient, and low-cost method for preparing lanthanide titanate ceramics. Summary of the Invention
[0004] To address the problems of long reaction times, high temperatures and pressures, and high energy consumption required in existing lanthanide titanate ceramic synthesis methods, this invention provides a single-phase europium titanate, its preparation method, and its application in the preparation of glass-ceramic solidified bodies.
[0005] The technical solution of this invention:
[0006] One of the objectives of this invention is to provide a method for preparing single-phase europium titanate. The method is as follows: using Eu2O3 and TiO2 as raw materials, mixing them with KCl and NaCl as molten salts, grinding them evenly, and then reacting the resulting mixed powder in an air atmosphere at 1000°C for 4 hours. After the reaction is completed, the mixture is naturally cooled to room temperature, and after washing and drying, single-phase europium titanate powder is obtained.
[0007] Further specifying, the molar ratio of Eu2O3 to TiO2 is 1:(2~4).
[0008] Further specified, the molar ratio of KCl to NaCl is 1:1, and the total mass ratio of molten salt to raw materials is (1-3):1.
[0009] Further specifying, the washing method is: repeatedly wash the above mixture three times with deionized water and anhydrous ethanol.
[0010] Further specified, the drying process is at a temperature of 60℃ for 6 hours.
[0011] Furthermore, Eu2O3 can be simulated as the radioactive europium oxide contained in waste salt.
[0012] The second objective of this invention is to provide europium titanate prepared by the above method, wherein the europium titanate is a single Eu2Ti2O7 phase.
[0013] The third objective of this invention is to provide a method for preparing a glass-ceramic solidified body using the above-mentioned europium titanate as a raw material. The method is as follows: europium titanate is mixed with borosilicate glass powder, ground evenly, and then sintered in air at 1200°C for 4 hours. After the reaction is completed, the mixture is naturally cooled to room temperature and mechanically crushed to obtain the solidified body.
[0014] Further specified, the europium titanate content is 10–50 wt.%.
[0015] Further specifying the preparation method of borosilicate glass powder, it is as follows: SiO2, B2O3, ZnO and CaO are mixed and ground evenly. The resulting mixed powder is then reacted in air at 1000℃ for 1 hour. After the reaction is completed, the powder is annealed and ground to obtain borosilicate glass powder.
[0016] Furthermore, SiO2, B2O3, ZnO and CaO are mixed in molar percentages of 40%, 28%, 10% and 22%, respectively.
[0017] To further specify, the annealing process is as follows: the melt is removed and allowed to cool naturally at room temperature.
[0018] Beneficial effects:
[0019] This invention uses europium oxide powder and titanium dioxide powder as reactants to prepare europium titanate using a binary KCl-NaCl molten salt medium. By screening the ratio of molten salt to reactants and controlling the reaction temperature, the synthesized europium titanate particles exhibit good crystallinity and high purity. Furthermore, the obtained europium titanate is composited with borosilicate glass to prepare a glass-ceramic cured body. The resulting europium titanate-containing borosilicate glass-ceramic cured body possesses excellent mechanical properties and stable chemical durability. Compared with existing technologies, it has the following advantages:
[0020] (1) This invention successfully synthesizes europium titanate precursor powder in an air atmosphere at a relatively low reaction temperature using a KCl-NaCl binary molten salt as the medium. This process is simple, with low synthesis temperature, low risk, good crystal morphology, and high phase purity. It transforms the traditional solid-solid reaction of europium titanate preparation using oxides as reactants via solid-state sintering into a solid-liquid reaction. The partial dissolution of reactants in the molten salt medium promotes uniform mixing and rapid diffusion of reactants at the atomic or molecular level, allowing subsequent reactions to proceed at lower temperatures. This facilitates efficient and energy-saving preparation of lanthanide titanate precursors and is of great significance for the safe treatment and disposal of high-level radioactive waste. It solves the problem of harsh reaction conditions for preparing titanate ceramics using oxides as reactants, and its engineering application will significantly reduce the energy consumption of titanate ceramic preparation.
[0021] (2) By screening the ratio of molten salt to reactants and controlling the reaction temperature, this invention reduces the reaction melting point of the reactant system by increasing the amount of TiO2, thereby promoting the forward reaction and obtaining high-purity single-phase Eu2Ti2O7 particles.
[0022] (3) In this invention, europium titanate is used to fix the lanthanide element europium in a way that the crystal lattice is completely occupied. Then, europium titanate is combined with borosilicate glass to prepare a glass-ceramic solid body containing europium titanate to further improve the leaching resistance of europium titanate ceramic, which is conducive to the fixation of lanthanide elements and realizes the stable storage of radioactive waste. Attached Figure Description
[0023] Figure 1 The XRD pattern of europium titanate ceramic powder prepared in Example 1;
[0024] Figure 2 The normalized leaching rate curve of europium titanate ceramic powder prepared in Example 1 is shown.
[0025] Figure 3 The XRD pattern of europium titanate ceramic powder prepared in Comparative Example 3 is shown.
[0026] Figure 4 The XRD pattern of europium titanate ceramic powder prepared in Comparative Example 4 is shown.
[0027] Figure 5 The XRD patterns of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6 are shown below.
[0028] Figure 6 The normalized leaching rate curves of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6 are shown.
[0029] Figure 7 Density curves of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6;
[0030] Figure 8 The Vickers hardness curves of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6 are shown.
[0031] Figure 9 This is a SEM image of the europium titanate ceramic powder prepared in Example 1. Detailed Implementation
[0032] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0033] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0034] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0035] Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, the materials, reagents, methods, and instruments used are all conventional materials, reagents, methods, and instruments in the art, and can be obtained commercially by those skilled in the art.
[0036] Example 1:
[0037] The method for preparing europium titanate ceramics in this embodiment includes the following steps:
[0038] a. Weigh out 11.30g of potassium chloride and 8.86g of sodium chloride according to the molar ratio of KCl and NaCl of 1:1, put them in a mortar, mix and grind them until uniform to obtain a binary mixed molten salt;
[0039] b. Weigh out 3.52g of europium oxide and 3.19g of titanium dioxide (the total mass ratio of inorganic salt to reactant is 3:1) according to the molar ratio of Eu2O3 to TiO2 of 1:4. Place them in the mortar and mix them and continue to grind until uniform to obtain a mixture of Eu2O3, TiO2, KCl and NaCl.
[0040] c. Transfer the mixture to a 50 ml corundum crucible and compact it. Place it in a high-temperature furnace and heat it to 1000 °C at a rate of 10 °C / min. Heat it in air for 4 h and remove the melt. Cool it rapidly at room temperature to obtain a mixture of molten salt and precursor product.
[0041] d. Wash the mixture repeatedly with deionized water and anhydrous ethanol and filter until no white precipitate is formed when the washing solution is tested with silver nitrate reagent;
[0042] e. The powder obtained after filtration is dried in a vacuum oven at 60°C for 6 hours to obtain europium titanate ceramic particles with a particle size of about 660 nm.
[0043] The crystal structure of the product was characterized, and the XRD results are as follows: Figure 1 As shown, by Figure 1 It can be seen that the europium titanate ceramic particles obtained in this embodiment are a single Eu2Ti2O7 phase.
[0044] The microstructure of the product was characterized, and SEM images were taken as follows. Figure 9 As shown, by Figure 9 It can be seen that the europium titanate particles obtained in this embodiment are relatively uniform, with an average diameter of about 661 nm.
[0045] The product was subjected to an Eu leaching rate test, and the results were... Figure 2 As shown, the leaching rate of Eu after 28 days was 1.12 × 10⁻⁶. -7 gm -1 d -1 .
[0046] Comparative Example 1:
[0047] The difference between this comparative example and Example 1 is that the total mass ratio of inorganic salt to reactants is 2:1, while the remaining process steps and parameter settings are the same as in Example 1.
[0048] The crystal phase structure of the europium titanate ceramic particles prepared in this comparative example was characterized. The results showed that the europium titanate ceramic particles were a mixture of Eu2Ti2O7, Eu2TiO5 and TiO2, and no pure Eu2Ti2O7 phase was formed.
[0049] Comparative Example 2:
[0050] The difference between this comparative example and Example 1 is that the total mass ratio of inorganic salt to reactants is 1:1, while the remaining process steps and parameter settings are the same as in Example 1.
[0051] The crystal phase structure of the europium titanate ceramic particles prepared in this comparative example was characterized. The results showed that the europium titanate ceramic particles were a mixture of Eu2Ti2O7 and Eu2TiO5, and no pure Eu2Ti2O7 phase was formed.
[0052] Comparative Example 3:
[0053] The difference between this comparative example and Example 1 is that the molar ratio of Eu2O3 to TiO2 is 1:2, while the remaining process steps and parameter settings are the same as in Example 1.
[0054] The crystal phase structure of the europium titanate ceramic particles prepared in this comparative example was characterized, and the XRD results are as follows: Figure 3 As shown, by Figure 3 It can be seen that the europium titanate ceramic particles are a mixture of Eu2Ti2O7 and Eu2TiO5, and a relatively pure Eu2Ti2O7 phase was not formed. This is mainly because the TiO2 content is low, the system has a high reaction melting point, and it is difficult to react completely to form a relatively pure Eu2Ti2O7 single phase.
[0055] Comparative Example 4:
[0056] The difference between this comparative example and Example 1 is that the molar ratio of Eu2O3 to TiO2 is 1:3, while the remaining process steps and parameter settings are the same as in Example 1.
[0057] The crystal phase structure of the europium titanate ceramic particles prepared in this comparative example was characterized, and the XRD results are as follows: Figure 4 As shown, by Figure 4 It can be seen that the europium titanate ceramic particles are a mixture of Eu2Ti2O7, Eu2TiO5, and TiO2, and a relatively pure Eu2Ti2O7 phase was not formed. Although the TiO2 content increased compared to Comparative Example 3, it still did not reach the melting point for complete reaction of the system, the reaction driving force was insufficient, and the reaction was not completely completed to form a relatively pure Eu2Ti2O7 single phase.
[0058] Example 2:
[0059] The glass-ceramic solidified body was prepared using the europium titanate ceramic particles obtained in Example 1 as raw material, and the specific steps are as follows:
[0060] a. Weigh out 6.01g of silicon dioxide, 4.87g of boron oxide, 2.03g of zinc oxide, and 3.08g of calcium oxide according to the molar percentages of SiO2, B2O3, ZnO, and CaO, respectively. Place them in a mortar, mix and grind until uniform to obtain a mixture.
[0061] b. Transfer the mixture to a 50 ml corundum crucible and compact it. Place it in a high-temperature furnace and heat it to 700 °C for 30 min at a rate of 10 °C / min. Then heat it to 1000 °C and react for 1 h. After the reaction is complete, take out the melt and cool it rapidly at room temperature to obtain a transparent borosilicate glass with europium titanate ceramic package capacity of 0 wt.%, named Glass.
[0062] c. The obtained borosilicate glass is ground into powder using mechanical crushing and collected for subsequent use.
[0063] d. Weigh 9g of borosilicate glass powder and 1g of europium titanate precursor powder according to a mass ratio of 9:1 of borosilicate glass to europium titanate ceramic particles, mix them in a mortar and grind them until uniform to obtain a mixture;
[0064] b. Press the mixture into tightly supported cylinders using a tablet press at 12 MPa for 5 min and transfer them into 50 ml corundum crucibles. Place them in a high-temperature furnace and sinter at 1200 °C for 4 h at a rate of 10 °C / min. After the reaction is complete, turn off the high-temperature furnace and allow it to cool naturally to room temperature inside the furnace to obtain a borosilicate glass-ceramic solidified body.
[0065] c. The obtained borosilicate glass-ceramic solidified body was separated from the corundum crucible by mechanical crushing to obtain a borosilicate glass-ceramic solidified body with a europium titanate ceramic inclusion capacity of 10 wt.%, named 10 wt.%.
[0066] Example 3:
[0067] The difference between this embodiment and embodiment 2 is that in step d, 8g of borosilicate glass powder and 2g of europium titanate precursor powder are weighed according to the mass ratio of borosilicate glass to europium titanate ceramic particles of 8:2. The remaining process steps and parameter settings are the same as in embodiment 2, and a borosilicate glass-ceramic solidified body with a europium titanate ceramic inclusion capacity of 20wt.% is obtained, which is named 20wt.%.
[0068] Example 4:
[0069] The difference between this embodiment and embodiment 2 is that in step d, 7g of borosilicate glass powder and 3g of europium titanate precursor powder are weighed according to the mass ratio of borosilicate glass to europium titanate ceramic particles of 7:3. The remaining process steps and parameter settings are the same as in embodiment 2, and a borosilicate glass-ceramic solidified body with a europium titanate ceramic inclusion capacity of 30wt.% is obtained, which is named 30wt.%.
[0070] Example 5:
[0071] The difference between this embodiment and embodiment 2 is that in step d, 6g of borosilicate glass powder and 4g of europium titanate precursor powder are weighed according to the mass ratio of borosilicate glass to europium titanate ceramic particles of 6:4. The remaining process steps and parameter settings are the same as in embodiment 2, and a borosilicate glass-ceramic solidified body with a europium titanate ceramic inclusion capacity of 40wt.% is obtained, which is named 40wt.%.
[0072] Example 6:
[0073] The difference between this embodiment and embodiment 2 is that in step d, 5g of borosilicate glass powder and 5g of europium titanate precursor powder are weighed according to the mass ratio of borosilicate glass to europium titanate ceramic particles of 5:5. The remaining process steps and parameter settings are the same as in embodiment 2, and a borosilicate glass-ceramic solidified body with a europium titanate ceramic inclusion capacity of 50wt.% is obtained, which is named 50wt.%.
[0074] The crystal phase structure of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6 was characterized, and the XRD results are as follows: Figure 5 As shown, by Figure 5 It is known that pure borosilicate glass exhibits a distinct broad peak in the 20°–35° range, primarily due to its amorphous state. With increasing europium titanate ceramic embedding ratio, the glass-ceramic diffraction peaks show almost no change. When the europium titanate ceramic embedding ratio reaches 40 wt.%, europium titanate diffraction peaks begin to appear, likely due to the excessive embedding of europium titanate.
[0075] The Eu leaching rate of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6 was further characterized, and the results are as follows: Figure 6 As shown, by Figure 6 It can be seen that the Eu leaching rates of the borosilicate glass-ceramic cured bodies prepared in Examples 2-6 were 2.05 × 10⁻⁶ after 28 days. -8 gm -1 d -1 1.21×10 -8 gm -1 d -1 1.42×10 -8 gm -1 d -1 2.35×10 -8 gm -1 d -1 and 2.16×10 -8 gm -1 d -1 .
[0076] The mechanical properties of the borosilicate glass-ceramic solidified bodies prepared in Examples 2-6 were further characterized. The density and Vickers hardness results are as follows: Figure 7 and 8 As shown, by Figure 7 and 8 It can be seen that as the ceramic embedding rate increases, the density of the glass-ceramic gradually increases, but the hardness first increases and then decreases. When the embedding rate increases to 30 wt.%, the hardness of the glass-ceramic reaches its maximum value of 19.53 GPa. Therefore, the maximum embedding rate is determined to be 30 wt.%.
[0077] In summary, the borosilicate glass-ceramic cured body exhibits the best mechanical properties when the europium titanate powder inclusion rate is 30 wt.%, and the normalized leaching rate of Eu on day 28 is only 1.42 × 10⁻⁶. -8 gm -1 d -1 The glass-ceramic cured body has a good morphology and excellent physicochemical properties.
[0078] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.
Claims
1. A method for preparing a glass-ceramic solidified body, characterized in that, Europium titanate was mixed with borosilicate glass powder, ground evenly, and sintered at 1200°C for 4 hours in air atmosphere. After the reaction was completed, it was naturally cooled to room temperature and mechanically crushed to obtain the product. The preparation method of europium titanate is as follows: Eu2O3 and TiO2 are used as raw materials, mixed with KCl and NaCl as molten salts, ground evenly, and the resulting mixed powder is reacted in air at 1000℃ for 4 hours. After the reaction is completed, it is naturally cooled to room temperature. After washing and drying, single-phase europium titanate powder is obtained. The molar ratio of Eu2O3 to TiO2 is 1:4, the molar ratio of KCl to NaCl is 1:1, and the total mass ratio of molten salt to raw materials is 3:
1. The preparation method of borosilicate glass powder is as follows: SiO2, B2O3, ZnO and CaO are mixed and ground evenly. The resulting mixed powder is reacted in air at 1000℃ for 1 hour. After the reaction is completed, it is annealed and ground to obtain borosilicate glass powder. SiO2, B2O3, ZnO and CaO are mixed in molar percentages of 40%, 28%, 10% and 22%, respectively.
2. The preparation method according to claim 1, characterized in that, The annealing process involves removing the melt and allowing it to cool naturally at room temperature.
3. The preparation method according to claim 1, characterized in that, The drying process was carried out at a temperature of 60℃ for 6 hours.
4. A glass-ceramic cured body prepared by the preparation method according to any one of claims 1-3, characterized in that, The glass-ceramic cured body contains 10~50 wt.% europium titanate.
Citation Information
Patent Citations
Preparation method of glass-ceramic composite material containing pyrochlore
CN108314323A