A fire-retardant powder coating with anti-static effect and preparation method thereof

By modifying graphene oxide and nano-silica, and combining specific chemical reagents and processes, powder coatings with antistatic and fire-retardant properties were prepared, solving the problem of insufficient antistatic and fire-retardant properties of existing powder coatings and achieving higher safety and applicability.

CN118185433BActive Publication Date: 2024-10-11HEBEI XINFURUI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410419782.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-10-11
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

Existing powder coatings are insufficient in terms of antistatic and fire-retardant properties, and cannot meet the requirements of high-temperature baking and static electricity accumulation, resulting in insufficient equipment safety.

Method used

By modifying graphene oxide and nano-silica, and combining them with specific chemical reagents and processes, modified fillers are prepared and mixed with polyester resin, epoxy resin, etc., to form powder coatings with antistatic and fire-retardant properties.

Benefits of technology

It achieves excellent antistatic and fire-retardant properties of powder coatings, improves the strength and toughness of coatings, reduces surface resistivity, enhances the wear resistance and fire insulation capabilities of coatings, and expands the application range of powder coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118185433B_ABST
    Figure CN118185433B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and specifically discloses a fireproof powder coating with antistatic effect and a preparation method thereof. Raw materials include polyester resin, epoxy resin, modified filler, curing agent, defoaming agent, antioxidant, dispersant and leveling agent. The raw materials are mixed, melt-blended and extruded to obtain the fireproof powder coating with antistatic effect. The modified filler includes modified graphene and flame-retardant modified silica, has a stable chemical structure, can improve the density of the carbon layer during the combustion process, has excellent fireproof performance, is uniformly dispersed in a matrix to form a network structure, forms a conductive network path between dispersed particles, reduces resistance, and promotes the dissipation of static charge. At the same time, the raw materials have excellent compatibility, and the obtained powder coating has excellent antistatic and fireproof performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a fireproof powder coating with antistatic effect and a preparation method thereof. Background Art

[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. Different from ordinary solvent-based coating and water-based coating, powder coating is completely solid powder, using air as dispersion medium, with no solvent pollution, 100% film formation, low energy consumption, and excellent physical and chemical properties. Powder coating has two categories: thermoplastic and thermosetting. Thermosetting powder coating uses thermosetting synthetic resin as film-forming material. During the drying process, the resin first melts and then solidifies into a smooth and hard coating film after chemical cross-linking. Powder coating is widely used in the electrical industry, shipbuilding industry, automotive industry, etc., and has received more and more attention.

[0003] Thermosetting powder coatings include epoxy resins, epoxy-polyesters, polyesters, polyurethanes, acrylic resins, etc. Due to the flammability of resins, conventional powder coatings do not have flame retardancy, and the high temperature baking time is short. For the situation where there is a requirement for heat insulation and non-flammability, conventional powder coatings cannot meet the requirements. In addition, the coatings formed by powder coatings mostly cannot play an excellent antistatic role, and are often subject to friction with dust in gas or air to produce static electricity accumulation. As static electricity accumulates to a certain extent, it causes static electricity discharge, further destroys the equipment, and causes fire or explosion accidents. Therefore, improving the fire retardancy and antistatic properties of powder coatings can greatly expand the scope of application and safety performance of powder coatings. Chinese patent application CN112280434A discloses a novel fire-retardant powder coating, which improves the flame retardancy and fire retardancy of the coating by adding graphene oxide, cross-linking and compounding with resin, using polyvinyl alcohol as a carbon forming agent, ammonium dihydrogen phosphate as a catalyst, and melamine as a foaming agent to obtain a specific expansive flame retardant, and graphene oxide and expansive flame retardant synergistically enhance the fire retardancy of the coating. However, the dispersion of the flame retardant components of the powder coating is poor, which greatly affects the fire resistance, and the antistatic performance is average. Chinese patent application CN107760164A discloses a graphene conductive powder coating, which can be used for conductive treatment of wood products before spraying. Graphene is used to improve the water resistance, barrier properties and hardness of the coating. After the wood products are treated and dried and cured, a smooth and dense conductive coating can be formed on their surface. However, the graphene used in the powder coating has few surface functional groups and has certain problems in dispersion. The addition of graphene to a dispersant for ultrasonic treatment to form a graphene slurry is not conducive to the actual production of powder coatings, and the fire resistance is average.

[0004] Therefore, it is necessary to provide a powder coating with excellent antistatic effect and good fire resistance. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a fire-retardant powder coating with anti-static effect and a preparation method thereof, which solves the problem that the powder coating has poor anti-static and fire-retardant properties.

[0007] (II) Technical solution

[0008] In order to achieve the above object, the present invention discloses a method for preparing a fire-retardant powder coating with antistatic effect, comprising the following steps:

[0009] Step 1: adding graphene oxide (GO) and thionyl chloride into reactor A, performing ultrasonic dispersion, reacting, filtering after the reaction, washing with tetrahydrofuran, and vacuum drying at 60° C. for 12 h to obtain chlorinated graphene;

[0010] Step 2: Add N,N-dimethylformamide, chlorinated graphene and lysine into reactor B, stir and mix, react, and after the reaction is completed, filter, wash with acetone, and vacuum dry at 60° C. for 12 h to obtain modified graphene;

[0011] Step 3: Add nano-silica and anhydrous ethanol to reactor C, perform ultrasonic dispersion, introduce nitrogen, and then add γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere to react. After the reaction, filter, wash with deionized water, and vacuum dry at 60° C. for 12 h to obtain epoxidized silica;

[0012] Step 4: Add epoxidized silicon dioxide and a mixed solvent into a reactor D, and after ultrasonic dispersion, add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine (C 16 H 15 N6O2P), stirring and mixing evenly to react, and after the reaction is completed, rotary evaporation to obtain flame retardant modified silicon dioxide;

[0013] Step 5: Add dichloromethane, modified graphene, flame-retardant modified silica, and triethylamine to reactor E, mix well, react for 3-5 hours in an ice bath at -5°C, and after the reaction, perform rotary evaporation. After rotary evaporation, wash with deionized water and saturated brine, filter, and vacuum dry at 60°C for 12 hours to obtain a modified filler;

[0014] Step six: Add polyester resin, epoxy resin, modified filler, curing agent, defoamer, antioxidant, dispersant and leveling agent into a high-speed mixer, mix at 70-80°C for 1-2 hours, and after cooling, transfer to a twin-screw extruder for melt blending, extrusion, tableting, crushing and sieving to obtain a fire-retardant powder coating with antistatic effect.

[0015] Preferably, in step 1, the mass ratio of graphene oxide to thionyl chloride is 100:25000-28000.

[0016] Preferably, the reaction temperature in step 1 is 65-75° C., and the reaction time is 15-18 h.

[0017] Preferably, in the step 2, the mass ratio of N,N-dimethylformamide, graphene chloride and lysine is 5000-5500:100:62-75.

[0018] Preferably, the reaction temperature in step 2 is 85-95° C., and the reaction time is 18-24 h.

[0019] Preferably, in step three, the mass ratio of nano-silica, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane is 100:2000-2400:55-62.

[0020] Preferably, the reaction temperature in step 3 is 65-75° C., and the reaction time is 18-22 h.

[0021] Preferably, the mixed solvent in step 4 consists of acetone and toluene in a volume ratio of 1:2.

[0022] Preferably, in the step 4, the mass ratio of epoxidized silicon dioxide, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine is 100:1500-1600:78-90.

[0023] Preferably, the reaction temperature in step 4 is 100-110° C., and the reaction time is 6-8 h.

[0024] Preferably, in the step 5, the mass ratio of dichloromethane, modified graphene, flame retardant modified silica and triethylamine is 900-1200:100:85-105:21-32.

[0025] Preferably, the mesh size of the sieve used in step six is ​​180 meshes.

[0026] Preferably, in step six, the mass ratio of polyester resin, epoxy resin, modified filler, curing agent, defoaming agent, antioxidant, dispersant and leveling agent is 100:12-15:6-10:1-3:0.3-0.8:1-1.5:0.8-1.2:0.5-1.

[0027] Preferably, the curing agent in step six includes one or more of TGIC curing agent, T105 curing agent, and sebacic acid dihydrazide.

[0028] Preferably, the defoaming agent in step six includes one or more of benzoin, polyoxyethylene polyoxypropanolamine ether defoaming agent, and polyethylene wax.

[0029] Preferably, the antioxidant in step six includes one or more of antioxidant 618 , antioxidant 1010 , and antioxidant 168 .

[0030] Preferably, the dispersant in step six includes one or more of BYK110 dispersant, dispersant NC, and microcrystalline wax.

[0031] Preferably, the leveling agent in step six includes one or more of leveling agent GLP588, organic modified polysiloxane, and polyester modified polyether.

[0032] Preferably, during the melt blending process in step six, the process parameters are: the temperature of zone 1 of melt blending is 105-125°C, the temperature of zone 2 of melt blending is 130-150°C, the temperature of zone 3 of melt blending is 120-145°C, the temperature of zone 4 of melt blending is 125-135°C, and the speed of the main engine is 1800-2500r / min.

[0033] Preferably, the fire retardant powder coating with antistatic effect is prepared by the method for preparing the fire retardant powder coating with antistatic effect.

[0034] (III) Beneficial technical effects

[0035] (1) In the present invention, thionyl chloride is used to modify graphene oxide, and acyl chloride is introduced on the surface of graphene oxide to obtain acyl chloride graphene. The acyl chloride groups on the surface of acyl chloride graphene react with the amino groups on lysine to introduce amide bonds and carboxyl groups to obtain modified graphene. γ-glycidyloxypropyltrimethoxysilane is used to modify nano-silica to obtain epoxidized silica. The epoxy groups on the epoxidized silica react with N-[(10-oxo-9,10-dihydro-9 The amino group on the flame-retardant modified silica reacts with the modified graphene to introduce an amide bond, thereby obtaining a modified filler. The modified filler is mixed with a polyester resin, an epoxy resin, a modified filler, a curing agent, a defoaming agent, an antioxidant, a dispersant, and a leveling agent, and then melt-blended and extruded to obtain a fire-retardant powder coating with an antistatic effect.

[0036] (2) The nano silicon dioxide and graphene oxide in the present invention have excellent mechanical properties, which can effectively improve the mechanical properties of the powder coating. The prepared powder coating has good strength and toughness, and the chemical structure is stable and not easy to be damaged. It also has the characteristics of wear resistance. The nano silicon dioxide and graphene oxide are modified to effectively avoid the agglomeration of nano silicon dioxide and graphene oxide. The modified filler and the introduction of silicon element can both improve the density of the carbon layer during the combustion process. At the same time, the organic flame retardant introduced has excellent flame retardant properties. The nitrogen contained in the present invention generates non-flammable gas during the combustion process, which reduces the concentration of oxygen in the combustion environment and greatly slows down the rate of the combustion reaction. The phosphorus element can generate acid substances such as phosphoric acid and phosphorous acid during the combustion process, promote the dehydration and carbonization of the matrix during the combustion process, prevent the conduction of heat, accelerate the formation of the carbon layer, and the generated PO· free radicals can capture ·OH and H· free radicals in the flame, interrupt the combustion chain reaction, reduce the heat released by the combustion, and further prevent the continuation of the combustion reaction. It has excellent fireproof properties.

[0037] (3) The modified filler in the present invention can be evenly dispersed in the matrix to form a network structure, forming a conductive network path between the dispersed particles. When the powder coating is sprayed, a conductive layer can be formed on the surface of the object, which reduces the resistance, promotes the dissipation of static charge, and has excellent antistatic performance. A large number of amide bonds introduced during the reaction process have excellent antistatic performance and are easy to form an adsorption layer, which effectively avoids the generation of static electricity. At the same time, after the surface dispersion treatment, the modified filler not only utilizes the solid electronic conductivity of the nanometer to evacuate the charge and resist static electricity, but also utilizes the hydrophilicity of the nanometer hydrophilic group on the surface of the matrix to conduct ion conduction to evacuate the charge, thereby reducing the surface resistivity and further improving the antistatic ability of the matrix.

[0038] (4) The epoxy resin in the present invention has more hydroxyl groups and ether bonds, and has low curing shrinkage, good corrosion resistance, good stability and good resistance. Introducing epoxy resin into polyester resin will effectively improve the disadvantage of poor water resistance of polyester resin, and improve the storage stability of water-based polyester coating and its paint film resistance. At the same time, the amide bond and amino group introduced into the modified filler can form hydrogen bonds with hydroxyl groups, effectively improving the compatibility between raw materials, and the obtained powder coating has excellent antistatic and fire retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0040] Figure 1 It is a schematic diagram of the structure of preparing modified graphene in the present invention;

[0041] Figure 2 This is a schematic diagram of the structure of the flame retardant modified silica prepared in the present invention;

[0042] Figure 3 It is a schematic diagram of the structure of preparing the modified filler in the present invention. DETAILED DESCRIPTION

[0043] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0044] Example 1

[0045] A method for preparing a fire-retardant powder coating with antistatic effect comprises the following steps:

[0046] Step 1, ultrasonically disperse and mix graphene oxide and thionyl chloride in a mass ratio of 100:25000, react at 65° C. for 18 hours, and after the reaction, filter, wash with tetrahydrofuran, and vacuum dry at 60° C. for 12 hours to obtain graphene chloride;

[0047] Step 2: N,N-dimethylformamide, chlorinated graphene and lysine in a mass ratio of 5000:100:62 were stirred and mixed, and reacted at 85°C for 24 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and vacuum dried at 60°C for 12 hours to obtain modified graphene;

[0048] Step 3: Ultrasonically disperse and mix the nano-silica and anhydrous ethanol, introduce nitrogen, and then add γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere, wherein the mass ratio of the added nano-silica, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane is 100:2000:55, and react at a temperature of 65° C. for 22 hours. After the reaction, filter, wash with deionized water, and vacuum dry at 60° C. for 12 hours to obtain epoxidized silica;

[0049] Step 4, ultrasonically disperse the epoxidized silica and the mixed solvent, wherein the mixed solvent consists of acetone and toluene in a volume ratio of 1:2, and then add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, wherein the added epoxidized silica, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine have a mass ratio of 100:1500:78, stir and mix evenly, react at 100°C for 8h, and after the reaction is completed, rotary evaporate to obtain flame retardant modified silica;

[0050] Step 5: Evenly mix dichloromethane, modified graphene, flame-retardant modified silica, and triethylamine in a mass ratio of 900:100:85:21, react for 3 hours in an ice bath at -5°C, and after the reaction, perform rotary evaporation. After rotary evaporation, wash with deionized water and saturated brine, filter, and vacuum dry at 60°C for 12 hours to obtain a modified filler;

[0051] Step six, add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:12:6:1:0.3:1:0.8:0.5 to a high-speed mixer, mix at 70°C for 2h, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of the first zone of melt blending is 105°C, the temperature of the second zone of melt blending is 130°C, the temperature of the third zone of melt blending is 120°C, the temperature of the fourth zone of melt blending is 125°C, the speed of the main engine is 1800r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a fire retardant powder coating with antistatic effect is obtained.

[0052] Example 2

[0053] A method for preparing a fire-retardant powder coating with antistatic effect comprises the following steps:

[0054] Step 1, mixing graphene oxide and thionyl chloride in a mass ratio of 100:26000 by ultrasonic dispersion, reacting at 70° C. for 16 hours, filtering after the reaction, washing with tetrahydrofuran, and vacuum drying at 60° C. for 12 hours to obtain graphene chloride;

[0055] Step 2: N,N-dimethylformamide, chlorinated graphene and lysine in a mass ratio of 5200:100:68 were stirred and mixed, and reacted at 90° C. for 20 h. After the reaction was completed, the mixture was filtered, washed with acetone, and vacuum dried at 60° C. for 12 h to obtain modified graphene;

[0056] Step 3: Ultrasonically disperse and mix the nano-silica and anhydrous ethanol, introduce nitrogen, and then add γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere, wherein the mass ratio of the added nano-silica, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane is 100:2100:58, and react at a temperature of 70° C. for 20 hours. After the reaction, filter, wash with deionized water, and vacuum dry at 60° C. for 12 hours to obtain epoxidized silica;

[0057] Step 4, ultrasonically disperse the epoxidized silica and the mixed solvent uniformly, wherein the mixed solvent consists of acetone and toluene in a volume ratio of 1:2, and then add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, wherein the added epoxidized silica, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine have a mass ratio of 100:1540:82, stir and mix uniformly, react at 105°C for 7h, and after the reaction is completed, rotary evaporate to obtain flame retardant modified silica;

[0058] Step 5: Evenly mix dichloromethane, modified graphene, flame-retardant modified silica, and triethylamine in a mass ratio of 1000:100:92:25, react for 4 hours in an ice bath at -5°C, and after the reaction, perform rotary evaporation. After rotary evaporation, wash with deionized water and saturated brine, filter, and vacuum dry at 60°C for 12 hours to obtain a modified filler;

[0059] Step six, add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:14:8:2:0.6:1.2:1:0.8 to a high-speed mixer, mix at 75°C for 1.5 hours, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of the first zone of melt blending is 115°C, the temperature of the second zone of melt blending is 140°C, the temperature of the third zone of melt blending is 135°C, the temperature of the fourth zone of melt blending is 130°C, the speed of the main engine is 2100r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a fire retardant powder coating with antistatic effect is obtained.

[0060] Example 3

[0061] A method for preparing a fire-retardant powder coating with antistatic effect comprises the following steps:

[0062] Step 1, ultrasonically disperse and mix graphene oxide and thionyl chloride in a mass ratio of 100:27000, react at 70°C for 17 hours, and after the reaction, filter, wash with tetrahydrofuran, and vacuum dry at 60°C for 12 hours to obtain graphene chloride;

[0063] Step 2: N,N-dimethylformamide, chlorinated graphene and lysine in a mass ratio of 5400:100:72 were stirred and mixed, and reacted at 90° C. for 22 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and vacuum dried at 60° C. for 12 hours to obtain modified graphene;

[0064] Step 3: Ultrasonic disperse and mix the nano-silica and anhydrous ethanol evenly, introduce nitrogen, and then add γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere, wherein the mass ratio of the added nano-silica, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane is 100:2300:60, and react at a temperature of 70° C. for 21 hours. After the reaction, filter, wash with deionized water, and vacuum dry at 60° C. for 12 hours to obtain epoxidized silica;

[0065] Step 4, ultrasonically disperse the epoxidized silica and the mixed solvent uniformly, wherein the mixed solvent consists of acetone and toluene in a volume ratio of 1:2, and then add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, wherein the added epoxidized silica, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine have a mass ratio of 100:1580:86, stir and mix uniformly, react at 105°C for 7h, and after the reaction is completed, rotary evaporate to obtain flame retardant modified silica;

[0066] Step 5: Evenly mix dichloromethane, modified graphene, flame-retardant modified silica, and triethylamine in a mass ratio of 1100:100:100:30, react for 4 hours in an ice bath at -5°C, and after the reaction, perform rotary evaporation. After rotary evaporation, wash with deionized water and saturated brine, filter, and vacuum dry at 60°C for 12 hours to obtain a modified filler;

[0067] Step six, add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:14:8:2:0.6:1.2:1:0.8 to a high-speed mixer, mix at 75°C for 1.5 hours, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of the first zone of melt blending is 115°C, the temperature of the second zone of melt blending is 140°C, the temperature of the third zone of melt blending is 135°C, the temperature of the fourth zone of melt blending is 130°C, the speed of the main engine is 2100r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a fire retardant powder coating with antistatic effect is obtained.

[0068] Example 4

[0069] A method for preparing a fire-retardant powder coating with antistatic effect comprises the following steps:

[0070] Step 1, ultrasonically disperse and mix graphene oxide and thionyl chloride in a mass ratio of 100:28000, react at 75°C for 15 hours, and after the reaction, filter, wash with tetrahydrofuran, and vacuum dry at 60°C for 12 hours to obtain graphene chloride;

[0071] Step 2: N,N-dimethylformamide, chlorinated graphene and lysine in a mass ratio of 5500:100:75 were stirred and mixed, and reacted at 95° C. for 18 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and vacuum dried at 60° C. for 12 hours to obtain modified graphene;

[0072] Step 3: Ultrasonically disperse and mix the nano-silica and anhydrous ethanol, introduce nitrogen, and then add γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere. The mass ratio of the added nano-silica, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane is 100:2400:62. React at a temperature of 75° C. for 18 hours. After the reaction, filter, wash with deionized water, and vacuum dry at 60° C. for 12 hours to obtain epoxidized silica;

[0073] Step 4, ultrasonically disperse the epoxidized silica and the mixed solvent uniformly, wherein the mixed solvent consists of acetone and toluene in a volume ratio of 1:2, and then add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, wherein the mass ratio of the added epoxidized silica, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine is 100:1600:90, stir and mix uniformly, react at 110°C for 6h, and after the reaction is completed, rotary evaporate to obtain flame retardant modified silica;

[0074] Step 5: Evenly mix dichloromethane, modified graphene, flame-retardant modified silica, and triethylamine in a mass ratio of 1200:100:105:32, react for 5 hours in an ice bath at -5°C, and after the reaction, perform rotary evaporation. After rotary evaporation, wash with deionized water and saturated brine, filter, and vacuum dry at 60°C for 12 hours to obtain a modified filler;

[0075] Step six, add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:15:10:3:0.8:1.5:1.2:1 to a high-speed mixer, mix at 80°C for 1h, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of the first zone of melt blending is 125°C, the temperature of the second zone of melt blending is 150°C, the temperature of the third zone of melt blending is 145°C, the temperature of the fourth zone of melt blending is 135°C, the speed of the main engine is 2500r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a fire retardant powder coating with antistatic effect is obtained.

[0076] Comparative Example 1

[0077] A method for preparing a powder coating comprises the following steps:

[0078] Step 1, ultrasonically disperse and mix graphene oxide and thionyl chloride in a mass ratio of 100:27000, react at 70°C for 17 hours, and after the reaction, filter, wash with tetrahydrofuran, and vacuum dry at 60°C for 12 hours to obtain graphene chloride;

[0079] Step 2: N,N-dimethylformamide, chlorinated graphene and lysine in a mass ratio of 5400:100:72 were stirred and mixed, and reacted at 90° C. for 22 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and vacuum dried at 60° C. for 12 hours to obtain modified graphene;

[0080] Step 3, the mass ratio of 1100:100:54:46:30 of dichloromethane, modified graphene, nano-silica, N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine and triethylamine was mixed evenly, and the mixture was reacted in an ice bath at -5°C for 4 hours. After the reaction was completed, the mixture was rotary evaporated, and after the rotary evaporation, the mixture was washed with deionized water and saturated brine. After washing, the mixture was filtered and vacuum dried at 60°C for 12 hours to obtain a modified filler;

[0081] Step 4: Add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:14:8:2:0.6:1.2:1:0.8 to a high-speed mixer, mix at 75°C for 1.5 hours, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of zone 1 of melt blending is 115°C, the temperature of zone 2 of melt blending is 140°C, the temperature of zone 3 of melt blending is 135°C, the temperature of zone 4 of melt blending is 130°C, the speed of the main engine is 2100r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a powder coating is obtained.

[0082] Comparative Example 2

[0083] A method for preparing a powder coating comprises the following steps:

[0084] Step 1: Ultrasonically disperse and mix nano-silica and anhydrous ethanol, introduce nitrogen, and then add γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere, wherein the mass ratio of the added nano-silica, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane is 100:2300:60, and react at a temperature of 70° C. for 21 hours. After the reaction, filter, wash with deionized water, and vacuum dry at 60° C. for 12 hours to obtain epoxidized silica;

[0085] Step 2, ultrasonically disperse the epoxidized silica and the mixed solvent uniformly, wherein the mixed solvent consists of acetone and toluene in a volume ratio of 1:2, and then add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, wherein the added epoxidized silica, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine have a mass ratio of 100:1580:86, stir and mix uniformly, react at 105°C for 7h, and after the reaction is completed, rotary evaporate to obtain flame retardant modified silica;

[0086] Step 3, mix dichloromethane, graphene oxide, flame retardant modified silica, and triethylamine in a mass ratio of 1100:100:100:30, react for 4 hours in an ice bath at -5°C, and after the reaction, perform rotary evaporation. After rotary evaporation, wash with deionized water and saturated brine, filter, and vacuum dry at 60°C for 12 hours to obtain a modified filler;

[0087] Step six, add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:14:8:2:0.6:1.2:1:0.8 to a high-speed mixer, mix at 75°C for 1.5 hours, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of the first zone of melt blending is 115°C, the temperature of the second zone of melt blending is 140°C, the temperature of the third zone of melt blending is 135°C, the temperature of the fourth zone of melt blending is 130°C, the speed of the main engine is 2100r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a powder coating is obtained.

[0088] Comparative Example 3

[0089] A method for preparing a powder coating comprises the following steps:

[0090] Step 1, mixing dichloromethane, graphene oxide, nano-silica, N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine and triethylamine in a mass ratio of 1100:100:54:46:30, reacting for 4 hours in an ice bath at -5°C, rotary evaporation after the reaction, washing with deionized water and saturated brine, filtering, and vacuum drying at 60°C for 12 hours to obtain a modified filler;

[0091] Step 2: Add polyester resin, epoxy resin, modified filler, TGIC curing agent, defoamer benzoin, antioxidant 618, BYK110 dispersant, and leveling agent GLP588 in a mass ratio of 100:14:8:2:0.6:1.2:1:0.8 to a high-speed mixer, mix at 75°C for 1.5 hours, and after cooling, transfer to a twin-screw extruder for melt blending. During the melt blending process, the process parameters are: the temperature of the first zone of melt blending is 115°C, the temperature of the second zone of melt blending is 140°C, the temperature of the third zone of melt blending is 135°C, the temperature of the fourth zone of melt blending is 130°C, the speed of the main engine is 2100r / min, extrusion, tableting, crushing, sieving, the mesh number of the sieve is 180 mesh, and a powder coating is obtained.

[0092] The graphene oxide used in the embodiments and comparative examples of the present invention was purchased from Hangzhou Zhitai Purification Technology Co., Ltd., with an average thickness of 0.5-1.2 nm and a diameter of 4-7 μm; nano-silicon dioxide was purchased from Jiangsu Tianxing New Materials Co., Ltd., with the item number TSP-H10 and an average particle size of 20 nm; the polyester resin was purchased from Guangzhou Qingtian Materials Technology Co., Ltd., which is polyester resin NH3307, industrial grade; the epoxy resin was purchased from Yueyang Baling Petrochemical Chemical Company, which is epoxy resin 014U, E-12 type, industrial grade; the TGIC curing agent was purchased from Yangzhou Youyi New Materials Co., Ltd.; the leveling agent GLP588 was purchased from Ningbo Nanhai Chemical Co., Ltd.; benzoin was purchased from Wuhan Yincai Technology Co., Ltd.; other materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.

[0093] The powder coatings prepared in Examples 1-4 and Comparative Examples 1-3 were used as samples for performance tests, and the relevant tests were as follows:

[0094] (1) Antistatic performance test: The powder coatings prepared in Examples 1-4 and the powder coatings prepared in Comparative Examples 1-3 were tested for antistatic performance in accordance with SJ / T 10694-2006. The results are shown in Table 1:

[0095] Table 1

[0096]

[0097] From the data analysis of Table 1, it can be seen that in Comparative Examples 1 and 2, a single component of the filler is modified, and the other filler components are not modified. When added to the matrix to prepare the powder coating, the antistatic performance is reduced, because the dispersibility between the raw materials is deteriorated, the compatibility is greatly reduced, and the synergistic effect between the two is reduced. The powder coatings prepared in Examples 1-4 have excellent antistatic performance, which fully illustrates the synergistic effect between the raw materials. In Comparative Example 3, graphene oxide and nano-silicon dioxide are not modified, and the modified filler is added to the matrix, and the resistance reaches 3.1×10 5 , the anti-static performance is greatly reduced.

[0098] (2) Fire resistance test: The ultra-thin steel structure fire retardant coating test device is used to test the fire resistance limit of the workpiece coated with powder coating. The test fire scene type is cellulose fire scene. The equipment is implemented in accordance with GB / T 9978 and uses Q235 steel plate with a size of 42×821.7mm. 3 , record the fire resistance limit time, test each group three times, take the average value, the test results are shown in Table 2:

[0099] Table 2

[0100]

[0101] From the data analysis of Table 1, it can be seen that the powder coating prepared in the embodiment has excellent fire resistance, forms a dense carbon layer at high temperature, can effectively improve the fire resistance limit, and has excellent fireproof and heat insulation properties. The organic flame retardant in Comparative Examples 1 and 3 has poor dispersibility, which further reduces the fire resistance of the powder coating. The fire resistance limit of the sample corresponding to Comparative Example 1 is 35.6 min, and the fire resistance limit of the sample corresponding to Comparative Example 3 is 30.5 min.

[0102] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a fire-retardant powder coating having an antistatic effect, characterized in that: The steps include: Step 1: adding graphene oxide and thionyl chloride into reactor A, performing ultrasonic dispersion, reacting, and after the reaction is completed, filtering, washing, and vacuum drying to obtain graphene chloride; Step 2: Add N,N-dimethylformamide, chlorinated graphene and lysine into reactor B, stir and mix, react, and after the reaction is completed, filter, wash and dry to obtain modified graphene; Step 3, adding nano-silica and anhydrous ethanol into reactor C, ultrasonically dispersing, introducing nitrogen, and then adding γ-glycidyloxypropyltrimethoxysilane in a nitrogen atmosphere to react, and after the reaction, filtering, washing, and drying to obtain epoxidized silica; Step 4: Add the epoxidized silica and the mixed solvent into the reactor D, and after ultrasonic dispersion, add N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine, stir and mix evenly, react, and after the reaction is completed, rotary evaporate to obtain flame-retardant modified silica; Step 5: adding dichloromethane, modified graphene, flame-retardant modified silica and triethylamine into reactor E, mixing evenly, reacting for 3-5 hours in an ice bath at -5°C, and after the reaction, rotary evaporation, washing, filtering and drying to obtain a modified filler; Step six: Add polyester resin, epoxy resin, modified filler, curing agent, defoamer, antioxidant, dispersant and leveling agent into a high-speed mixer, mix at 70-80°C for 1-2 hours, and after cooling, transfer to a twin-screw extruder for melt blending, extrusion, tableting, crushing and sieving to obtain a fire-retardant powder coating with antistatic effect.

2. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: In the step 2, the mass ratio of N,N-dimethylformamide, graphene chloride and lysine is 5000-5500:100:62-75, the reaction temperature is 85-95° C., and the reaction time is 18-24 hours.

3. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: In the step 4, the mixed solvent consists of acetone and toluene in a volume ratio of 1:

2.

4. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: In the step 4, the mass ratio of epoxidized silicon dioxide, the mixed solvent and N-[(10-oxo-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-yl)methyl]-1,3,5-triazine-2,4,6-triamine is 100:1500-1600:78-90, the reaction temperature is 100-110°C, and the reaction time is 6-8h.

5. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: In the step 5, the mass ratio of dichloromethane, modified graphene, flame retardant modified silica and triethylamine is 900-1200:100:85-105:21-32.

6. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: The mesh size of the sieve screened in step 6 is 180 meshes.

7. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: In the step six, the mass ratio of the polyester resin, the epoxy resin, the modified filler, the curing agent, the defoaming agent, the antioxidant, the dispersant and the leveling agent is 100:12-15:6-10:1-3:0.3-0.8:1-1.5:0.8-1.2:0.5-1.

8. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: During the melt blending process in step 6, the process parameters are: the temperature of the first zone of melt blending is 105-125°C, the temperature of the second zone of melt blending is 130-150°C, the temperature of the third zone of melt blending is 120-145°C, the temperature of the fourth zone of melt blending is 125-135°C, and the speed of the main engine is 1800-2500r / min.

9. The method for preparing a fire-retardant powder coating with antistatic effect according to claim 1, characterized in that: The curing agent in step 6 includes one or more of TGIC curing agent, T105 curing agent, and sebacic acid dihydrazide; The defoaming agent in step 6 includes one or more of benzoin, polyoxyethylene polyoxypropanolamine ether defoaming agent, and polyethylene wax; The antioxidant in step 6 includes one or more of antioxidant 618, antioxidant 1010, and antioxidant 168; The dispersant in step 6 includes one or more of BYK110 dispersant, dispersant NC, and microcrystalline wax; The leveling agent in step six includes one or more of the leveling agent GLP588, organic modified polysiloxane, and polyester modified polyether.

10. A fire retardant powder coating with antistatic efficacy prepared by the method for preparing a fire retardant powder coating with antistatic efficacy according to any one of claims 1 to 9.