Powder material and preparation method thereof

CN118173867BActive Publication Date: 2024-11-05SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410483389.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-19
Publication Date
2024-11-05
Estimated Expiration
2044-04-19

AI Technical Summary

Technical Problem

[0011]有鉴于此,本申请提供一种粉体材料及其制备方法,旨在改善锂镧锆氧粉体材料由于铝的掺杂量过多或过少而导致的性能不均衡的问题

Benefits of technology

[0030] The benefit of this application is that it provides a powder material with relatively balanced properties and a preparation method thereof.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118173867B_ABST
    Figure CN118173867B_ABST
Patent Text Reader

Abstract

The present application discloses a powder material and a preparation method thereof. The powder material can be used to form a solid electrolyte in a battery, and the chemical formula of the powder material is Li 7‑ 3x La3Zr2Al x O 12 , wherein the value range of X is: 0.05 to 1; the benefit of the present application is that it provides a powder material with relatively balanced performance and a preparation method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a powder material and a preparation method thereof. Background Art

[0002] Batteries (secondary batteries) have been widely used in various fields, such as power storage devices for mobile phones, notebooks, and tablet computers.

[0003] However, current batteries have higher requirements on safety and charging performance when used as power batteries.

[0004] Among them, compared with liquid batteries, the electrolytes of solid-state batteries (including all-solid-state batteries and semi-solid-state batteries) are wholly or partially composed of solid electrolytes.

[0005] Because solid electrolytes are non-flammable, high temperature resistant, non-corrosive, and non-volatile, the mechanical strength, thermal stability, and electrochemical stability of solid electrolytes are better than those of liquid battery electrolytes.

[0006] Therefore, solid-state batteries are undoubtedly more suitable as energy storage devices for electric vehicles such as electric vehicles.

[0007] Lithium lanthanum zirconium oxide powder material with garnet structure is a commonly used solid electrolyte raw material. Some related technologies have explored how to improve its electrochemical performance. Among them, element doping is a relatively important technical direction.

[0008] In some related technologies, it was found that aluminum doping can improve the electrochemical properties of solid electrolytes such as ionic conductivity, so a higher aluminum doping amount was used. This part of the related technology did not realize the negative impact of aluminum doping on ionic conductivity; nor did it realize the impact of aluminum doping on safety performance such as mass specific heat capacity peak.

[0009] In other related technologies, although it is believed that aluminum doping can improve the ionic conductivity of solid electrolytes, it is believed that aluminum doping will affect the original crystal structure, especially the concentration of lithium ions after forming the solid electrolyte. Therefore, a lower aluminum doping amount is used. Although this part of the related technology is aware of the impact of excessive aluminum doping, it does not give a clear relationship between the aluminum doping amount and electrochemical performance. These related technologies are too conservative in aluminum doping, and cannot effectively improve the electrochemical performance of solid electrolytes, giving up the potential for material modification. Of course, these related technologies are also not aware of the impact of aluminum doping on safety performance such as mass specific heat capacity peak, that is, safety performance and powder performance are not used as performance targets to limit the aluminum doping amount.

[0010] In fact, when lithium lanthanum zirconium oxide powder materials are doped with aluminum, the electrochemical properties are often correlated with the powder properties and / or safety performance. If we only focus on improving the electrochemical performance, we will ultimately fail to take into account the correlation between the powder performance and / or safety performance, resulting in uneven performance of the solid-state battery and inability to truly apply it to the market. Summary of the invention

[0011] In view of this, the present application provides a powder material and a preparation method thereof, aiming to improve the problem of uneven performance of lithium lanthanum zirconium oxide powder materials caused by excessive or insufficient aluminum doping.

[0012] The embodiment of the present application is implemented as follows: a powder material is suitable for constituting a solid electrolyte in a battery, and the chemical formula of the powder material is Li 7-3x La3Zr2Al x O 12 , where the value range of X is: 0.05 to 1.

[0013] Optionally, in some embodiments of the present application, the value range of X is: 0.2 to 0.6.

[0014] Optionally, in some embodiments of the present application, the value range of X is: 0.05 to 0.095, or 0.105 to 0.195, or 0.205 to 0.245, or 0.255 to 0.295, or 0.305 to 0.345, or 0.355 to 0.595, or 0.605 to 1.0.

[0015] Optionally, in some embodiments of the present application, the ratio of the peak value of mass specific heat capacity of the powder material to the ionic conductivity ranges from 2100 to 15000.

[0016] Optionally, in some embodiments of the present application, the ratio of the elastic modulus of the powder material to the ionic conductivity of the powder material ranges from 66 to 430.

[0017] Accordingly, the present invention also provides a method for preparing a powder material, comprising the following steps:

[0018] Mixing the precursors of the components in the powder material to obtain a first mixed solution;

[0019] adding a complexing agent to the first mixed solution to obtain a second mixed solution;

[0020] freeze-drying the second mixed solution to obtain a first powder material;

[0021] Grinding the first powder material to obtain a second powder material;

[0022] heat-treating the second powder material to obtain a third powder material;

[0023] Grinding the third powder material to obtain a fourth powder material;

[0024] Drying the fourth powder material to obtain the powder material;

[0025] Wherein, the chemical formula of the powder material is Li 7-3x La3Zr2Al x O 12 , where the value range of X is: 0.05 to 1.

[0026] Optionally, in some embodiments of the present application, the first mixed solution includes: LiOH, La(NO3)3, Zr(NO3)4 and Al(NO3)3·9H2O.

[0027] Optionally, in some embodiments of the present application, the complexing agent is one or more of malic acid, citric acid, malonic acid, succinic acid, succinic acid, lactic acid, and ethylenediaminetetraacetic acid.

[0028] Optionally, in some embodiments of the present application, the insulation temperature of the heat treatment ranges from 600°C to 1200°C; the protection time of the heat treatment ranges from 4h to 15h.

[0029] Correspondingly, an embodiment of the present application further provides a battery, comprising a solid electrolyte composed of the above-mentioned powder material or the powder material prepared by the above-mentioned preparation method.

[0030] The benefit of the present application lies in that it provides a powder material with relatively balanced performance and a preparation method thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 It is a schematic diagram of the main steps of a method for preparing a powder material provided in an embodiment of the present application;

[0033] Figure 2 This is a physical photo of a powder material provided in Example 1 of the present application;

[0034] Figure 3The figure shows the numerical changes of the ionic conductivity of the powder materials of each embodiment of the present application;

[0035] Figure 4 The numerical changes of the peak values ​​of mass specific heat capacity of the powder materials of various embodiments of the present application are shown;

[0036] Figure 5 The figure shows the numerical changes of the elastic modulus of the powder materials in various embodiments of the present application;

[0037] Figure 6 The numerical changes of the initial voltage of the batteries prepared by the same process using the powder materials of each embodiment of the present application are shown;

[0038] Figure 7 The numerical changes of the ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material of each embodiment of the present application are shown;

[0039] Figure 8 The figure shows the numerical changes of the ratio of the elastic modulus value to the ionic conductivity of the powder material of each embodiment of the present application;

[0040] Fig. 9 The figure shows the numerical change of the ratio of the mass specific heat capacity peak value to the initial voltage of the powder material in each embodiment of the present application;

[0041] Fig.10 The numerical changes of the ratio of the elastic modulus value to the initial voltage of the powder material in each embodiment of the present application are shown. DETAILED DESCRIPTION

[0042] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0044] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0045] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or more", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0046] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0047] The technical solution of this application is as follows:

[0048] In a first aspect, an embodiment of the present application provides a powder material suitable for constituting a solid electrolyte in a battery, wherein the chemical formula of the powder material is Li 7-3x La3Zr2Al x O 12 . The value range of X is: 0.05 to 1.

[0049] Specifically, the powder material of the present application is equivalent to aluminum doping on the basis of lithium lanthanum zirconium oxide powder material, but this does not mean that when preparing the powder material of the present application, undoped lithium lanthanum zirconium oxide powder material must be prepared in advance.

[0050] In the technical solution of the present application, aluminum is doped to replace lithium. Since aluminum ions (+3) have a higher valence than Li ions (+1), the aluminum-doped solid electrolyte has a lower lithium ion concentration and a higher vacancy concentration, and the arrangement of lithium ions tends to be disordered, thereby improving the ionic conductivity of the solid electrolyte; and it can effectively reduce the initial voltage and improve the fast charging and discharging performance of the solid-state battery it constitutes.

[0051] However, as the amount of aluminum doping increases, the concentration of lithium ions in the solid electrolyte further decreases and the vacancy concentration further increases. Since there is an optimal value for the concentration of lithium ions / vacancies as carriers, when a certain equilibrium point is exceeded, the ionic conductivity tends to decrease.

[0052] Reference Figure 3 As shown, the test data of the embodiments of the present application also proves the above trend.

[0053] Therefore, even if the safety performance and powder performance of the powder material are not considered, and only the ionic conductivity of the powder material is considered, the doping amount of aluminum needs to be controlled rather than simply increased or decreased.

[0054] Therefore, the doping amount of aluminum in the powder material of the present application is limited so that the solid electrolyte formed by it has corresponding ionic conductivity.

[0055] In some embodiments of the present application, the value range of X may be a value range defined by the following combinations of two preset values:

[0056] 0.05, 0.095, 0.1, 0.105, 0.15, 0.195, 0.2, 0.205, 0.245, 0.25, 0.255, 0.295, 0.3, 0.305, 0.345, 0.35, 0.355, 0.4, 0.45, 0.5, 0.55, 0.595, 0.6, 0.605, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.

[0057] As a preferred solution, the value range of X can be at least one of the following value ranges: 0.05 to 0.095, 0.105 to 0.195, 0.205 to 0.245, 0.255 to 0.295, 0.305 to 0.345, 0.355 to 0.595, 0.605 to 1.0.

[0058] As the amount of aluminum doping increases, the peak value of the mass specific heat capacity of the powder material tends to decrease. The peak value of the mass specific heat capacity of the powder material often determines the maximum temperature rise of the battery; the larger the peak value of the mass specific heat capacity, the smaller the maximum temperature rise of the battery, and the safer the battery.

[0059] Therefore, from the perspective of balancing the two properties of ionic conductivity and mass specific heat capacity peak, it is necessary to control the doping amount of aluminum.

[0060] Reference Figure 4 and Figure 7 As shown, the test data of the embodiments of the present application also proves the above trend.

[0061] Therefore, it is necessary to balance the ratio of the ionic conductivity of the powder material to the peak value of the mass specific heat capacity of the powder material.

[0062] In some embodiments of the present application, the ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material ranges from 2182 to 2990.

[0063] It should be noted that in the present application, the ratio of each performance parameter is the numerical value generated when the following preset units are used as the measurement units as the corresponding numerator and denominator in the ratio:

[0064] The preset unit of ionic conductivity σ is mS / cm;

[0065] The preset unit of mass specific heat capacity peak value C is J / (kg·℃);

[0066] The default unit of elastic modulus E is GPa;

[0067] The preset unit of the initial voltage V is mV;

[0068] The default unit of critical current density is mA / cm 2 ;

[0069] The preset unit of the maximum battery temperature rise is ℃;

[0070] The default unit of specific surface area is m 2 / g;

[0071] The preset unit of median particle size is μm;

[0072] The default unit of tap density is g / cm 3 .

[0073] Take the ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material as an example.

[0074] At this time, it is assumed that the ionic conductivity is 0.1 mS / cm; and the mass specific heat capacity peak is 3134 J / (kg·℃).

[0075] Since they are all the preset units defined above, the ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material is the ratio calculated as 3134 / 0.1.

[0076] In this application, the ratio between any two performance parameters is subject to the above ratio definition. It should be noted that for dimensionless molecular weight and density, they are directly treated as constants and ratioed with other dimensioned performance parameters in preset units.

[0077] Reference Figure 7 As shown, it is obvious that when X takes a value between 0.205 and 0.5, the ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material is relatively gentle, indicating that in this interval, the ionic conductivity of the mass specific heat capacity peak value and the ionic conductivity performance of the powder material are relatively balanced. Within this interval, as a further preferred scheme, when X takes the following values: 0.205 to 0.245, 0.255 to 0.295, 0.305 to 0.345, 0.355 to 0.5, the ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material is very gentle, indicating that the balance of these two properties is better.

[0078] The above scheme is used to control the doping amount of aluminum so that the powder material can take into account both ionic conductivity and mass specific heat capacity peak.

[0079] Similarly, comparing the ionic radius under the same coordination number, the ionic radius of aluminum (0.39 angstroms) is smaller than the ionic radius of lithium (0.59 angstroms), and the ionic charge is greater, so the force on the anion is greater, and the stronger binding force is beneficial to improving the elastic modulus of the solid electrolyte.

[0080] Reference Figure 5 As shown, the data of the examples of the present application indeed show a trend that the elastic modulus of the powder material gradually increases with the increase of the aluminum doping amount.

[0081] The elastic modulus of the powder material is positively correlated with the critical current density of the electrolyte of the solid-state battery it constitutes, that is, the higher the elastic modulus of the powder material, the higher the critical current density of the electrolyte of the solid-state battery it constitutes.

[0082] It should be noted that parameters such as elastic modulus in this application are not direct performance parameters of powder materials, but are measured according to the sample preparation method and testing method of this application. For the sake of convenience, they are briefly described as the performance of powder materials, such as "elastic modulus of powder materials", but they are actually the performance of sheets made of powder materials. Similar parameters include ionic conductivity, etc.

[0083] Reference Figures 1 to 5As shown, the increase in critical current density brought about by the increase in the elastic modulus of the powder material can compensate for the decrease in ionic conductivity to a certain extent. Therefore, when safety performance such as the peak mass specific heat capacity is not considered, the relative electrochemical performance can still be maintained even when the ionic conductivity has shown a downward trend due to the increase in the amount of aluminum doping.

[0084] However, although the elastic modulus is not a direct electrochemical property, it is itself a powder property (the powder properties in this application include both the physical and chemical properties of the powder itself and the physical and chemical properties of the solid electrolyte composed of the powder), but it is related to the critical current density in the electrochemical properties, so it can be equated with the electrochemical properties.

[0085] Reference Figure 8 As shown, based on the complementary effect of critical current density and ionic conductivity, the powder material of the present application also needs to balance the elastic modulus and ionic conductivity of the powder material.

[0086] As a preferred solution, the ratio of the elastic modulus to the ionic conductivity of the powder material ranges from 66 to 430.

[0087] Among them, when X takes the following values: 0.05 to 0.095, 0.105 to 0.195, 0.205 to 0.245, 0.255 to 0.295, 0.305 to 0.345, 0.355 to 0.45, the ratio of the elastic modulus to the ionic conductivity of the powder material is flat.

[0088] Based on such interval selection, the ratio of the elastic modulus to the ionic conductivity of the powder material can range from 66 to 130.

[0089] Reference Fig. 9 and Fig.10 As shown, a similar balance also exists in the ratio of the mass specific heat capacity peak to the initial voltage and the ratio of the elastic modulus to the initial voltage. Therefore, the selection of the X range and the selection of the performance parameter itself can also be performed based on the above logic and the data of the embodiments of the present application, which will not be repeated here.

[0090] In a second aspect, an embodiment of the present application further provides a method for preparing a powder material, comprising the following steps:

[0091] Mixing the precursors of the components in the powder material to obtain a first mixed solution;

[0092] adding a complexing agent to the first mixed solution to obtain a second mixed solution;

[0093] freeze-drying the second mixed solution to obtain a first powder material;

[0094] Grinding the first powder material to obtain a second powder material;

[0095] heat-treating the second powder material to obtain a third powder material;

[0096] Grinding the third powder material to obtain a fourth powder material;

[0097] Drying the fourth powder material to obtain the powder material;

[0098] Wherein, the chemical formula of the powder material is Li 7-3x La3Zr2Al x O 12 , where the value range of X is: 0.05 to 1.

[0099] Optionally, in some embodiments of the present application, the first mixed solution includes: LiOH, La(NO3)3, Zr(NO3)4 and Al(NO3)3·9H2O.

[0100] Optionally, in some embodiments of the present application, the complexing agent is one or more of malic acid, citric acid, malonic acid, succinic acid, succinic acid, lactic acid, and ethylenediaminetetraacetic acid.

[0101] Optionally, in some embodiments of the present application, the insulation temperature of the heat treatment ranges from 600°C to 1200°C; the protection time of the heat treatment ranges from 4h to 15h.

[0102] In a third aspect, an embodiment of the present application further provides a battery, specifically a solid-state battery, which comprises a solid electrolyte composed of the above-mentioned powder material or the powder material prepared by the above-mentioned preparation method.

[0103] The present application is further described below with reference to the embodiments:

[0104] Example 1

[0105] Li 6.85 La3Zr2Al 0.05 O 12

[0106] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.89 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.19 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0107] Step 2: Add 37.51 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0108] Step 3: freeze-dry the second mixed solution, first using liquid nitrogen to freeze the solution, and then using a freeze dryer to dry it to obtain a dry powder.

[0109] Step 4: Use agate to grind the dry powder and grind it for 30 minutes to obtain fine powder particles.

[0110] Step 5: Use a box furnace to heat treat the refined powder at 750 degrees for 6 hours.

[0111] Step 6: Perform high-energy planetary ball milling. The ball milling system is as follows: use 6 mm zirconium oxide balls, the mass ratio of zirconium oxide balls to solid electrolyte materials is 4:1, the mass ratio of grinding medium isopropanol to solid electrolyte materials is 3:1, the rotation speed is 450 rpm, and the ball milling time is 9 hours.

[0112] Step 7: After ball milling, the mixture is dried in a blast oven at 80 degrees to obtain the final powder material.

[0113] Example 2Li 6.715 La3Zr2Al 0.095 O 12

[0114] The difference between it and Example 1 is:

[0115] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.85 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.36 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0116] Step 2: Add 37.23 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0117] Example 3

[0118] Li 6.7 La3Zr2Al 0.1 O 12

[0119] The difference between it and embodiment 1 is:

[0120] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.85 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.38 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0121] Step 2: Add 37.19 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0122] Example 4

[0123] Li 6.685 La3Zr2Al 0.105 O 12

[0124] The difference between it and embodiment 1 is:

[0125] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.84 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.39 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0126] Step 2: Add 37.16 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly by magnetic stirring to obtain a second mixed solution.

[0127] Example 5

[0128] Li 6.55 La3Zr2Al 0.15 O 12

[0129] The difference between it and embodiment 1 is:

[0130] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.80 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.56 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0131] Step 2: Add 36.88 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0132] Example 6

[0133] Li 6.415 La3Zr2Al 0.195 O 12

[0134] The difference between it and embodiment 1 is:

[0135] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.77 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.73 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0136] Step 2: Add 36.6 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0137] Example 7

[0138] Li 6.4 La3Zr2Al 0.2 O 12

[0139] The difference between it and embodiment 1 is:

[0140] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.76 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.75 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0141] Step 2: Add 36.56 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0142] Example 8

[0143] Li 6.385 La3Zr2Al 0.205 O 12

[0144] The difference between it and embodiment 1 is:

[0145] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.76 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.77 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0146] Step 2: Add 36.53 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0147] Example 9

[0148] Li 6.265 La3Zr2Al 0.245 O 12

[0149] The difference between it and embodiment 1 is:

[0150] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.73 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.92 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0151] Step 2: Add 36.28 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0152] Example 10

[0153] Li 6.25 La3Zr2Al 0.25 O 12

[0154] The difference between it and embodiment 1 is:

[0155] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.72 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.94 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0156] Step 2: Add 36.25 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0157] Embodiment 11

[0158] Li 6.235 La3Zr2Al 0.255 O 12

[0159] The difference between it and embodiment 1 is:

[0160] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.72 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 0.96 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0161] Step 2: Add 36.22 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0162] Example 12

[0163] Li 6.115 La3Zr2Al 0.295 O 12

[0164] The difference between it and embodiment 1 is:

[0165] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.68 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.11 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0166] Step 2: Add 35.97 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0167] Example 13

[0168] Li 6.1 La3Zr2Al 0.3 O 12

[0169] The difference between it and embodiment 1 is:

[0170] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.68 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.13 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0171] Step 2: Add 35.93 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0172] Embodiment 14

[0173] Li 6.085 La3Zr2Al 0.305 O 12

[0174] The difference between it and embodiment 1 is:

[0175] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.68 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.14 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0176] Step 2: Add 35.9 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0177] Embodiment 15

[0178] Li 5.965 La3Zr2Al 0.345 O 12

[0179] The difference between it and embodiment 1 is:

[0180] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.64 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.29 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0181] Step 2: Add 35.65 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0182] Example 16

[0183] Li 5.95 La3Zr2Al 0.35 O 12

[0184] The difference between it and embodiment 1 is:

[0185] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.64 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.31 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0186] Step 2: Add 35.62 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0187] Embodiment 17

[0188] Li 5.935 La3Zr2Al 0.355 O 12

[0189] The difference between it and embodiment 1 is:

[0190] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.63 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.33 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0191] Step 2: Add 35.59 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0192] Embodiment 18

[0193] Li 5.8 La3Zr2Al 0.4 O 12

[0194] The difference between it and embodiment 1 is:

[0195] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.6 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.5 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0196] Step 2: Add 35.3 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0197] Embodiment 19

[0198] Li 5.65 La3Zr2Al 0.45 O 12

[0199] The difference between it and embodiment 1 is:

[0200] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.56 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.69 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0201] Step 2: Add 34.99 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0202] Embodiment 20

[0203] Li 5.5 La3Zr2Al 0.5 O 12

[0204] The difference between it and embodiment 1 is:

[0205] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.51 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 1.88 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0206] Step 2: Add 34.67 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0207] Embodiment 21

[0208] Li 5.35 La3Zr2Al 0.55 O 12

[0209] The difference between it and embodiment 1 is:

[0210] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.47 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.06 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0211] Step 2: Add 34.36 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0212] Embodiment 22

[0213] Li 5.215 La3Zr2Al 0.595 O 12

[0214] The difference between it and embodiment 1 is:

[0215] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.44 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.23 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0216] Step 2: Add 34.07 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0217] Embodiment 23

[0218] Li 5.2 La3Zr2Al 0.6 O 12

[0219] The difference between it and embodiment 1 is:

[0220] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.43 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.25 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0221] Step 2: Add 34.04 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0222] Embodiment 24

[0223] Li 5.185 La3Zr2Al 0.605 O 12

[0224] The difference between it and embodiment 1 is:

[0225] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.43 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.27 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0226] Step 2: Add 34.01 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0227] Embodiment 25

[0228] Li 5.05 La3Zr2Al 0.65 O 12

[0229] The difference between it and embodiment 1 is:

[0230] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.39 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.44 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0231] Step 2: Add 33.73 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly by magnetic stirring to obtain a second mixed solution.

[0232] Embodiment 26

[0233] Li 4.9 La3Zr2Al 0.7 O 12

[0234] The difference between it and embodiment 1 is:

[0235] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.35 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.63 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0236] Step 2: Add 33.41 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0237] Embodiment 27

[0238] Li 4.75 La3Zr2Al 0.75 O 12

[0239] The difference between it and embodiment 1 is:

[0240] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.31 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 2.81 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0241] Step 2: Add 33.10 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0242] Embodiment 28

[0243] Li 4.6 La3Zr2Al 0.8 O 12

[0244] The difference between it and embodiment 1 is:

[0245] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.27 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 3 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0246] Step 2: Add 32.78 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0247] Embodiment 29

[0248] Li 4.45 La3Zr2Al 0.85 O 12

[0249] The difference between it and embodiment 1 is:

[0250] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.23 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 3.19 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0251] Step 2: Add 32.47 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0252] Embodiment 30

[0253] Li 4.3 La3Zr2Al 0.9 O 12

[0254] The difference between it and embodiment 1 is:

[0255] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.18 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 3.38 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0256] Step 2: Add 32.15 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0257] Embodiment 31

[0258] Li 4.15 La3Zr2Al 0.95 O 12

[0259] The difference between it and embodiment 1 is:

[0260] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.14 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 3.56 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0261] Step 2: Add 31.84 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0262] Embodiment 32

[0263] Li4La3Zr2Al1O 12

[0264] The difference between it and embodiment 1 is:

[0265] Step 1: First add 150 mL of deionized water and 5 mL of concentrated nitric acid into a beaker, add a magnetic bar for magnetic stirring, and then add 1.1 g of LiOH, 9.78 g of La(NO3)3, 6.79 g of Zr(NO3)4, and 3.75 g of Al(NO3)3·9H2O in sequence. After the previous raw material is fully dissolved, add the next raw material to obtain a first mixed solution.

[0266] Step 2: Add 31.52 g of citric acid monohydrate to the first mixed solution obtained in step 1, and mix evenly with magnetic stirring to obtain a second mixed solution.

[0267] The following describes a method for preparing a solid electrolyte and a solid-state battery from the powder material of the present application.

[0268] Solid electrolyte sheet preparation:

[0269] First, the solid electrolyte powder material was ground in an agate mortar for 20 minutes, and 1g of the powder was taken for tableting. The mold diameter was 1 / 2 inch, and a manual press was used for pressurization. The tableting pressure was 300MPa. The tableted electrolyte sheet was heat treated in a box furnace. The heat treatment system was 1150 degrees for 6 hours, the heating rate was 3 degrees per minute, and the cooling stage was furnace cooling. After heat treatment, a densely sintered solid electrolyte sheet was obtained.

[0270] Preparation of button cells:

[0271] Production of button-type lithium symmetric battery: Grind the solid electrolyte sheet to a thickness of 0.3mm. Place a metal lithium sheet with a diameter of 6.5mm, a polished electrolyte sheet, and a metal lithium sheet with a diameter of 6.5mm in the center of the button-type battery shell in sequence, fix and assemble to obtain a sandwich structure Li / LLZO / Li button-type symmetric battery. Before the test, keep the symmetric battery in an oven at 80 degrees for 1 hour, then cool it to room temperature for testing. In this application, the button-type battery is used for performance testing

[0272] Soft pack battery production:

[0273] The solid electrolyte nanopowder is prepared into an acetone slurry and coated on the surface of the diaphragm to obtain an LLZO coated diaphragm. The solid electrolyte nanopowder is mixed evenly with the lithium cobalt oxide positive electrode active material, the conductive agent and the binder in a mass ratio of 10:87:1.5:1.5 to prepare a positive electrode NMP slurry, which is coated on the Al foil and vacuum dried to prepare the positive electrode. Graphite, the conductive agent and the binder are mixed evenly in a mass ratio of 97:1.5:1.5 to prepare a negative electrode aqueous slurry, which is coated on the Cu foil and vacuum dried to prepare the negative electrode. The above-mentioned positive and negative electrode sheets and LLZO coated diaphragms are assembled with commercial electrolytes to form soft-pack batteries.

[0274] The following describes the test methods for various performance parameters of the powder material of the present application.

[0275] Density and ionic conductivity tests:

[0276] According to T / SPSTS019-2021 group standard performance requirements and test methods for solid electrolytes for solid-state lithium batteries.

[0277] Elastic modulus test:

[0278] The fixed pressure load is 20mN, and the hardness tester is used to test the indentation elastic modulus of the solid electrolyte sheet. The calculation formula is E = (1-Vs2) / (1 / Er-(1-Vi2) / Ei), where E is the indentation elastic modulus, Er is the elastic modulus converted by indentation contact, Ei is the elastic modulus of the indenter 1140GPa, Vi is the Poisson's ratio of the indenter 0.07, and the Poisson's ratio of Vs is 0.28. Each sample tests 2 surfaces, a total of 60 points are tested, and 10 samples are selected for Gaussian fitting to obtain the median elastic modulus of the sample.

[0279] Specific heat capacity test:

[0280] The specific heat capacity test was conducted using a differential scanning calorimeter, using the DSC sapphire method, and a Tzero aluminum crucible. Under the same conditions, the sapphire standard was used as a reference sample for measurement, and then the specific heat capacity of the solid electrolyte sample was obtained by calculation from the known specific heat capacity of sapphire. The specific heat capacity test was conducted using the three-stage method of isothermal-heating-isothermal. The specific process is as follows: (a) First, 15±0.5 mg of the sample was weighed, and the sample was isothermalized at the starting temperature for 5 to 10 minutes, with a working atmosphere and flow rate of nitrogen 50 mL / min; (b) Then, the sample was heated from the starting temperature to the ending temperature at a heating rate of 10 K / min; (c) Finally, the sample was isothermalized at the ending temperature for 5 to 10 minutes. The result obtained after the test was a peak-shaped curve of the specific heat capacity changing with temperature. The peak value was taken to obtain the mass specific heat capacity peak value of the corresponding sample.

[0281] Median particle size test:

[0282] The determination method is carried out in accordance with the relevant provisions of GB / T19077 particle size analysis laser diffraction method.

[0283] Specific surface area test:

[0284] The determination method is carried out in accordance with the relevant provisions of GB / T19587 gas adsorption BET method for determining the specific surface area of ​​solid substances.

[0285] Tap density test:

[0286] The determination method is carried out in accordance with the relevant provisions of GB / T5162 Determination of the tap density of metal powders.

[0287] Test of initial voltage and critical current density:

[0288] LAND was used to test the initial voltage and critical current density of button-type lithium symmetric cells. The charge and discharge current density used for the symmetric cell was 1 mA / cm 2 The duration of one charge and discharge cycle is 1h. The critical current density is 1, 1.5, 2, 2.5...10mA / cm 2 The charge and discharge were carried out for 10 h at each current density.

[0289] The magnitude of the initial voltage is related to the interface resistance and the resistance of the solid electrolyte. Under the same interface conditions, the greater the ionic conductivity of the solid electrolyte, the smaller the corresponding impedance and the smaller the initial voltage. The critical current density is defined as the maximum current density of a symmetrical battery without short circuit. The larger the value, the stronger the battery's ability to resist lithium dendrite penetration. Under the same interface conditions, the solid electrolyte with a high elastic modulus has a stronger ability to inhibit lithium dendrites.

[0290] Soft pack battery hot box test:

[0291] The hot box test is carried out using a programmed hot and cold cycle temperature shock box. The soft pack battery is 100% SOC and the test temperature is 140 degrees for 30 minutes. A thermocouple is connected to the battery surface for temperature monitoring, and a temperature data is recorded every second. The temperature change of the battery sample from the beginning of heating to the end of the test can be recorded. The rest of the relevant measurement requirements are carried out in accordance with the relevant provisions of GB31241-2022 Safety Technical Specifications for Lithium-ion Batteries and Battery Packs for Portable Electronic Products.

[0292] Relevant tests were performed on the powder materials of Example 1 to Example 47, and the test results are shown in Table 1 to Table 4.

[0293] Table 1

[0294]

[0295]

[0296]

[0297] Table 2

[0298]

[0299]

[0300] Table 3

[0301]

[0302]

[0303] Table 4

[0304]

[0305]

[0306] The powder material and preparation method thereof provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of ​​the present application. At the same time, for technicians in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A powder material suitable for constituting a solid electrolyte in a battery, characterized in that: The chemical formula of the powder material is Li 7-3x La3Zr2Al x O 12 , where the value range of X is: 0.305 to 0.

65.

2. The powder material according to claim 1, characterized in that: The value range of X is: 0.305 to 0.345, or 0.355 to 0.

595.

3. The powder material according to claim 1, characterized in that: The ratio of the mass specific heat capacity peak value to the ionic conductivity of the powder material ranges from 2100 to 15000.

4. The powder material according to claim 1, characterized in that: The ratio of the elastic modulus of the powder material to the ionic conductivity of the powder material ranges from 66 to 430.

5. A method for preparing a powder material, characterized in that: The steps include: Mixing the precursors of the components in the powder material to obtain a first mixed solution; adding a complexing agent to the first mixed solution to obtain a second mixed solution; freeze-drying the second mixed solution to obtain a first powder material; Grinding the first powder material to obtain a second powder material; heat-treating the second powder material to obtain a third powder material; Grinding the third powder material to obtain a fourth powder material; Drying the fourth powder material to obtain the powder material; Wherein, the chemical formula of the powder material is Li 7-3x La3Zr2Al x O 12 , where the value range of X is: 0.305 to 0.

65.

6. The preparation method according to claim 5, characterized in that: The first mixed solution includes: LiOH, La(NO3)3, Zr(NO3)4 and Al(NO3)3·9H2O.

7. The preparation method according to claim 5, characterized in that: The complexing agent is one or more of malic acid, citric acid, malonic acid, succinic acid, succinic acid, lactic acid, and ethylenediaminetetraacetic acid.

8. The preparation method according to claim 5, characterized in that: The insulation temperature of the heat treatment ranges from 600° C. to 1200° C.; the protection time of the heat treatment ranges from 4 h to 15 h.

9. A battery, characterized in that: A solid electrolyte comprising the powder material according to any one of claims 1 to 4 or the powder material prepared by the preparation method according to any one of claims 5 to 8.