A SEBS rubber composition and preparation method thereof
Hydroxy-modified SEBS was prepared by H2O2 and UV irradiation, combining polyols and isocyanates to solve the compatibility and oil resistance problems of SEBS and TPU during processing, and achieve high performance and stability of SEBS-TPU composite materials.
Patent Information
- Application Number
- CN202410495757.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-24
AI Technical Summary
There are compatibility problems and differences in processing parameters during the processing process of SEBS and TPU, which leads to unstable uniformity and performance of composite materials and low resistance to chemicals, affecting their application life and performance.
Hydroxy-modified SEBS (SEBS-OH) was prepared by strong oxidation of H2O2 and UV irradiation, and polyurethane prepolymers were prepared with polyols and isocyanates to form SEBS-TPU rubber particles, improving compatibility and improving mechanical properties and Oil resistance.
It significantly improves the compatibility and mechanical properties between SEBS and TPU, enhances the oil resistance of the material, avoids material layering or phase separation, and improves the overall performance and sustainability of the material.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and in particular to a SEBS rubber composition and a preparation method thereof. Background Art
[0002] SEBS (styrene-ethylene-butylene-styrene) rubber has good weather resistance, excellent thermal stability, good mechanical strength and elasticity, but SEBS has relatively low resistance to certain chemicals, especially some solvents and greases, which affects its application life and performance in specific chemical environments.
[0003] TPU has good oil resistance while providing excellent wear resistance, high elasticity and strength, while SEBS has good elasticity and flexibility; it helps to improve the material. Combining SEBS (styrene-ethylene-butylene-styrene) with TPU can produce a composite material that has high strength and wear resistance while maintaining good flexibility, elasticity and tear resistance. In addition, SEBS and TPU are both thermoplastic materials, so the composite material can be reshaped and recycled, which is important for reducing waste in the production process and supporting sustainable development. Combining the unique properties of SEBS and TPU, new materials that meet special application needs can be developed, such as high-performance oil-resistant seals, wear-resistant pipes, medical device components, flexible electronic equipment housings, etc.
[0004] Although the combination of SEBS and TPU has the above advantages, the current production process still faces the following challenges:
[0005] (1) Compatibility issues: SEBS is a non-polar or low-polar polymer, while TPU is usually a polar polymer. The polarity difference between the two in molecular structure may lead to compatibility issues, affecting the uniformity and performance of the composite material; poor interface compatibility may lead to insufficient interface adhesion between SEBS and TPU, affecting the mechanical strength and durability of the material;
[0006] (2) Processing issues: The optimal processing parameters for the two materials are relatively complex and need to be carefully adjusted to ensure that the materials can be well mixed and formed. During the processing, if the processing conditions are not appropriate, material stratification or phase separation may occur, resulting in unstable performance of the finished product. Summary of the invention
[0007] In order to solve the above problems, the present application provides a SEBS rubber composition and a preparation method thereof. The preparation method of the SEBS rubber composition comprises the following steps:
[0008] S1: In H 2 O 2The hydroxyl-modified SEBS, i.e. SEBS-OH, was prepared by strong oxidation and UV irradiation.
[0009] S2: dissolving SEBS-OH in solvent A, mixing with polyol and additives, reacting with isocyanate to obtain a polyurethane prepolymer, and recovering solvent A;
[0010] S3: reacting the polyurethane prepolymer with the chain extender and granulating to obtain rubber particles containing SEBS-TPU.
[0011] Preferably, the specific preparation method of SEBS-OH in step S1 includes:
[0012] S101:H 2 O 2 Under the action of catalyst A, hydroxyl radical OH is generated, and the reaction principle is as follows:
[0013]
[0014] S102: SEBS reacts with ·OH, ·OH attacks the SEBS chain, causing the SEBS chain to break and form a new free radical SEBS·. The reaction principle is as follows:
[0015] SEBS-H+·OH→SEBS·+H2O;
[0016] S103: SEBS and O 2 , H 2 O 2 Under the action of UV irradiation and photoinitiator, the peroxide hydroxyl group is introduced into the SEBS chain. The reaction principle is as follows:
[0017]
[0018] SEBS-OO·+H2O2→SEBS-O-OH+·OH+1 / 2O2;
[0019] S104: Under the action of catalyst B, the peroxide hydroxyl groups on the SEBS chain are decomposed and converted into hydroxyl groups. The reaction principle is as follows:
[0020]
[0021] S105: washing and drying the SEBS-OH obtained in S104 to obtain SEBS-OH particles;
[0022] The catalyst A is a transition metal ion compound or a metal oxide, and the catalyst B is a transition metal ion compound.
[0023] Preferably, the preparation method of the polyurethane prepolymer described in step S2 is:
[0024] S201: Add polyol and additives into a reaction kettle, heat to 100-120°C, evacuate for 0.5-1h, remove moisture, and cool to 60-80°C to obtain solution A;
[0025] S202: adding the dried SEBS-OH particles to solvent A, heating to 80-100° C., stirring until the SEBS-OH particles are completely dissolved in solvent A, and cooling to 60-80° C. to obtain solution B;
[0026] S203: adding solution B to solution A, mixing evenly, adding isocyanate, maintaining the temperature at 60-80° C., mixing and reacting for 1.5-2 hours, and obtaining a polyurethane prepolymer with NCO terminal;
[0027] The solvent A is anhydrous toluene or xylene.
[0028] Preferably, the preparation method of the SEBS-TPU rubber particles described in step S3 is:
[0029] S301: After heating the polyurethane prepolymer, a chain extender is added and mixed;
[0030] S302: Casting the mixed material into a SEBS-TPU rubber sheet, crushing the SEBS-TPU rubber sheet, and granulating it with an extruder to obtain SEBS-TPU rubber particles.
[0031] Preferably, a photoinitiator is added to the reaction of steps S101 and S102, and the reaction is carried out under UV irradiation.
[0032] Preferably, the photoinitiator used in steps S101, S102, and S103 is an aromatic ketone photosensitizer or a thioether photosensitizer.
[0033] Preferably, the UV irradiation wavelength of step S103 is 315-350nm, the UV irradiation time is 10-15min, and the UV irradiation intensity is 70-80mW / cm 2 .
[0034] Preferably, in step S101, the UV irradiation wavelength is 220-280 nm, the UV irradiation time is 0.5-1 h, and the UV irradiation intensity is 10-20 mW / cm 2 ;
[0035] In step S102, the UV irradiation wavelength is 100-200nm, the UV irradiation time is 0.5-1h, and the UV irradiation intensity is 40-50mW / cm 2 .
[0036] Preferably, the catalyst A is FeSO 4, Cu 2 SO 4 、MnO 2 、TiO 2 At least one of the catalyst B is FeSO 4 , Cu 2 SO 4 At least one of .
[0037] The present invention also provides a SEBS rubber composition prepared according to any one of the above preparation methods.
[0038] Compared with the known public technologies, the technical solution provided by this application has the following beneficial effects:
[0039] (1) This application is approved by H 2 O 2 The strong oxidation effect of the reaction medium combined with UV irradiation effectively introduces hydroxyl groups (SEBS-OH) on the surface of SEBS, providing active points for further chemical modification. The polyurethane prepolymer is prepared by reacting hydroxyl-modified SEBS (SEBS-OH), polyols and isocyanates. The active hydroxyl groups of SEBS-OH form chemical bonds with isocyanates, which significantly improves the compatibility between SEBS and TPU, and significantly improves the mechanical properties and chemical resistance of the prepared product. The active hydroxyl groups of SEBS-OH form chemical bonds with isocyanates, which enhances the interaction between molecules and forms a relatively tight molecular structure, providing a higher physical barrier to the penetration of oil molecules, limiting the penetration of oil molecules, and thus improving the oil resistance of the material.
[0040] (2) The preparation method of the SEBS rubber composition of the present application does not need to consider the difference in processing parameters between SEBS and TPU. Hydroxyl-modified SEBS (SEBS-OH) is used as an alcohol that can react with isocyanate. The SEBS-TPU rubber composition is prepared in the same way as TPU, so there will be no material stratification or phase separation.
[0041] (3) This application uses UV light with a wavelength of 220-280nm to irradiate H 2 O 2 , which is more conducive to H 2 O 2Absorb light energy and decompose into hydroxyl radicals ·OH. At the same time, UV light can promote the reduction of transition metal ion catalysts, so that transition metal ion catalysts can be recycled and the generation of ·OH is enhanced. SEBS is irradiated with an irradiation wavelength of 100-200nm to excite SEBS molecules to a high energy state. The high energy state SEBS molecules are easy to be strongly oxidized by hydroxyl radicals ·OH to attack the carbon-hydrogen bonds of SEBS molecules to form free radicals SEBS·. UV light with an irradiation wavelength of 315-350nm can promote the reaction of SEBS· and O 2 The reaction generates SEBS-OO·, SEBS-OO· and H 2 O 2 Further reaction produces SEBS-O-OH and ·OH. ·OH can be used to attack excited SEBS molecules in a cycle. Under the action of the catalyst, -O-OH decomposes into -OH and O 2 , O 2 Under UV light, SEBS· is oxidized to make H 2 O 2 be fully utilized;
[0042] (4) The SEBS rubber composition of the present application can be combined by selecting SEBS, isocyanate and polyol with different properties according to different application scenarios. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0044] In the following examples of the present invention, the raw materials used are as follows:
[0045] H 2 O 2 : Content 50%, Anhui Jinyueguan New Material Technology Co., Ltd.;
[0046] Benzophenone: content 99%, Jiangsu Bosite Chemical Technology Co., Ltd.;
[0047] Phenyl methyl sulfide: content 99%, Jiangsu Bosite Chemical Technology Co., Ltd.;
[0048] FeSO 4 7H 2 O: content 99%, Chongqing Xuanyu Chemical Co., Ltd.;
[0049] PEA-2000: polyethylene adipate glycol, molecular weight 2000, hydroxyl value 53-59 mg / KOH / g, Qingdao Xinyutian Chemical Co., Ltd.
[0050] PPG-2000: polyoxypropylene glycol, molecular weight 2000, hydroxyl value 51-62 mg / KOH / g, Shanghai Gaoqiao Petrochemical Company;
[0051] POL-256: polyester diol, molecular weight 2000, hydroxyl value 53-59 mg / KOH / g, Qingdao Xinyutian Chemical Co., Ltd.
[0052] N-330: polyether triol, molecular weight 3000, hydroxyl value 54-57mg / KOH / g, Jiangsu Zhongshan Chemical Co., Ltd., Jiangsu Zhongshan Chemical Co., Ltd.;
[0053] Antioxidant 4020: Ningbo Aikemu New Materials Co., Ltd.
[0054] Silicone oil: Shandong Luderui New Materials Co., Ltd.;
[0055] Methyl stearate: Jiangsu Bosite Chemical Technology Co., Ltd.;
[0056] Carbon black: Tianjin Baochi Chemical Technology Co., Ltd.;
[0057] TDI-80: toluene diisocyanate, Yantai Wanhua Polyurethane Co., Ltd.;
[0058] MDI: diphenylmethane diisocyanate, Yantai Wanhua Polyurethane Co., Ltd.;
[0059] BDO: 1,4-dihydroxybutane, Sichuan Tianhua Co., Ltd.;
[0060] PG: Propylene glycol, Mitsui Chemicals, Ltd., Japan;
[0061] T-9: stannous octoate, Air Products & Chemicals, USA;
[0062] T-12: Dibutyl dilaurate; Air Products & Chemicals, Inc.;
[0063] HQEE: hydroquinone dihydroxyethyl ether, Shandong Yantai Yusheng Chemical Co., Ltd.;
[0064] MOCA: 3,3'-dichloro-4,4'-diphenylmethanediamine, Zhangjiagang Yarui Chemical Co., Ltd.;
[0065] SEBS-G1651: SEBS rubber, American Kraton brand G1651;
[0066] SEBS-MD6945: SEBS rubber, American Kraton brand MD6945;
[0067] SEBS-G1652: SEBS rubber, American Kraton brand G1652;
[0068] SEBS-G1654: SEBS rubber, American Kraton brand G1654;
[0069] SEBS-FG1901: SEBS rubber, American Kraton brand FG1901.
[0070] Example 1
[0071] S1: In H 2 O 2 The hydroxyl-modified SEBS, i.e., SEBS-OH, is prepared under strong oxidation and UV irradiation. The specific steps are as follows:
[0072] S101: Add 400gH into the photocatalytic reactor. 2 O 2 , 30gFeSO 4 7H 2 O, 5.5g of benzophenone was stirred, and the UV lamp was turned on at the same time. The irradiation wavelength was 260nm, the UV irradiation time was 1h, and the UV irradiation intensity was 10mW / cm 2 , the reaction principle of the process includes:
[0073] H2O2+Fe2+→OH2-+·OH+Fe3+,
[0074]
[0075]
[0076] S102: Add 100g SEBS-G1651 to the photocatalytic reactor, adjust the UV irradiation wavelength to 145nm, and the UV irradiation intensity to 40mW / cm 2 , stirred for 1h, the reaction principle of the process is as follows:
[0077] SEBS-H+·OH→SEBS·+H2O;
[0078] S103: oxygen is introduced into the photocatalytic reactor to maintain the pressure in the reactor at 10-15 MPa, the UV irradiation wavelength is adjusted to 320 nm, and the UV irradiation intensity is 70 mW / cm 2 , stirring for 10-15 minutes. The reaction principle of this process includes:
[0079]
[0080] SEBS*+O2→SEBS+1O2,
[0081] SEBS*+O2→SEBS-OO·,
[0082] SEBS-OO·+H2O2→SEBS-O-OH+·OH+1 / 2O2,
[0083] 1O2+H2O→2·OH;
[0084] Among them, SEBS* represents the excited state of SEBS molecules. The excited state SEBS reacts with oxygen to generate singlet oxygen (1O2) and superoxide radicals (-O2·), and the singlet oxygen (1O2) reacts with water to generate hydroxyl radicals.
[0085] S104: Add catalyst 5gFeSO 4 7H 2 O, continue stirring for 40min, the reaction principle of this process is as follows:
[0086]
[0087] S105: The material in the photoreactor is released, washed with water, and dried to obtain SEBS-OH rubber particles.
[0088] S2: dissolving SEBS-OH in solvent A and mixing with polyol, reacting with isocyanate to obtain polyurethane prepolymer, and recovering solvent A. The specific steps are as follows:
[0089] S201: 40g PEA-2000, 5g PPG-2000, 10g POL-256, 2g antioxidant 4020, 0.1g silicone oil, 1g T-9, 1g methyl stearate, and 1g carbon black were added to a reaction kettle, heated to 100-120°C, vacuumed for 0.5-1h, removed moisture, and cooled to 60-80°C to obtain solution A;
[0090] S202: adding 40 g of the dried SEBS-OH particles obtained in step S105 to 50 g of toluene, heating to 80-100° C., stirring until the SEBS-OH particles are completely dissolved in toluene, and cooling to 60-80° C. to obtain solution B;
[0091] S203: adding solution B to solution A, mixing evenly, adding 90g MDI, maintaining the temperature at 60-80°C, mixing and reacting for 1.5-2h, and recovering the toluene solvent to obtain a polyurethane prepolymer with NCO terminal.
[0092] S3: reacting the polyurethane prepolymer with the chain extender and granulating to obtain rubber particles containing SEBS-TPU. The specific steps are as follows:
[0093] S301: Heat the polyurethane prepolymer obtained in step S203 to 90-95° C., add 2 g BDO, and mix quickly;
[0094] S302: The mixed material is cast into a SEBS-TPU rubber sheet through a casting machine. After the SEBS-TPU rubber sheet is crushed, it is granulated by an extruder to obtain SEBS-TPU rubber particles. The temperature of the extruder feeding zone is 90-100°C, the temperature of the middle section is 220-240°C, and the temperature of the end section is 120-130°C.
[0095] Example 2
[0096] Step S1 in this embodiment is the same as that in Embodiment 1.
[0097] S2: dissolving SEBS-OH in solvent A and mixing with polyol, reacting with isocyanate to obtain polyurethane prepolymer, and recovering solvent A. The specific steps are as follows:
[0098] S201: Add 40g PPG-2000, 5g PPG-1000, 10g N-330, 2g antioxidant 4020, 0.1g silicone oil and 1g T-9 into a reaction kettle, heat to 100-120°C, evacuate for 0.5-1h, remove moisture, and cool to 60-80°C to obtain solution A;
[0099] S202: adding 40 g of the dried SEBS-OH particles obtained in step S105 to 50 g of xylene, heating to 80-100° C., stirring until the SEBS-OH particles are completely dissolved in toluene, and cooling to 60-80° C. to obtain solution B;
[0100] S203: adding solution B to solution A, mixing evenly, adding 90g TDI-80, maintaining the temperature at 60-80°C, mixing and reacting for 1.5-2h, and recovering the xylene solvent to obtain a polyurethane prepolymer with NCO terminal.
[0101] S3: reacting the polyurethane prepolymer with the chain extender and granulating to obtain rubber particles containing SEBS-TPU. The specific steps are as follows:
[0102] S301: Heat the polyurethane prepolymer obtained in step S203 to 90-95° C., add 2.5 g PG, and mix quickly;
[0103] S302: The mixed material is cast into a SEBS-TPU rubber sheet through a casting machine. After the SEBS-TPU rubber sheet is crushed, it is granulated by an extruder to obtain SEBS-TPU rubber particles. The temperature of the extruder feeding zone is 90-100°C, the temperature of the middle section is 200-220°C, and the temperature of the end section is 120-130°C.
[0104] Example 3
[0105] S1: In H 2 O 2 The hydroxyl-modified SEBS, i.e., SEBS-OH, is prepared under strong oxidation and UV irradiation. The specific steps are as follows:
[0106] S101: Add 400gH into the photocatalytic reactor. 2 O 2 、20gMnO 2 , 6g phenyl methyl sulfide were stirred, and the UV lamp was turned on at the same time, with an irradiation wavelength of 220nm, a UV irradiation time of 40min, and a UV irradiation intensity of 15mW / cm 2 , the reaction principle of the process is as follows:
[0107]
[0108] S102: Add 100g SEBS-MD6945 to the photocatalytic reactor, adjust the UV irradiation wavelength to 110nm, and the UV irradiation intensity to 45mW / cm 2 , stirring for 1h;
[0109] S103: oxygen is introduced into the photocatalytic reactor to maintain the pressure in the reactor at 10-15 MPa, the UV irradiation wavelength is adjusted to 350 nm, and the UV irradiation intensity is 80 mW / cm 2 , stirring for 10-15 minutes;
[0110] S104: Add catalyst 5gFeSO 4 7H 2 O, continue stirring for 1h;
[0111] S105: The material in the photoreactor is released, washed with water, and dried to obtain SEBS-OH particles.
[0112] Steps S2 and S3 of this embodiment are the same as those of Embodiment 1.
[0113] Example 4
[0114] S1: In H 2 O 2 The hydroxyl-modified SEBS, i.e., SEBS-OH, is prepared under strong oxidation and UV irradiation. The specific steps are as follows:
[0115] S101: Add 500gH into the photocatalytic reactor. 2 O 2 、30gMnO 2 , 7g phenyl methyl sulfide were stirred, and the UV lamp was turned on at the same time, with an irradiation wavelength of 280nm, a UV irradiation time of 1h, and a UV irradiation intensity of 20mW / cm2 ;
[0116] S102: Add 100g SEBS-G1654 to the photocatalytic reactor, adjust the UV irradiation wavelength to 200nm, and the UV irradiation intensity to 50mW / cm 2 , stirring for 1h;
[0117] S103: oxygen is introduced into the photocatalytic reactor to maintain the pressure in the reactor at 10-15 MPa, the UV irradiation wavelength is adjusted to 315 nm, and the UV irradiation intensity is 75 mW / cm 2 , stirring for 10-15 minutes;
[0118] S104: Add 5gCu catalyst 2 SO 4 , continue stirring for 40 min;
[0119] S105: The material in the photoreactor is released, washed with water, and dried to obtain SEBS-OH particles.
[0120] S2: dissolving SEBS-OH in solvent A and mixing with polyol, reacting with isocyanate to obtain polyurethane prepolymer, and recovering solvent A. The specific steps are as follows:
[0121] S201: 35 g PCL-2000, 10 g PTMG-1000, 5 g PEA-1000, 2 g antioxidant 1010, 0.1 g silicone oil, and 1 g T-12 were added to a reaction kettle, heated to 100-120° C., vacuumed for 0.5-1 h, removed moisture, and cooled to 60-80° C. to obtain solution A;
[0122] S202: adding 30 g of the dried SEBS-OH particles obtained in step S105 to 50 g of toluene, heating to 80-100° C., stirring until the SEBS-OH particles are completely dissolved in toluene, and cooling to 60-80° C. to obtain solution B;
[0123] S203: Add solution B to solution A, mix well, add 80g MDI, maintain the temperature at 60-80°C, mix and react for 1.5-2h, and recover the toluene solvent to obtain a NCO-terminated polyurethane prepolymer.
[0124] S3: reacting the polyurethane prepolymer with the chain extender and granulating to obtain rubber particles containing SEBS-TPU. The specific steps are as follows:
[0125] S301: Heat the polyurethane prepolymer obtained in step S203 to 90-95° C., add 3 g HQEE, and mix quickly;
[0126] S302: The mixed material is cast into a SEBS-TPU rubber sheet through a casting machine. After the SEBS-TPU rubber sheet is crushed, it is granulated by an extruder to obtain SEBS-TPU rubber particles. The temperature of the extruder feeding zone is 90-100°C, the temperature of the middle section is 210-230°C, and the temperature of the end section is 130-140°C.
[0127] Example 5
[0128] S1: In H 2 O 2 The hydroxyl-modified SEBS, i.e., SEBS-OH, is prepared under strong oxidation and UV irradiation. The specific steps are as follows:
[0129] S101: Add 500gH into the photocatalytic reactor. 2 O 2 、30gMnO 2 , 7g phenyl methyl sulfide were stirred, and the UV lamp was turned on at the same time, with an irradiation wavelength of 250nm, a UV irradiation time of 30min, and a UV irradiation intensity of 15mW / cm 2 ;
[0130] S102: Add 100g SEBS-G1652 to the photocatalytic reactor, adjust the UV irradiation wavelength to 200nm, and the UV irradiation intensity to 40mW / cm 2 , stirring for 30 minutes;
[0131] S103: oxygen is introduced into the photocatalytic reactor to maintain the pressure in the reactor at 10-15 MPa, the UV irradiation wavelength is adjusted to 350 nm, and the UV irradiation intensity is 70 mW / cm 2 , stirring for 10-15 minutes;
[0132] S104: Add 5gCu catalyst 2 SO 4 , continue stirring for 30 min;
[0133] S105: The material in the photoreactor is released, washed with water, and dried to obtain SEBS-OH particles.
[0134] S2: dissolving SEBS-OH in solvent A and mixing with polyol, reacting with isocyanate to obtain polyurethane prepolymer, and recovering solvent A. The specific steps are as follows:
[0135] S201: Add 30g PPG-2000, 10g PPG-1000, 10g POL-256, 2g antioxidant 1010, 0.1g silicone oil and 1g T-12 into a reaction kettle, heat to 100-120°C, evacuate for 0.5-1h, remove moisture, and cool to 60-80°C to obtain solution A;
[0136] S202: adding 30 g of the dried SEBS-OH particles obtained in step S105 to 50 g of toluene, heating to 80-100° C., stirring until the SEBS-OH particles are completely dissolved in toluene, and cooling to 60-80° C. to obtain solution B;
[0137] S203: Add solution B to solution A, mix well, add 60g TDI, maintain the temperature at 60-80°C, mix and react for 1.5-2h, and recover the toluene solvent to obtain a NCO-terminated polyurethane prepolymer.
[0138] S3: reacting the polyurethane prepolymer with the chain extender and granulating to obtain rubber particles containing SEBS-TPU. The specific steps are as follows:
[0139] S301: Heat the polyurethane prepolymer obtained in step S203 to 90-95° C., add 2.5 g MOCA, and mix quickly;
[0140] S302: The mixed material is cast into a SEBS-TPU rubber sheet through a casting machine. After the SEBS-TPU rubber sheet is crushed, it is granulated by an extruder to obtain SEBS-TPU rubber particles. The temperature of the extruder feeding zone is 90-100°C, the temperature of the middle section is 200-220°C, and the temperature of the end section is 120-130°C.
[0141] -OH content test method:
[0142] The -OH content in SEBS-OH prepared in S1 was determined by chemical titration. The specific method is as follows:
[0143] Weigh 2g SEBS-OH rubber particles and 30g xylene into a clean conical flask, heat and reflux for 30 minutes, wait for the solution to cool to 60°C, add two drops of phenolphthalein indicator to the solution, use NaOH as the titrant, and record the volume of NaOH consumed at the neutralization point.
[0144] Based on the volume of titrant consumed and its concentration, the total amount of -OH in the sample can be calculated. The formula is as follows:
[0145] -OH content (mol) = NaOH volume (L) × NaOH concentration (mol / L);
[0146] -OH content in SEBS-OH = -OH content (mol) × 17 (-OH molar mass g / mol) × 100% / 2 g (SEBS-OH mass).
[0147] The content of SEBS-OH rubber particles -OH in step S1 in Example 1, Example 3 and Example 4 is shown in Table 1.
[0148] Table 1 Content of SEBS-OH rubber particles -OH in step S1 in Example 1, Example 3-Example 5
[0149] Example 1 Example 3 Example 4 Example 5 -OH content (%) 2.27% 1.93% 2.08% 1.52%
[0150] Comparative Example 1
[0151] The difference between this comparative example and Example 1 is that the UV irradiation wavelength in steps S101, S102 and S103 is 320 nm.
[0152] Comparative Example 2
[0153] The difference between this comparative example and Example 1 is that the UV irradiation wavelength in steps S101, S102 and S103 is 260 nm.
[0154] Comparative Example 3
[0155] The difference between this comparative example and Example 1 is that the UV irradiation wavelength in steps S101, S102 and S103 is 145 nm.
[0156] Comparative Example 4
[0157] The difference between this comparative example and Example 1 is that the UV irradiation wavelength in step S101 is 300 nm, the UV irradiation wavelength in step S102 is 260 nm, and the UV irradiation wavelength in step S103 is 380 nm.
[0158] The content of SEBS-OH rubber particles -OH in step S1 in comparative examples 1-4 is shown in Table 2.
[0159] Table 2 Content of SEBS-OH rubber particles -OH in step S1 in Example 1 and Comparative Examples 1-4
[0160] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 -OH content (%) 2.27% 0.87% 1.12% 0.94% 1.28%
[0161] Comparative Example 5
[0162] S1: Use of SEBS:
[0163] The SEBS of the same quality as American Kraton brand FG1901 is used to replace the SEBS-OH rubber particles in Example 5. The SEBS of FG1901 is G1652 grafted with maleic anhydride at a grafting rate of 1.5%. The SEBS used in Example 5 is G1652.
[0164] Steps S2 and S3 are consistent with those in Example 5.
[0165] Comparative Example 6
[0166] S1: Use of SEBS, same as Comparative Example 5.
[0167] S2: Preparation of polyurethane prepolymer, which differs from Example 5 in that maleic anhydride grafted SEBS is not added;
[0168] S3: Preparation of SEBS-TPU rubber particles, the specific steps are as follows:
[0169] S301: Heat the polyurethane prepolymer obtained in step S2 to 90-95° C., add 2.8 g MOCA, and mix quickly;
[0170] S302: The mixed material is cast into a TPU rubber sheet by a casting machine. The TPU rubber sheet is crushed and then mixed with 30g SEBS-FG1901 in step S1 by an extruder to obtain SEBS-TPU rubber particles.
[0171] Comparative Example 7
[0172] S1: SEBS uses SEBS-G1651 without hydroxyl modification.
[0173] S2: Preparation of polyurethane prepolymer, which differs from Example 1 in that SEBS-G1651 is not added;
[0174] S3: Preparation of SEBS-TPU rubber particles, the specific steps are as follows:
[0175] S301: Heat the polyurethane prepolymer prepared in step S2 to 90-95° C., add 2.4 g BDO, and mix quickly;
[0176] S302: The mixed material is cast into a TPU rubber sheet by a casting machine. The TPU rubber sheet is crushed and then mixed with 40g SEBS-G1651 in step S1 by an extruder to obtain SEBS-TPU rubber particles.
[0177] Comparative Example 8
[0178] S1: SEBS uses SEBS-G1651 without hydroxyl modification.
[0179] S2: Preparation of polyurethane prepolymer, which differs from Example 2 in that SEBS-G1651 is not added;
[0180] S3: Preparation of SEBS-TPU rubber particles, the specific steps are as follows:
[0181] S301: Heat the polyurethane prepolymer obtained in step S2 to 90-95° C., add 2.7 g PG, and mix quickly;
[0182] S302: The mixed material is cast into a TPU rubber sheet by a casting machine. The TPU rubber sheet is crushed and then mixed with 40g SEBS-G1651 in step S1 by an extruder to obtain SEBS-TPU rubber particles.
[0183] Comparative Example 9
[0184] S1: SEBS uses SEBS-MD6945 without hydroxyl modification.
[0185] S2: Preparation of polyurethane prepolymer, which differs from Example 3 in that SEBS-MD6945 is not added;
[0186] S3: Preparation of SEBS-TPU rubber particles, the specific steps are as follows:
[0187] S301: Heat the polyurethane prepolymer prepared in step S2 to 90-95° C., add 2.4 g BDO, and mix quickly;
[0188] S302: The mixed material is cast into a TPU rubber sheet by a casting machine. The TPU rubber sheet is crushed and then mixed with 40g SEBS-MD6945 in step S1 by an extruder to obtain SEBS-TPU rubber particles.
[0189] Comparative Example 10
[0190] S1: SEBS uses SEBS-G1654 without hydroxyl modification.
[0191] S2: Preparation of polyurethane prepolymer, which differs from Example 4 in that SEBS-G1654 is not added;
[0192] S3: Preparation of SEBS-TPU rubber particles, the specific steps are as follows:
[0193] S301: Heat the polyurethane prepolymer obtained in step S2 to 90-95° C., add 3.2 g HQEE, and mix quickly;
[0194] S302: The mixed material is cast into a TPU rubber sheet by a casting machine. The TPU rubber sheet is crushed and then mixed with 30g SEBS-G1654 in step S1 by an extruder to obtain SEBS-TPU rubber particles.
[0195] The mechanical property test, chemical property test and weather resistance test of SEBS-TPU rubber were carried out using the rubber testing method. The test results are shown in Tables 3 to 12.
[0196] Table 3 Mechanical properties test results of Example 5, Comparative Example 5 and Comparative Example 6
[0197]
[0198]
[0199] Table 4 Oil resistance test results of Example 5, Comparative Example 5 and Comparative Example 6 (test conditions: 70°C × 7d)
[0200]
[0201] Table 5 Mechanical properties test results of Example 1 and Comparative Example 7
[0202]
[0203]
[0204] Table 6 Oil resistance test results of Example 1 and Comparative Example 7 (test conditions: 70°C × 7d)
[0205]
[0206] Table 7 Mechanical properties test results of Example 2 and Comparative Example 8
[0207]
[0208]
[0209] Table 8 Oil resistance test results of Example 2 and Comparative Example 8 (test conditions: 70°C × 7d)
[0210]
[0211] Table 9 Mechanical properties test results of Example 3 and Comparative Example 9
[0212]
[0213]
[0214] Table 10 Oil resistance test results of Example 3 and Comparative Example 9 (test conditions: 70°C × 7d)
[0215]
[0216] Table 11 Mechanical properties test results of Example 4 and Comparative Example 10
[0217]
[0218]
[0219] Table 12 Oil resistance test results of Example 4 and Comparative Example 10 (test conditions: 70°C × 7d)
[0220]
[0221] It can be concluded from Table 1-Table 2 that hydroxyl groups are successfully introduced into SEBS molecules through free radical reaction; it can be concluded from Table 3-Table 4 that SEBS-OH modified by hydroxyl groups has better compatibility with TPU than SEBS grafted by maleic anhydride, and the mechanical properties and oil resistance of the obtained rubber composition are better. Table 3-Table 12 shows that SEBS-OH reacts chemically with isocyanate, which significantly improves the compatibility between SEBS and TPU, so that the mechanical properties and oil resistance of the rubber composition of SEBS and TPU can be significantly improved. The above embodiments are only used to illustrate the technical solutions of the present application, not to limit them; although the present application is described in detail with reference to the aforementioned embodiments, ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein by equivalent; and these modifications or replacements will not make the essence of the corresponding technical solutions deviate from the protection scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing a SEBS rubber composition, characterized in that: The following steps are involved: S1: Preparation of hydroxyl-modified SEBS, i.e., SEBS-OH, under strong oxidation by H2O2 and UV irradiation; S2: dissolving SEBS-OH in solvent A, mixing with polyol and additives, reacting with isocyanate to obtain a polyurethane prepolymer, and recovering solvent A; S3: reacting the polyurethane prepolymer with the chain extender and granulating to obtain rubber particles containing SEBS-TPU.
2. The preparation method of SEBS rubber composition according to claim 1, characterized in that, The specific preparation method of SEBS-OH in step S1 includes: S101: H2O2 generates hydroxyl radical OH under the action of catalyst A. The reaction principle is as follows: S102: SEBS reacts with ·OH, ·OH attacks the SEBS chain, causing the SEBS chain to break and form a new free radical SEBS·. The reaction principle is as follows: SEBS-H+·OH→SEBS·+H2O; S103: SEBS· and O2, H2O2 are oxidized under UV irradiation and the action of photoinitiator, and the peroxide hydroxyl group is introduced into the SEBS chain. The reaction principle is as follows: SEBS-OO·+H2O2→SEBS-O-OH+·OH+1 / 2O2; S104: Under the action of catalyst B, the peroxide hydroxyl groups on the SEBS chain are decomposed and converted into hydroxyl groups. The reaction principle is as follows: S105: washing and drying the SEBS-OH obtained in S104 to obtain SEBS-OH particles; The catalyst A is a transition metal ion compound or a metal oxide, and the catalyst B is a transition metal ion compound.
3. The preparation method of SEBS rubber composition according to claim 2, characterized in that, The preparation method of the polyurethane prepolymer described in step S2 is: S201: Add polyol and additives into a reaction kettle, heat to 100-120°C, evacuate for 0.5-1h, remove moisture, and cool to 60-80°C to obtain solution A; S202: adding the dried SEBS-OH particles to solvent A, heating to 80-100° C., stirring until the SEBS-OH particles are completely dissolved in solvent A, and cooling to 60-80° C. to obtain solution B; S203: adding solution B to solution A, mixing evenly, adding isocyanate, maintaining the temperature at 60-80° C., mixing and reacting for 1.5-2 hours, and obtaining a polyurethane prepolymer with NCO terminal; The solvent A is anhydrous toluene or xylene.
4. The method for preparing a SEBS rubber composition according to claim 3, wherein The preparation method of the SEBS-TPU rubber particles described in step S3 is: S301: After heating the polyurethane prepolymer, a chain extender is added and mixed; S302: Casting the mixed material into a SEBS-TPU rubber sheet, crushing the SEBS-TPU rubber sheet, and granulating it with an extruder to obtain SEBS-TPU rubber particles.
5. The preparation method of SEBS rubber composition according to claim 2, characterized in that, In steps S101 and S102, a photoinitiator is added to the reaction, and the reaction is carried out under UV irradiation.
6. The method for preparing a SEBS rubber composition according to claim 5, wherein: The photoinitiator used in steps S101, S102, and S103 is an aromatic ketone photosensitizer or a thioether photosensitizer.
7. The method for preparing a SEBS rubber composition according to claim 5, characterized in that: The UV irradiation wavelength of step S103 is 315-350nm, the UV irradiation time is 10-15min, and the UV irradiation intensity is 70-80mW / cm 2 .
8. The method for preparing a SEBS rubber composition according to claim 5, wherein: In step S101, the UV irradiation wavelength is 220-280nm, the UV irradiation time is 0.5-1h, and the UV irradiation intensity is 10-20mW / cm 2 ; In step S102, the UV irradiation wavelength is 100-200nm, the UV irradiation time is 0.5-1h, and the UV irradiation intensity is 40-50mW / cm 2 .
9. The method for preparing a SEBS rubber composition according to claim 2, wherein: The catalyst A is at least one of FeSO4, Cu2SO4, MnO2, and TiO2, and the catalyst B is at least one of FeSO4 and Cu2SO4.
10. A SEBS rubber composition, characterized in that: Obtained according to any one of the preparation methods of claims 1-9.
Citation Information
Patent Citations
SEBS-based compatibilizer and preparation method thereof
CN108250389A
Modified SEBS composite material for automobile injection molding interior decoration, and preparation method thereof
CN111117140A