A process for preparing rubber adhesive by using resorcinol-formaldehyde modification
Hexamethylene diisocyanate and aluminum hydroxide were added by using a styrene-divinylbenzene copolymer resin catalyst and microwave heating in the preparation of resorcinol-formaldehyde resin, combined with vacuum suction filtration and freeze-drying dehydration treatment, using hexamethylene diisocyanate and aluminum hydroxide. Glass fiber and diatomaceous earth fillers solve the safety risks and insufficient performance problems of the prior art resorcinol-formaldehyde resin, and realize rubber adhesives with high dispersion, thermal stability and mechanical properties.
Patent Information
- Application Number
- CN202410452144.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-04-16
AI Technical Summary
When preparing rubber adhesives, the existing resorcinol-formaldehyde resins have high moisture content, easy resorcinol and many by-products, resulting in safety risks, poor adhesion and durability and poor thermal stability. , and not environmentally friendly enough.
Using styrene-divinylbenzene copolymer resin as catalyst, the formaldehyde addition rate is controlled by microwave heating and controlling, combined with vacuum suction filtration and freeze-drying dehydration treatment, further adding hexamethylene diisocyanate, butyl hydroxyanisole and hydroxide Aluminum, using glass fiber and diatomaceous earth as fillers, forms a modified resorcinol-formaldehyde resin, improving reaction selectivity and adhesive properties.
It significantly improves the dispersion, thermal stability, mechanical properties and oxidation resistance of rubber adhesives, reduces the generation of by-products, enhances the adhesiveness and wear resistance, and meets the use requirements.
Smart Images

Figure CN118185529B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesive preparation, and specifically relates to a process for preparing a rubber adhesive by utilizing resorcinol-formaldehyde modification. Background Art
[0002] Rubber adhesives are a type of chemical preparation specifically used to bond rubber to other materials. They can effectively improve the bonding strength between rubber and metal, fabric, plastic and other materials. Rubber adhesives are usually composed of high molecular polymers, plasticizers, stabilizers, fillers and other additives.
[0003] According to the chemical composition and application method, rubber adhesives can be divided into the following categories: solvent-based adhesives, solvent-free adhesives, two-component adhesives. They have excellent mechanical properties and chemical resistance.
[0004] Resorcinol-formaldehyde resin is a commonly used adhesive, especially in the rubber industry, where it is used to improve the bonding properties between rubber and reinforcing materials such as carbon black, fillers or fibers. By modifying the resorcinol-formaldehyde resin, the properties of the adhesive can be further improved to make it more suitable for specific applications.
[0005] When the existing resorcinol-formaldehyde resin is used to prepare rubber adhesives, the product water content of the resorcinol-formaldehyde resin itself is high during the preparation process; resorcinol is easily released during use, which is toxic, not environmentally friendly, and easily has a large content of by-products. Therefore, the rubber adhesive prepared using the resorcinol-formaldehyde resin has safety risks during use, and has poor adhesion and durability, and poor thermal stability. Summary of the invention
[0006] In view of the above problems, the present invention provides a process for preparing rubber adhesive by using resorcinol-formaldehyde modification.
[0007] The technical solution of the present invention is: a process for preparing a rubber adhesive by modifying resorcinol-formaldehyde, comprising the following steps:
[0008] S1. Preparation of resorcinol-formaldehyde resin
[0009] First, styrene-divinylbenzene copolymer resin, resorcinol and organic solvent are mixed in a mass ratio of 1:1.5:3, and stirred evenly at a temperature of 65-70°C to obtain a premix, and a sodium hydroxide solution with a concentration of 1.8-2 mol / L is added to the premix, and the stirring is continued for 2-3 hours to obtain a product A, and the added sodium hydroxide solution accounts for 2-3% of the total weight of the premix. Secondly, formaldehyde solution is continuously added to product A at a rate of 10-15 g / min to obtain product B, and the added formaldehyde solution accounts for 20-25% of the total weight of product A. Then, product B is transferred to a reaction tube, and 2-3% of the total weight of product B is added to the reaction tube. oxalic acid, continue stirring for 10-15 minutes, then place the reaction tube in a microwave synthesizer for microwave radiation heating for 10-20 minutes, until the temperature rises to 95-100°C, to obtain product C, and finally, distill and granulate product C to obtain resorcinol-formaldehyde resin; wherein, styrene-divinylbenzene copolymer resin is used as a catalyst to provide a large number of acid sites, promote the condensation reaction between resorcinol and formaldehyde, improve the selectivity of the reaction, and reduce the generation of by-products. Microwave heating is used to achieve rapid and uniform heating and reduce by-products. Compared with the one-time addition of formaldehyde, the addition rate of formaldehyde is controlled to ensure that formaldehyde can be added continuously, which is helpful to control the reaction rate and balance and reduce the generation of by-products.
[0010] S2. Mixed processing
[0011] Calculated by weight, 40-60 parts of the above-mentioned resorcinol-formaldehyde resin are mixed with 300-400 parts of toluene, and stirred evenly at a temperature of 35-40°C to obtain a mixture A. Then, the mixture A is added to a mixer, and 6-8 parts of hexamethylene diisocyanate, 8-20 parts of polyurethane, 2-4 parts of butylated hydroxyanisole and 2-4 parts of aluminum hydroxide are added in sequence, and the mixing is treated at a speed of 150-170rpm for 2-3h to obtain a mixture B; wherein the hexamethylene diisocyanate can be used as a cross-linking agent and a curing agent, and can react with the hydroxyl group in the resorcinol-formaldehyde resin to form a stable isocyanate bond, thereby improving the adhesion between the adhesive and the rubber substrate, and can provide better heat resistance stability, so that the adhesive can still maintain its performance at a higher temperature. Butylated hydroxyanisole, as an antioxidant, can prevent the adhesive from being degraded due to oxidation during storage and use, thereby extending its service life. Aluminum hydroxide, as a heat stabilizer, improves the thermal stability of the rubber adhesive, so that it can work at a higher temperature without losing performance.
[0012] S3, Mixing treatment
[0013] The mixture B is placed in a mixer, and 3-4 parts of glass fiber and 3-4 parts of diatomaceous earth are added thereto. The mixture is heated to 90-100°C at a rate of 10-15°C / min and mixed for 45-50 minutes. After the mixing is completed, a mixed rubber material is obtained; wherein the glass fiber and diatomaceous earth are used as fillers to improve the mechanical strength and wear resistance of the adhesive.
[0014] S4, cooling molding
[0015] The mixed rubber material is cooled to room temperature after kneading, and is allowed to stand for 8-16 hours to mature the mixed rubber material, and then placed in a calender, and calendered, cooled and cured at a temperature of 110-120°C. After the curing treatment, a resorcinol-formaldehyde modified rubber adhesive is obtained. The purpose of cooling and standing the mixed rubber material after kneading is to mature the rubber material to improve its processing performance and bonding performance. The purpose of the calendering treatment is to prepare a film with a certain thickness and width, while ensuring that the surface of the film is smooth and uniform, and to remove possible bubbles and impurities. This process is crucial to improving the bonding performance of the final product. The curing treatment develops or enhances the mechanical properties and bonding ability of the adhesive through chemical reactions or physical changes.
[0016] Furthermore, in the step S1, the product C is subjected to vacuum filtration + freeze drying dehydration treatment before being distilled and granulated.
[0017] Note: When dehydrating product C by combining vacuum filtration and freeze drying, firstly quickly remove the free water in the sample by vacuum filtration, and then freeze dry the bound water or solvent that is difficult to remove after filtration.
[0018] Furthermore, the specific process of vacuum filtration + freeze drying dehydration treatment of product C is as follows: pour product C into a filtration device for vacuum filtration to remove free water in product C, wherein the vacuum degree of vacuum filtration is 0.02-0.03MPa, and the vacuum filtration time is 1-2h. Then, the vacuum filtered product C is placed in a vacuum freeze drying chamber for secondary dehydration to remove bound water and solvent in product C, wherein the pressure in the vacuum freeze drying chamber is 2-10Pa.
[0019] Description: Vacuum filtration can quickly remove part of the water and shorten the freeze-drying time. Removing part of the water by vacuum filtration in advance can reduce the heat energy required during the freeze-drying process. Due to the pre-vacuum filtration, freeze-drying can be carried out at a lower temperature to better protect heat-sensitive substances.
[0020] Furthermore, in step S2, hexamethylene diisocyanate, polyurethane, butylated hydroxyanisole and aluminum hydroxide are first mixed, and then added to the mixer in an intermittent feeding manner using an intermittent reciprocating feeding device, wherein the interval time between two adjacent feedings is 5-10 minutes.
[0021] Note: Compared with one-time addition, intermittent addition can more finely control the conditions of the chemical reaction, which helps to optimize the quality and yield of the rubber adhesive. At the same time, it can also reduce the side reactions caused by too fast a reaction speed and improve the purity and consistency of the rubber adhesive.
[0022] Furthermore, the intermittent feeding device comprises an outer mounting cylinder, a feeding cylinder provided with an outer wall of the outer mounting cylinder, an intermittent lifting frame provided on an inner wall of the outer mounting cylinder, and a controller;
[0023] The outer wall of the installation outer cylinder is evenly provided with a plurality of through holes from top to bottom, and the feeding cylinder is connected with the inside of the installation outer cylinder through each of the through holes. A feeding port is provided at the upper end of the feeding cylinder, and an automatic opening and closing cover is provided at each through hole;
[0024] The intermittent lifting frame is slidably connected to the inner wall of the mounting outer cylinder, and a plurality of quantitative delivery recesses are evenly arranged on the side wall from top to bottom. The bottom end of the intermittent lifting frame abuts against the outer bottom end of the mounting outer cylinder, and a material guiding ramp is arranged at the bottom end of each of the quantitative delivery recesses. The through-ports correspond one to one with the quantitative delivery recesses. A plurality of mounting ports are arranged at the opening at the bottom end of the mounting outer cylinder, and an inductive mounting block is connected to each of the mounting ports through a micro spring rod. A gravity sensor is arranged on the side wall of the inductive mounting block. A mounting frame is arranged on the upper end of the mounting outer cylinder, and the bottom end of the mounting frame is connected to the upper end of the intermittent lifting frame through an electric telescopic rod. A timer is arranged on the mounting frame, and the controller is electrically connected to the gravity sensor, the electric telescopic rod and the timer.
[0025] Description: When the intermittent feeding device is in use, hexamethylene diisocyanate, polyurethane, butylated hydroxyanisole and aluminum hydroxide are mixed and added to the feeding barrel through the feeding port. When the feeding barrel is filled with the above mixture, each automatic opening and closing cover is opened to allow the mixture in the feeding barrel to be evenly dispersed to the corresponding quantitative feeding recess through each through-port until each quantitative feeding recess is filled with the mixture, and then each automatic opening and closing cover is closed. Then, the electric telescopic rod is started by the controller, and the intermittent lifting frame is driven to move downward in the installation outer cylinder through the extension of the electric telescopic rod. When the bottom end of the quantitative feeding recess at the bottom moves out of the installation outer cylinder, the mixture in the quantitative feeding recess is added to the mixer under the action of the material guide ramp. When the upper end of the quantitative feeding recess is aligned with the upper end of the quantitative feeding recess, the intermittent lifting frame is moved downward in the installation outer cylinder. When the bottom end of the quantitative feeding recess is moved out of the installation outer cylinder, the mixture in the quantitative feeding recess is added to the mixer under the action of the material guide ramp. When the induction mounting block contacts, the micro spring rod will be compressed into the mounting port, and the gravity sensor detects the gravity signal and sends it to the controller. At this time, the controller controls the timer to count. When the timing time is reached, the controller continues to control the electric telescopic rod to extend and drive the intermittent lifting frame to move downward in the mounting outer cylinder until the upper end of the quantitative delivery recess at the upper end position contacts the induction mounting block. Repeat the above steps to add the mixture in each quantitative delivery recess from bottom to top to the mixer, and the interval time between two adjacent additions remains consistent. The above process not only strictly controls the amount of mixture added each time, but also controls the time interval between two adjacent additions. The operation is simple, no human participation is required, and the degree of automation is high, which meets the operational requirements of intermittent feeding.
[0026] Furthermore, a connecting frame assembly is provided at the bottom end of the mounting outer cylinder, and the connecting frame assembly includes a mounting ring sleeved on the outer wall of the mounting outer cylinder, a connecting rod circumferentially arranged on the outer wall of the mounting ring, and an electromagnetic suction plate hinged to the bottom end of each connecting rod.
[0027] Description: Before adding materials, install the outer cylinder just above the mixer feed port, and fix it to the outer wall of the mixer through the electromagnetic suction plates connected to the bottom of each turning rod, so that the intermittent feeding device is fixed to the upper end of the mixer as a whole, saving space. At the same time, since the electromagnetic suction plate connected to the bottom of the turning rod is hinged, it can be fixed on different inclined planes and has high applicability.
[0028] Furthermore, an inclined material guiding pipe is provided on the side wall of the feeding cylinder and corresponding to each of the through openings.
[0029] Note: The purpose of setting the inclined material guide tube is to facilitate adding the mixture in the feeding barrel into each quantitative feeding notch in batches, thereby improving the material guiding effect.
[0030] Further, the mixing treatment method in step S3 is as follows: first, γ-methacrylate propyl silane and isopropanol are mixed in a weight ratio of 1:3, stirred and dissolved in a magnetic stirrer at room temperature, and ammonia water is added to adjust the pH to 7-8 to form a plating solution; second, glass fiber and diatomaceous earth are respectively placed in the above plating solution, heated in a water bath, reacted at a temperature of 60-80°C for 30-40 minutes, and after the reaction, the glass fiber and diatomaceous earth are taken out and washed with distilled water and dried; third, glass fiber, diatomaceous earth and epoxy resin are mixed in a weight ratio of 1:1:3 to form a suspension, and the mixture B of the above weight components is mixed with the suspension, and sodium tripolyphosphate accounting for 2-3% of the total weight of the mixture B and the suspension is added thereto, and stirred continuously for 15-20 minutes at a temperature of 80-90°C to obtain a mixed rubber material. .
[0031] Description: This mixing method can effectively reduce thermal oxidation degradation and extend the service life of the rubber adhesive by avoiding high temperature and prolonged mechanical shearing. It is usually carried out at a lower temperature, which reduces energy consumption, reduces dust generation, and improves the working environment. Before mixing, the surface of the glass fiber and diatomaceous earth is modified by using γ-methacrylate propyl silane. The surface modification of the glass fiber and diatomaceous earth usually involves the introduction of new functional groups, which can produce chemical or physical entanglement with the mixture B to enhance the interfacial adhesion, thereby improving its compatibility and bonding performance, so that the prepared rubber adhesive has high dispersibility, good mechanical properties, high peel strength and tensile strength, and high safety performance, which meets the use requirements.
[0032] Furthermore, the stirring rate of the stirring process is 350-450 rpm.
[0033] Note: Controlling the mixing process parameters is of great significance for ensuring product quality, improving production efficiency and reducing costs.
[0034] Compared with the prior art, the beneficial effects of the present invention are:
[0035] During the preparation of the rubber adhesive of the present invention, hexamethylene diisocyanate is used as a crosslinking agent and a curing agent, which can react with the hydroxyl group in the resorcinol-formaldehyde resin to form a stable isocyanate bond, thereby providing better heat resistance and stability, and enabling the adhesive to maintain its performance at a relatively high temperature. Butylated hydroxyanisole is used as an antioxidant, which can prevent the adhesive from being degraded due to oxidation during storage and use, thereby extending its service life. Aluminum hydroxide is used as a heat stabilizer to improve the heat stability of the rubber adhesive, so that it can work at a relatively high temperature without losing its performance. Glass fiber and diatomaceous earth are used as fillers to improve the mechanical strength and wear resistance of the adhesive. The resorcinol-formaldehyde resin used is prepared by selecting a specific catalyst, using microwaves for uniform heating, and controlling the addition of formaldehyde in batches, thereby overcoming the problems of many byproducts, a large amount of free resorcinol, poor environmental protection, and high volatility during the preparation of the existing resorcinol-formaldehyde resin. The rubber adhesive prepared by the method of the present invention has the advantages of high dispersibility, high heat stability, good mechanical properties, and low oxidation resistance, thereby meeting the use requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the structure of the intermittent lifting frame of the present invention when it is installed inside the outer cylinder;
[0037] Figure 2 It is a schematic structural diagram of an intermittent lifting frame of the present invention partially sliding out of an installation outer cylinder.
[0038] Among them, 1-installation outer cylinder, 10-through opening, 11-installation opening, 110-micro spring rod, 111-sensing installation block, 112-gravity sensor, 12-installation frame, 120-electric telescopic rod, 121-timer, 13-installation collar, 14-connecting turning rod, 15-electromagnetic suction plate, 2-feeding cylinder, 20-feeding opening, 21-inclined material guide pipe, 3-intermittent lifting frame, 30 quantitative feeding recess, 31-material guide ramp, 4-controller. DETAILED DESCRIPTION
[0039] In order to further understand the content of the present invention, the present invention is described in detail below through examples.
[0040] Example 1
[0041] A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification comprises the following steps:
[0042] S1. Preparation of resorcinol-formaldehyde resin
[0043] First, styrene-divinylbenzene copolymer resin, resorcinol and organic solvent are mixed in a mass ratio of 1:1.5:3, and stirred evenly at a temperature of 65°C to obtain a premix, and a sodium hydroxide solution with a concentration of 1.8 mol / L is added to the premix, and the stirring is continued for 2 hours to obtain a product A, and the added sodium hydroxide solution accounts for 2% of the total weight of the premix. Secondly, formaldehyde solution is continuously added to product A at a rate of 10 g / min to obtain product B, and the added formaldehyde solution accounts for 20% of the total weight of product A. Then, product B is transferred to a reaction tube, and oxalic acid accounting for 2% of the total weight of product B is added to the reaction tube, and stirring is continued for 10 minutes. The reaction tube is then placed in a microwave synthesizer for microwave radiation heating for 10 minutes until the temperature rises to 95°C to obtain product C. Finally, product C is distilled and granulated to obtain resorcinol-formaldehyde resin;
[0044] S2. Mixed processing
[0045] 40 parts of the above resorcinol-formaldehyde resin and 300 parts of toluene were mixed by weight, and stirred evenly at a temperature of 35° C. to obtain a mixture A. Then, the mixture A was added to a mixer, and 6 parts of hexamethylene diisocyanate, 8 parts of polyurethane, 2 parts of butylated hydroxyanisole and 2 parts of aluminum hydroxide were added in sequence, and the mixture was mixed at a speed of 150 rpm for 2 hours to obtain a mixture B.
[0046] S3, Mixing treatment
[0047] The mixture B is placed in a mixer, and 3 parts of glass fiber and 3 parts of diatomaceous earth are added thereto, and the mixture is heated to 90°C at a rate of 10°C / min and mixed for 45 minutes to obtain a mixed rubber material;
[0048] S4, calendering and curing
[0049] The mixed rubber material after kneading is cooled to room temperature and allowed to stand for 8 hours to mature, and then put into a calender, and subjected to calendering treatment, cooling and curing treatment at a temperature of 110° C. After the curing treatment, a resorcinol-formaldehyde modified rubber adhesive is obtained.
[0050] Example 2
[0051] A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification comprises the following steps:
[0052] S1. Preparation of resorcinol-formaldehyde resin
[0053] First, styrene-divinylbenzene copolymer resin, resorcinol and organic solvent are mixed in a mass ratio of 1:1.5:3, and stirred evenly at a temperature of 68°C to obtain a premix, and a sodium hydroxide solution with a concentration of 1.9 mol / L is added to the premix, and the stirring is continued for 2.5 hours to obtain a product A, and the added sodium hydroxide solution accounts for 2.5% of the total weight of the premix. Secondly, formaldehyde solution is continuously added to product A at a rate of 13 g / min to obtain product B, and the added formaldehyde solution accounts for 23% of the total weight of product A. Then, product B is transferred to a reaction tube, and oxalic acid accounting for 2.5% of the total weight of product B is added to the reaction tube, and stirring is continued for 13 minutes. The reaction tube is then placed in a microwave synthesizer for microwave radiation heating for 15 minutes until the temperature rises to 98°C to obtain product C. Finally, product C is distilled and granulated to obtain resorcinol-formaldehyde resin;
[0054] S2. Mixed processing
[0055] Calculated by weight, 50 parts of the above resorcinol-formaldehyde resin and 350 parts of toluene were mixed, and stirred evenly at a temperature of 38° C. to obtain a mixture A. Then, the mixture A was added to a mixer, and 7 parts of hexamethylene diisocyanate, 15 parts of polyurethane, 3 parts of butylated hydroxyanisole and 3 parts of aluminum hydroxide were added in sequence, and the mixture was mixed at a speed of 160 rpm for 2.5 hours to obtain a mixture B;
[0056] S3, Mixing treatment
[0057] The mixture B was placed in a mixer, and 3.5 parts of glass fiber and 3.5 parts of diatomaceous earth were added thereto. The mixture was heated to 95°C at a rate of 13°C / min and mixed for 48 minutes. After the mixing was completed, a mixed rubber material was obtained.
[0058] S4, calendering and curing
[0059] The mixed rubber material after kneading is cooled to room temperature and allowed to stand for 12 hours to mature, and then put into a calender, and subjected to calendering treatment, cooling and curing treatment at a temperature of 115° C. After the curing treatment, a resorcinol-formaldehyde modified rubber adhesive is obtained.
[0060] Example 3
[0061] A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification comprises the following steps:
[0062] S1. Preparation of resorcinol-formaldehyde resin
[0063] First, styrene-divinylbenzene copolymer resin, resorcinol and organic solvent are mixed in a mass ratio of 1:1.5:3, and stirred evenly at a temperature of 70°C to obtain a premix, and a sodium hydroxide solution with a concentration of 2 mol / L is added to the premix, and the stirring is continued for 3 hours to obtain a product A, and the added sodium hydroxide solution accounts for 3% of the total weight of the premix. Secondly, formaldehyde solution is continuously added to product A at a rate of 15 g / min to obtain product B, and the added formaldehyde solution accounts for 25% of the total weight of product A. Then, product B is transferred to a reaction tube, and oxalic acid accounting for 3% of the total weight of product B is added to the reaction tube, and stirring is continued for 15 minutes. The reaction tube is then placed in a microwave synthesizer for microwave radiation for 20 minutes until the temperature rises to 100°C to obtain product C. Finally, product C is distilled and granulated to obtain resorcinol-formaldehyde resin;
[0064] S2. Mixed processing
[0065] Calculated by weight, 60 parts of the above resorcinol-formaldehyde resin and 400 parts of toluene were mixed, and stirred evenly at a temperature of 40° C. to obtain a mixture A. Then, the mixture A was added to a mixer, and 8 parts of hexamethylene diisocyanate, 20 parts of polyurethane, 4 parts of butylated hydroxyanisole and 4 parts of aluminum hydroxide were added in sequence, and the mixture was mixed at a speed of 170 rpm for 3 hours to obtain a mixture B;
[0066] S3, Mixing treatment
[0067] The mixture B is placed in a mixer, and 4 parts of glass fiber and 4 parts of diatomaceous earth are added thereto, and the temperature is raised to 100°C at a rate of 15°C / min, and mixed for 50 minutes. After the mixing is completed, a mixed rubber material is obtained;
[0068] S4, calendering and curing
[0069] The mixed rubber material after kneading is cooled to room temperature and allowed to stand for 16 hours to mature, and then put into a calender, and subjected to calendering treatment, cooling and curing treatment at a temperature of 120° C. After the curing treatment, a resorcinol-formaldehyde modified rubber adhesive is obtained.
[0070] According to the national standard GB2794.81, the absolute viscosity of the rubber adhesive obtained in Examples 1-3 was measured using a NDJ.79 type viscometer. The rubber adhesive obtained in Examples 1-3 was quickly added to the viscometer II test unit, the viscometer was turned on, and the data was read when the rotor rotated 12Q ± 2s, and the test results were recorded in Table 1;
[0071] According to the national standard GB7124.86, the shear resistance of the rubber adhesive of Examples 1-3 was tested using a Testometric M350.20 Ⅺ, I electronic tensile testing machine. The sample was placed in the center of the holder. After setting various parameters, the sample was stretched at a speed of 5 mm / min and the mark of the working part of the sample was tracked by the extension pointer. The load data when the sample was torn off was recorded to obtain the shear strength data of the rubber adhesive to the metal, and the test results were recorded in Table 1.
[0072] Table 1 Performance of rubber adhesives prepared using the process of Examples 1-3
[0073] Example 1 Example 2 Example 3 Absolute viscosity (mPa·s) 3500 4800 4900 Shear strength(MPa) 1.58 2.42 2.54
[0074] It can be seen from Table 1 that, under the premise of the rubber adhesive prepared by the process of Examples 1-3, the absolute viscosity is proportional to the shear strength value. A higher absolute viscosity means that the adhesive can form a denser network structure during the curing process, which may lead to a higher shear strength. The absolute viscosity and shear strength values of the rubber adhesive prepared by the process of Example 3 are the largest, providing the rubber adhesive with better coating uniformity and lower leakage risk, and at the same time, it can effectively resist separation or cracking caused by external forces.
[0075] Example 4
[0076] The difference between this embodiment and embodiment 3 is that:
[0077] In the step S1, the product C is subjected to vacuum filtration + freeze drying dehydration treatment before distillation and granulation;
[0078] The specific process of vacuum filtration + freeze drying dehydration treatment of product C is as follows: pour product C into a filtration device for vacuum filtration to remove free water in product C, wherein the vacuum degree of vacuum filtration is 0.02MPa, and the vacuum filtration time is 1h. Then, the vacuum filtered product C is placed in a vacuum freeze drying chamber for secondary dehydration to remove bound water and solvent in product C, wherein the pressure in the vacuum freeze drying chamber is 2Pa.
[0079] Example 5
[0080] The difference between this embodiment and embodiment 4 is that:
[0081] In the step S1, the product C is subjected to vacuum filtration + freeze drying dehydration treatment before distillation and granulation;
[0082] The specific process of vacuum filtration + freeze drying dehydration treatment of product C is as follows: pour product C into a filtration device for vacuum filtration to remove free water in product C, wherein the vacuum degree of vacuum filtration is 0.025MPa, and the vacuum filtration time is 1.5h. Then, the vacuum filtered product C is placed in a vacuum freeze drying chamber for secondary dehydration to remove bound water and solvent in product C, wherein the pressure in the vacuum freeze drying chamber is 6Pa.
[0083] Example 6
[0084] The difference between this embodiment and embodiment 4 is that:
[0085] In the step S1, the product C is subjected to vacuum filtration + freeze drying dehydration treatment before distillation and granulation;
[0086] The specific process of vacuum filtration + freeze drying dehydration treatment of product C is as follows: pour product C into a filtration device for vacuum filtration to remove free water in product C, wherein the vacuum degree of vacuum filtration is 0.03MPa, and the vacuum filtration time is 2h. Then, the vacuum filtered product C is placed in a vacuum freeze drying chamber for secondary dehydration to remove bound water and solvent in product C, wherein the pressure in the vacuum freeze drying chamber is 10Pa.
[0087] Weigh 2.0 g of the resorcinol-formaldehyde resin samples prepared by the processes of Examples 4-6, grind them to disperse them evenly, put them into 10 ml volumetric flasks, dissolve them with methanol and dilute them to the mark to form extracts, and centrifuge the extracts to remove insoluble solid particles to obtain clear supernatants. Under the set high performance liquid chromatography conditions, under the same chromatographic conditions, the free resorcinol content in the three supernatants was determined respectively. The mass fraction (M) of free resorcinol in the supernatant was calculated as follows:
[0088]
[0089] Where, m is the mass concentration of the adhesive resin sample, mg·mL -1 , the M determination results of the three supernatant samples are shown in Table 2;
[0090] Table 2: Mass fraction of free resorcinol in the resorcinol-formaldehyde resin samples prepared by the process of Examples 4-5
[0091] Example 4 Example 5 Example 6 <![CDATA[m / (mg·mL -1 )]]> 2.66 2.73 2.75 A / (Au·s) 0.91 0.85 0.59 M×100 1.8 1.63 1.13
[0092] As can be seen from Table 2, on the basis of Example 3, the percentages of free resorcinol in the resorcinol-formaldehyde resin samples prepared by the processes of Examples 4-6 are 1.8%, 1.63% and 1.13%, respectively. The free resorcinol content will significantly affect the mechanical properties, thermal stability, bonding properties, etc. of the prepared resorcinol-formaldehyde resin, and the free resorcinol percentage in the resorcinol-formaldehyde resin sample prepared by the process of Example 6 is the smallest, that is, the amount of free resorcinol is the least. Therefore, the rubber adhesive prepared by the resorcinol-formaldehyde resin sample prepared by the process of Example 6 has the best thermal stability, mechanical properties and bonding properties.
[0093] Example 7
[0094] The difference between this embodiment and embodiment 6 is that:
[0095] In the step S2, hexamethylene diisocyanate, polyurethane, butylated hydroxyanisole and aluminum hydroxide are first mixed, and then added to the mixer in an intermittent feeding manner using an intermittent feeding device, wherein the interval between two adjacent feedings is 5 minutes;
[0096] like Figure 1 , 2 As shown, the intermittent feeding device comprises an outer cylinder 1, a feeding cylinder 2 provided with an outer wall of the outer cylinder 1, an intermittent lifting frame 3 provided on the inner wall of the outer cylinder 1, and a controller 4;
[0097] The outer wall of the installation outer cylinder 1 is evenly provided with 8 through holes 10 from top to bottom, and the feeding cylinder 2 is connected to the inside of the installation outer cylinder 1 through each through hole 10. The upper end of the feeding cylinder 2 is provided with a feeding port 20, and each through hole 10 is provided with an automatic opening and closing cover plate 100;
[0098] The intermittent lifting frame 3 is slidably connected to the inner wall of the mounting outer cylinder 1, and four quantitative delivery notches 30 are evenly arranged on the side wall from top to bottom. The bottom end of the intermittent lifting frame 3 abuts against the outer bottom end of the mounting outer cylinder 1, and a material guide ramp 31 is arranged at the bottom end of each quantitative delivery notch 30. The through-hole 10 corresponds to the quantitative delivery notch 30 one by one. Two mounting ports 11 are arranged at the opening at the bottom end of the mounting outer cylinder 1, and a sensing mounting block 111 is connected to each mounting port 11 through a micro spring rod 110. A gravity sensor 112 is arranged on the side wall of the sensing mounting block 111. A mounting frame 12 is arranged at the upper end of the mounting outer cylinder 1, and the bottom end of the mounting frame 12 is connected to the upper end of the intermittent lifting frame 3 through an electric telescopic rod 120. A timer 121 is arranged on the mounting frame 12, and the controller 4 is electrically connected to the gravity sensor 112, the electric telescopic rod 120 and the timer 121.
[0099] A connecting frame assembly is provided at the bottom end of the feeding barrel 2, and the connecting frame assembly includes a mounting collar 13 sleeved on the outer wall of the feeding barrel 2, a connecting rod 14 circumferentially arranged on the outer wall of the mounting collar 13, and an electromagnetic suction plate 15 hinged to the bottom end of each connecting rod 14;
[0100] An inclined material guide pipe 21 is provided on the side wall of the feeding cylinder 2 and corresponding to each through opening 10;
[0101] Among them, the gravity sensor 112, the electric telescopic rod 120, the timer 121 and the controller 4 all adopt the existing technology;
[0102] When the intermittent feeding device is in use, hexamethylene diisocyanate, polyurethane, butylated hydroxyanisole and aluminum hydroxide are mixed and added to the feeding barrel 2 through the feeding port 20. When the feeding barrel 2 is filled with the above mixture, each automatic opening and closing cover 100 is opened to allow the mixture in the feeding barrel 2 to be evenly dispersed to the corresponding quantitative feeding recess 30 through each through-port 10, until each quantitative feeding recess 30 is filled with the mixture, each automatic opening and closing cover 100 is closed, and then, the electric telescopic rod 120 is started by the controller 4, and the intermittent lifting frame 3 is driven to move downward in the installation outer cylinder 1 through the extension effect of the electric telescopic rod 120. When the bottom end of the quantitative feeding recess 30 at the bottom moves out of the installation outer cylinder 1, under the action of the material guide ramp 31 , so that the mixture in the quantitative delivery recess 30 is added to the mixer. When the upper end of the quantitative delivery recess 30 contacts the inductive mounting block 111, the micro spring rod 110 is compressed into the mounting port 11, and the gravity sensor 112 detects the gravity signal and sends it to the controller 4. At this time, the controller 4 controls the timer 121 to count. When the timing time is reached, the controller 4 continues to control the electric telescopic rod 120 to extend and drive the intermittent lifting frame 3 to move downward in the mounting outer cylinder 1 until the upper end of the quantitative delivery recess 30 located at the upper end position contacts the inductive mounting block 111. Repeat the above steps to add the mixture in each quantitative delivery recess 30 from bottom to top to the mixer, and the interval time between two adjacent additions remains consistent.
[0103] Example 8
[0104] The difference between this embodiment and embodiment 7 is that:
[0105] In the step S2, hexamethylene diisocyanate, polyurethane, butylated hydroxyanisole and aluminum hydroxide are first mixed, and then added to the mixer in an intermittent feeding manner using an intermittent feeding device, wherein the interval time between two adjacent feedings is 10 minutes.
[0106] Example 9
[0107] The difference between this embodiment and embodiment 8 is that:
[0108] The mixing method in step S3 is as follows: first, γ-methacrylate propyl silane and isopropanol are mixed in a weight ratio of 1:3, stirred and dissolved in a magnetic stirrer at room temperature, and ammonia water is added dropwise to adjust the pH to 7 to form a plating solution; secondly, glass fiber and diatomaceous earth are respectively placed in the above-mentioned plating solution, heated in a water bath, and reacted at a temperature of 60° C. for 30 minutes. After the reaction is completed, the glass fiber and diatomaceous earth are taken out and washed and dried with distilled water; thirdly, glass fiber, diatomaceous earth and epoxy resin are mixed in a weight ratio of 1:1:3 to form a suspension, and the mixture B of the above-mentioned weight components is mixed with the suspension, and sodium tripolyphosphate accounting for 2% of the total weight of the mixture B and the suspension is added thereto, and stirring is continued for 15 minutes at a temperature of 80° C. to obtain a mixed rubber material;
[0109] The stirring rate of the stirring process is 350 rpm.
[0110] Example 10
[0111] The difference between this embodiment and embodiment 9 is that:
[0112] The mixing method in step S3 is as follows: first, γ-methacrylate propyl silane and isopropanol are mixed in a weight ratio of 1:3, stirred and dissolved in a magnetic stirrer at room temperature, and ammonia water is added dropwise to adjust the pH to 8 to form a plating solution; secondly, glass fiber and diatomaceous earth are respectively placed in the above-mentioned plating solution, heated in a water bath, and reacted at a temperature of 80°C for 40 minutes. After the reaction is completed, the glass fiber and diatomaceous earth are taken out and washed and dried with distilled water; thirdly, glass fiber, diatomaceous earth and epoxy resin are mixed in a weight ratio of 1:1:3 to form a suspension, and the mixture B of the above-mentioned weight components is mixed with the suspension, and sodium tripolyphosphate accounting for 3% of the total weight of the mixture B and the suspension is added thereto, and stirring is continued for 20 minutes at a temperature of 80-90°C to obtain a mixed rubber material;
[0113] The stirring rate of the stirring process is 450 rpm.
[0114] The rubber adhesive prepared by the prior art process and the rubber adhesive prepared by the method of Examples 6-10 were tested for various properties, and the test results are shown in Table 1:
[0115] Table 1: Performance test table of rubber adhesive prepared by the prior art process and rubber adhesive prepared by the method of Examples 6-10
[0116] Viscosity (mPa·s) Peel strength (N / m) Bond strength (MPa) Example 6 2362 0.8 14.7 Example 7 2456 0.84 15.2 Example 8 2590 0.95 15.9 Example 9 2630 1.0 16.1 Example 10 2780 1.2 16.3 Prior art 2050 0.5 10.3
[0117] It can be seen from Table 1 that, on the basis of Example 6, the viscosity, peel strength and bonding strength of the rubber adhesive prepared by the process of Examples 7-10 increase in sequence, and viscosity, peel strength and bonding strength are key indicators, which respectively reflect the fluidity, durability and bonding ability of the adhesive, indicating that the fluidity, durability and bonding ability of the rubber adhesive prepared by the process methods of Examples 7-10 are gradually improved, among which, the viscosity, peel strength and bonding strength of Example 10 are the largest, and its viscosity is better, its mechanical properties are good, and its thermal stability is high. Therefore, on the basis that the process of Examples 7-10 is superior to the prior art, Example 10 is the best embodiment.
Claims
1. A process for preparing a rubber adhesive by modifying resorcinol-formaldehyde, characterized in that: The following steps are involved: S1. Preparation of resorcinol-formaldehyde resin First, styrene-divinylbenzene copolymer resin, resorcinol and organic solvent are mixed in a mass ratio of 1:1.5:3, and stirred evenly at a temperature of 65-70°C to obtain a premix, and a sodium hydroxide solution with a concentration of 1.8-2 mol / L is added to the premix, and the stirring is continued for 2-3 hours to obtain a product A, and the added sodium hydroxide solution accounts for 2-3% of the total weight of the premix; secondly, a formaldehyde solution is continuously added to the product A at a rate of 10-15 g / min to obtain a product B, and the added formaldehyde solution accounts for 20-25% of the total weight of the product A; then, the product B is transferred to a reaction tube, and oxalic acid accounting for 2-3% of the total weight of the product B is added to the reaction tube, and the stirring is continued for 10-15 minutes, and then the reaction tube is placed in a microwave synthesizer for microwave radiation heating for 10-20 minutes until the temperature rises to 95-100°C to obtain a product C; finally, the product C is distilled and granulated to obtain a resorcinol-formaldehyde resin; S2. Mixed processing 40-60 parts of the above resorcinol-formaldehyde resin and 300-400 parts of toluene are mixed by weight, and stirred evenly at a temperature of 35-40° C. to obtain a mixture A. Then, the mixture A is added to a mixer, and 6-8 parts of hexamethylene diisocyanate, 8-20 parts of polyurethane, 2-4 parts of butylated hydroxyanisole and 2-4 parts of aluminum hydroxide are added, and the mixture is mixed at a speed of 150-170 rpm for 2-3 hours to obtain a mixture B; S3, Mixing treatment The mixture B is placed in a mixer, and 3-4 parts of glass fiber and 3-4 parts of diatomaceous earth are added thereto, and the mixture is heated to 90-100°C at a rate of 10-15°C / min, and mixed for 45-50 minutes to obtain a mixed rubber material; S4, calendering and curing The mixed rubber material after kneading is cooled to room temperature and allowed to stand for 8-16 hours to mature, and then put into a calender, and subjected to calendering treatment, cooling and curing treatment at a temperature of 110-120° C., and after the curing treatment, a resorcinol-formaldehyde modified rubber adhesive is obtained.
2. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 1, characterized in that: In the step S1, the product C is subjected to vacuum filtration and freeze-drying dehydration treatment before being distilled and granulated.
3. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 2, characterized in that: The specific process of vacuum filtration + freeze drying dehydration treatment of product C is as follows: pour product C into a filtration device for vacuum filtration to remove free water in product C, wherein the vacuum degree of vacuum filtration is 0.02-0.03MPa, and the vacuum filtration time is 1-2h. Then, the vacuum filtered product C is placed in a vacuum freeze drying chamber for secondary dehydration to remove bound water and solvent in product C, wherein the pressure in the vacuum freeze drying chamber is 2-10Pa.
4. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 1, characterized in that: In the step S2, hexamethylene diisocyanate, polyurethane, butylated hydroxyanisole and aluminum hydroxide are first mixed, and then added to the mixer in an intermittent feeding manner using an intermittent feeding device, wherein the interval time between two adjacent additions is 5-10 minutes.
5. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 4, characterized in that: The intermittent feeding device comprises an outer mounting cylinder (1), a feeding cylinder (2) arranged on the outer wall of the outer mounting cylinder (1), an intermittent lifting frame (3) arranged on the inner wall of the outer mounting cylinder (1), and a controller (4); The outer wall of the installation outer cylinder (1) is evenly provided with a plurality of through-holes (10) from top to bottom, the feeding cylinder (2) is connected to the interior of the installation outer cylinder (1) through each of the through-holes (10), a feeding port (20) is provided at the upper end of the feeding cylinder (2), and an automatic opening and closing cover plate (100) is provided at each through-hole (10); The intermittent lifting frame (3) is slidably connected to the inner wall of the mounting outer cylinder (1), and the side wall is evenly provided with a plurality of quantitative delivery notches (30) from top to bottom. The bottom end of the intermittent lifting frame (3) abuts against the outer bottom end of the mounting outer cylinder (1), and the bottom end of each of the quantitative delivery notches (30) is provided with a material guiding ramp (31). The through opening (10) corresponds to the quantitative delivery notches (30) one by one. A plurality of mounting openings (11) are provided at the bottom opening of the mounting outer cylinder (1), and each of the mounting openings (11) is provided with a micro spring rod. The rod (110) is connected to a sensing mounting block (111), a gravity sensor (112) is provided on the side wall of the sensing mounting block (111), a mounting frame (12) is provided at the upper end of the mounting outer cylinder (1), and the bottom end of the mounting frame (12) is connected to the upper end of the intermittent lifting frame (3) through an electric telescopic rod (120), a timer (121) is provided on the mounting frame (12), and the controller (4) is electrically connected to the gravity sensor (112), the electric telescopic rod (120) and the timer (121).
6. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 5, characterized in that: A connecting frame assembly is provided at the bottom end of the feeding barrel (2), and the connecting frame assembly comprises a mounting ring (13) sleeved on the outer wall of the feeding barrel (2), a connecting rod (14) circumferentially arranged on the outer wall of the mounting ring (13), and an electromagnetic suction plate (15) hinged to the bottom end of each connecting rod (14).
7. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 5, characterized in that: An inclined material guiding pipe (21) is provided on the side wall of the feeding cylinder (2) and corresponding to each of the through openings (10).
8. The process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 1, characterized in that: The mixing treatment method in step S3 is as follows: first, γ-methacrylate propyl silane and isopropanol are mixed in a weight ratio of 1:3, stirred and dissolved in a magnetic stirrer at room temperature, and ammonia water is added dropwise to adjust the pH to 7-8 to form a plating solution; secondly, glass fiber and diatomaceous earth are respectively placed in the above-mentioned plating solution, heated in a water bath, and reacted at a temperature of 60-80°C for 30-40 minutes. After the reaction is completed, the glass fiber and diatomaceous earth are taken out and washed with distilled water and dried; thirdly, glass fiber, diatomaceous earth and epoxy resin are mixed in a weight ratio of 1:1:3 to form a suspension, and the mixture B of the above-mentioned weight components is mixed with the suspension, and sodium tripolyphosphate accounting for 2-3% of the total weight of the mixture B and the suspension is added thereto, and stirring is continued for 15-20 minutes at a temperature of 80-90°C to obtain a mixed rubber material.
9. A process for preparing a rubber adhesive by using resorcinol-formaldehyde modification according to claim 8, characterized in that: The stirring rate of the magnetic stirrer is 350-450 rpm.