Film-forming composition, surface treatment method for copper-containing materials, use
By treating the surface of copper materials with a film-forming composition and a hydrated hydrazine solution, a uniform oxide film layer is formed, which solves the problems of poor bonding strength and airtightness between copper and resin, and achieves efficient metal-resin bonding.
Patent Information
- Application Number
- CN202211590396.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-12-12
AI Technical Summary
Existing nano-surface processing technologies are not ideal for copper applications, resulting in weak bonding strength, poor airtightness, and high processing costs.
A film-forming composition comprising potassium persulfate, sodium hydroxide and benzotriazole is used to treat the surface of copper material to form a uniform oxide film layer. This is followed by a second immersion in a hydrated hydrazine solution, and then injection molding to tightly bond the oxide film with the resin.
It improves the bonding strength and airtightness between copper materials and resin, reduces process costs, and forms a uniform oxide film layer that meets the requirements for high airtightness.
Smart Images

Figure CN118186385B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of materials processing technology, and in particular to a film-forming composition, a surface treatment method for copper-containing materials, and their applications. Background Technology
[0002] Nanomaterial surface treatment (NMT) is a widely used metal-resin bonding technology. It involves first nano-treating the metal surface, and then directly injection molding the resin onto the metal surface to obtain an integrated metal-plastic product. This technology has been widely used in the automotive, toy, and component packaging industries.
[0003] However, existing nano-surface processing technologies are generally only applicable to materials such as aluminum alloys, magnesium alloys, and stainless steel, and their application effect on copper is not ideal.
[0004] Therefore, an increasing number of studies are dedicated to providing a nano-surface processing technology applicable to copper.
[0005] For example, some manufacturers use micro-etching technology to treat the surface of copper. After micro-etching, pits are formed on the surface of copper, which can have a certain bonding force when combined with plastic, but the bonding strength is weak.
[0006] For example, some manufacturers use electroplating to first plate a layer of nickel film on the copper surface, giving it a coral-like appearance. This can achieve a good bonding effect between copper and plastic. However, this method is very expensive, and due to the characteristics of electroplating, the film thickness produced at different locations on the copper surface will be inconsistent, affecting the stability of the material's performance.
[0007] For example, some manufacturers use a copper treatment method. The specific steps are roughly as follows: first, acid etching is performed to create small holes on the copper surface, and then a thin film is oxidized on the copper surface. Although the presence of acid etching holes and oxide film is beneficial to improving the bonding ability between metallic copper and plastic, the oxide film layer formed by this method is uneven and thin, and the pores in the film layer are small. During injection molding, the depth of the resin bonding with copper is too shallow, resulting in poor air tightness of the product. Summary of the Invention
[0008] Therefore, it is necessary to provide a film-forming composition that, when used to surface treat copper-containing materials, can not only improve the bonding force between the copper-containing materials and the resin, but also improve the airtightness of the bonded material and reduce the impact on the performance of the bonded material.
[0009] Furthermore, it is necessary to provide a surface treatment method and application for copper-containing materials.
[0010] One embodiment of this application provides a film-forming composition comprising potassium persulfate, sodium hydroxide, benzotriazole, and water, wherein the mass fraction of potassium persulfate is 10% to 12%, the mass fraction of sodium hydroxide is 8% to 15%, and the mass fraction of benzotriazole is 15% to 20%.
[0011] An embodiment of this application also provides a surface treatment method for copper-containing materials, comprising the following steps:
[0012] The copper-containing material is placed in the film-forming composition as described in any of the above embodiments and subjected to a first immersion to form an oxide film layer; the copper-containing material is selected from elemental copper or copper alloy.
[0013] In one embodiment, the conditions for the first soaking satisfy one or more of the following conditions:
[0014] (1) The temperature of the first soaking is 50℃~80℃;
[0015] (2) The first soaking time is 5 to 10 minutes.
[0016] In one embodiment, the thickness of the oxide film is 500 nanometers to 3000 nanometers.
[0017] In one embodiment, the following steps are also included:
[0018] The copper-containing material that has formed the oxide film layer is then placed in a hydrated hydrazine solution for a second immersion.
[0019] In one embodiment, the mass fraction of ammonia in the hydrated hydrazine solution is 3% to 10%.
[0020] In one embodiment, the temperature of the second immersion is 50°C to 70°C.
[0021] In one embodiment, the second soaking time is 1 to 4 minutes.
[0022] One embodiment of this application also provides a processed copper material, which is obtained by the surface treatment method for copper-containing materials as described in any of the above embodiments.
[0023] An embodiment of this application also provides a bonding material, including resin and processed copper material as described in the above embodiment, wherein the resin is bonded to the processed copper material by an injection molding process.
[0024] The above-mentioned film-forming composition is used to treat the surface of copper-containing materials. The copper-containing materials are immersed in the film-forming composition, which can quickly form a uniform and smooth oxide film layer on the surface of the copper-containing materials. The processed copper material obtained after surface treatment has good bonding ability with resin. The metal-resin bonded material has good density, can meet the requirements of high airtightness, and will not have an adverse effect on the properties of the copper metal itself. Attached Figure Description
[0025] Figure 1 This is an image obtained by SEM scanning of a cross-section of the processed copper material in Embodiment 3 of this application;
[0026] Figure 2 This is an image obtained by SEM scanning of the front side of the processed copper material in Embodiment 3 of this application. Detailed Implementation
[0027] To facilitate understanding of this application, a more comprehensive description of the application is provided below with reference to embodiments and accompanying drawings. This application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.
[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used in this application's specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used in this application includes any and all combinations of one or more of the associated listed items.
[0029] In this application, the technical features described in an open-ended manner include both closed-ended technical solutions comprised of the listed features and open-ended technical solutions that include the listed features. Unless otherwise shown or indicated in the operational embodiments, all figures used to represent the quantities, physicochemical properties, etc., of ingredients in the specification and claims are to be understood to be adjusted by the term "about" in all cases. For example, therefore, unless stated to the contrary, the numerical parameters listed in the foregoing specification and appended claims are approximations, and those skilled in the art can appropriately modify these approximations to obtain the desired characteristics by utilizing the teachings disclosed herein. The use of numerical ranges indicated by endpoints includes all numbers within that range and any range within that range; for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4, and 5, etc.
[0030] The weights of the relevant components mentioned in the embodiments of this invention can refer not only to the specific content of each component, but also to the proportional relationship between the weights of the components. Therefore, any scaling up or down of the content of the relevant components according to the embodiments of this invention is within the scope disclosed in the embodiments of this invention. Specifically, the weights mentioned in the embodiments of this invention can be well-known units of mass in the chemical industry, such as μg, mg, g, and kg.
[0031] One embodiment of this application provides a film-forming composition comprising potassium persulfate, sodium hydroxide, benzotriazole, and water, wherein the mass fraction of potassium persulfate is 10%–12%, the mass fraction of sodium hydroxide is 8%–15%, and the mass fraction of benzotriazole is 15%–20%.
[0032] Potassium persulfate is a film-forming agent in the film-forming composition, acting as a catalyst to accelerate the formation of an oxide film on the copper metal surface. Understandably, the mass fraction of potassium persulfate can be, for example, but not limited to, 10%, 10.2%, 10.4%, 10.6%, 10.8%, 11%, 11.2%, 11.4%, 11.6%, 11.8%, 12%, etc.
[0033] Sodium hydroxide is the main salt in the film-forming composition. Under the catalysis of potassium persulfate, it reacts with copper-containing materials to form a dark red or black copper oxide, i.e., an oxide film. Understandably, the mass fraction of sodium hydroxide can be, for example, but not limited to, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, etc.
[0034] Benzotriazole is a slow-release agent in the film-forming composition, which can prevent excessive corrosion of the copper-containing material surface by sodium hydroxide, effectively ensuring that the copper-containing material surface still has good smoothness after surface treatment. Understandably, the mass fraction of benzotriazole can be, for example, but not limited to, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, etc.
[0035] By using the above-mentioned film-forming composition to surface treat copper-containing materials, a uniform and smooth oxide film layer can be quickly formed on the surface of the copper-containing materials. The processed copper material obtained after surface treatment has good bonding ability with resin. The resulting metal-resin bonded material has good density, can meet the requirements of high airtightness, and will not have an adverse effect on the properties of the copper metal itself.
[0036] An embodiment of this application also provides a surface treatment method for copper-containing materials, comprising the following steps:
[0037] The copper-containing material is placed in the film-forming composition as described in any of the above embodiments and subjected to a first immersion to form an oxide film layer; the copper-containing material is selected from elemental copper or copper alloy.
[0038] After treating the copper surface with a film-forming composition, a uniform oxide film layer can be formed on the surface of the copper-containing material. The oxide film layer is relatively thick, and the interparticle gaps in the oxide film layer can accommodate more resin. The surface-treated copper material is tightly bonded to the resin through injection molding, resulting in a very strong bond. The bond strength between the processed copper material and the resin can reach the strength level of other metals such as aluminum alloys and magnesium alloys bonded to resin.
[0039] In one embodiment, the temperature of the first immersion is 50°C to 80°C. It is understood that the temperature of the first immersion may be, for example, but not limited to, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc.
[0040] In one embodiment, the first soaking time is 5 to 10 minutes. Understandably, the first soaking time may be, for example, but not limited to, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc.
[0041] In one embodiment, the thickness of the oxide film is 500 nm to 3000 nm. A thicker oxide film can create more gaps for bonding with the resin, allowing the resin to penetrate deeper into the copper-containing material during injection molding, thus resulting in a tighter bond between the processed copper and the resin. Understandably, the thickness of the oxide film can be, for example, but not limited to, 500 nm, 800 nm, 1000 nm, 1200 nm, 1500 nm, 1800 nm, 200 nm, 2200 nm, 2500 nm, 2800 nm, 3000 nm, etc.
[0042] In one embodiment, the following steps are also included:
[0043] The copper-containing material with the oxide film layer formed is then placed in a hydrated hydrazine solution for a second immersion.
[0044] The hydrated hydrazine solution is absorbed and adsorbed into the oxide film layer of the copper-containing material through immersion. The presence of the hydrated hydrazine solution is conducive to further promoting the tight bonding between the resin and the processed copper material during injection molding.
[0045] In one embodiment, the mass fraction of ammonia in the hydrated hydrazine solution is 3% to 10%. It is understood that the mass fraction of ammonia in the hydrated hydrazine solution may, for example, but not limited to, be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0046] In one embodiment, the temperature of the second immersion is 50°C to 70°C. It is understood that the temperature of the second immersion may be, for example, but not limited to, 50°C, 55°C, 60°C, 65°C, 70°C, etc.
[0047] In one embodiment, the second soaking time is 1 to 4 minutes. Understandably, the second soaking time can be, for example, but is not limited to, 1 minute, 2 minutes, 3 minutes, 4 minutes, etc.
[0048] One embodiment of this application also provides a processed copper material, which is obtained by the surface treatment method of copper-containing materials as described in any of the above embodiments.
[0049] An embodiment of this application also provides a bonding material, including resin and processed copper as described in the above embodiment, wherein the resin is bonded to the processed copper by an injection molding process.
[0050] The surface treatment method for copper-containing materials in any of the above embodiments has the following advantages:
[0051] (1) By surface treatment of copper-containing materials with the film-forming composition in any of the above embodiments, a uniform and smooth oxide film layer can be quickly formed on the surface of the copper-containing materials. Then, the copper-containing materials are tightly bonded to the resin by injection molding. The bonding force between the copper-containing materials and the resin is comparable to that between other metals such as aluminum alloys and magnesium alloys and the resin.
[0052] (2) The above method can form a uniform oxide film layer by simply soaking, which has a lower processing cost and a more uniform oxide film layer.
[0053] (3) The oxide film layer formed by the above method is thicker, and the interparticle gaps on the oxide film layer can provide more space for bonding with the resin, so that the resin and the processed copper material can achieve a tight bond. The above method does not require the step of first etching small holes on the copper surface by acid etching, the operation process is simpler, and the metal-resin bonded material produced has good density, which can meet the requirements of high airtightness.
[0054] The following detailed description, in conjunction with specific embodiments and comparative examples, further illustrates the film-forming composition, surface treatment method for copper-containing materials, and applications of this application. It is understood that the following embodiments are more specific, and other embodiments are not limited thereto.
[0055] Example 1
[0056] Step 1: Formulate the film composition
[0057] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 10%, the mass fraction of sodium hydroxide is 12%, and the mass fraction of benzotriazole is 15%.
[0058] Step 2: Surface treatment of copper-containing materials
[0059] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0060] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0061] Example 2
[0062] Step 1: Formulate the film composition
[0063] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 12%, the mass fraction of sodium hydroxide is 8%, and the mass fraction of benzotriazole is 20%.
[0064] Step 2: Surface treatment of copper-containing materials
[0065] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: immersion at a constant temperature of 80°C for 10 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer with a thickness of 3000 nanometers is generated on the surface of the copper-containing material.
[0066] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 70°C for a second immersion for 1 minute. The mass fraction of ammonia in the hydrated hydrazine solution is 3%.
[0067] Example 3
[0068] Step 1: Formulate the film composition
[0069] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 11%, the mass fraction of sodium hydroxide is 15%, and the mass fraction of benzotriazole is 18%.
[0070] Step 2: Surface treatment of copper-containing materials
[0071] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: immersion at a constant temperature of 60°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer with a thickness of 1000 nanometers is generated on the surface of the copper-containing material.
[0072] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 60°C for a second immersion for 4 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 10%.
[0073] Comparative Example 1
[0074] Step 1: Formulate the film composition
[0075] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 15%, the mass fraction of sodium hydroxide is 12%, and the mass fraction of benzotriazole is 15%.
[0076] Step 2: Surface treatment of copper-containing materials
[0077] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0078] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0079] Comparative Example 2
[0080] Step 1: Formulate the film composition
[0081] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 6%, the mass fraction of sodium hydroxide is 12%, and the mass fraction of benzotriazole is 15%.
[0082] Step 2: Surface treatment of copper-containing materials
[0083] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0084] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0085] Comparative Example 3
[0086] Step 1: Formulate the film composition
[0087] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 10%, the mass fraction of sodium hydroxide is 20%, and the mass fraction of benzotriazole is 15%.
[0088] Step 2: Surface treatment of copper-containing materials
[0089] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0090] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0091] Comparative Example 4
[0092] Step 1: Formulate the film composition
[0093] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 10%, the mass fraction of sodium hydroxide is 5%, and the mass fraction of benzotriazole is 15%.
[0094] Step 2: Surface treatment of copper-containing materials
[0095] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0096] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0097] Comparative Example 5
[0098] Step 1: Formulate the film composition
[0099] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 10%, the mass fraction of sodium hydroxide is 12%, and the mass fraction of benzotriazole is 25%.
[0100] Step 2: Surface treatment of copper-containing materials
[0101] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0102] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0103] Comparative Example 6
[0104] Step 1: Formulate the film composition
[0105] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 10%, the mass fraction of sodium hydroxide is 12%, and the mass fraction of benzotriazole is 10%.
[0106] Step 2: Surface treatment of copper-containing materials
[0107] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0108] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0109] Comparative Example 7
[0110] Step 1: Formulate the film composition
[0111] The film-forming composition comprises potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of sodium m-nitrobenzenesulfonate is 10%, the mass fraction of sodium hydroxide is 12%, and the mass fraction of benzotriazole is 15%.
[0112] Step 2: Surface treatment of copper-containing materials
[0113] Copper is selected as the copper-containing material. The copper-containing material to be processed is cleaned and then placed in the film-forming composition prepared in step one for the first immersion. The conditions for the first immersion are: maintaining a constant temperature of 50°C for 5 minutes until the surface of the copper-containing material turns dark red or black. At this time, a uniform oxide film layer is generated on the surface of the copper-containing material, and the thickness of the oxide film layer is 500 nanometers.
[0114] Then, the copper-containing material that has formed an oxide film is removed, cleaned, and the residual film-forming composition on the surface of the copper-containing material is removed. Then, the copper-containing material is placed in a hydrated hydrazine solution at 50°C for a second immersion for 2 minutes. The mass fraction of ammonia in the hydrated hydrazine solution is 5%.
[0115] The main process parameters of the surface treatment methods for copper-containing materials in Examples 1 to 3 and Comparative Examples 1 to 7 are summarized in Table 1 below.
[0116] Table 1 Summary of main process parameters for surface treatment methods of copper-containing materials
[0117]
[0118] Figure 1 and Figure 2 The images shown are obtained by SEM scanning of the cross-section and front side of the processed copper material in Example 3. The oxide film layer is about 1000nm thick and has a uniform surface morphology with a dense, fluffy appearance. This film can effectively contain the molten resin, thereby greatly improving the bonding ability between the processed copper material and the resin.
[0119] The copper-containing material was surface-treated according to the methods of Examples 1 to 3 and Comparative Examples 1 to 7 to obtain the processed copper material. The processed copper material was then bonded to resin through injection molding to form a bonded material between the processed copper material and the resin. The bonded material was subjected to performance tests such as shear strength test at the bond joint (including normal state, after IR3, and after IR6) and air tightness test. The test results are shown in Table 2 below.
[0120] The test method for the shear strength test at the joint is as follows: the joint material is stretched up and down using a universal tensile testing machine, and the shear strength at which the material detaches from the joint is calculated based on the area of the joint.
[0121] The method for testing the shear strength of the joint after IR3 is as follows: After the prepared bonding material is placed in the reflow oven and run 3 times, the shear force of the joint is tested again.
[0122] The method for testing the shear strength of the joint after IR6 is as follows: After the prepared bonding material is placed in the reflow oven and run 6 times, the shear force of the joint is tested again.
[0123] The airtightness test method is as follows: a helium mass spectrometer leak detector is used for testing.
[0124] Table 2. Test results of shear strength and airtightness of the combined materials.
[0125] Shear strength airtightness IR3 shear strength IR6 shear strength Example 1 <![CDATA[>30N / mm 2 ]]> <![CDATA[<5×10 -8 Pa·m 3 / s]]> <![CDATA[>25N / mm 2 ]]> <![CDATA[>20N / mm 2 ]]> Example 2 <![CDATA[>30N / mm 2 ]]> <![CDATA[<5×10 -8 Pa·m 3 / s]]> <![CDATA[>25N / mm 2 ]]> <![CDATA[>20N / mm 2 ]]> Example 3 <![CDATA[>30N / mm 2 ]]> <![CDATA[<5×10 -8 Pa·m 3 / s]]> <![CDATA[>25N / mm 2 ]]> <![CDATA[>20N / mm 2 ]]> Comparative Example 1 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 ]]> Comparative Example 2 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 ]]> Comparative Example 3 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 ]]> Comparative Example 4 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 ]]> Comparative Example 5 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 <!-- 8 -->]]> Comparative Example 6 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 ]]> Comparative Example 7 <![CDATA[>20N / mm 2 ]]> <![CDATA[>5×10 -8 Pa·m 3 / s]]> <![CDATA[>15N / mm 2 ]]> <![CDATA[>10N / mm 2 ]]>
[0126] As shown in Table 2, the processed copper material formed by surface treatment of the copper-containing materials in Examples 1 to 3 and the resulting bond material by resin injection molding have better performance in terms of shear strength and air tightness compared with Comparative Examples 1 to 7.
[0127] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0128] The above embodiments merely illustrate several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the inventive concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A surface treatment method for copper-containing materials, characterized in that, Includes the following steps: A copper-containing material is placed in a film-forming composition and immersed for the first time to form an oxide film layer. The film-forming composition consists of potassium persulfate, sodium hydroxide, benzotriazole and water, wherein the mass fraction of potassium persulfate is 10%~12%, the mass fraction of sodium hydroxide is 8%~15%, the mass fraction of benzotriazole is 15%~20%, and the balance is water. The copper-containing material that has formed the oxide film layer is then placed in a hydrated hydrazine solution for a second immersion. The copper-containing material is selected from elemental copper or copper alloys.
2. The surface treatment method for copper-containing materials according to claim 1, characterized in that, The temperature for the first soaking is 50℃~80℃.
3. The surface treatment method for copper-containing materials according to claim 1, characterized in that, The first soaking time is 5 to 10 minutes.
4. The surface treatment method for copper-containing materials according to claim 1, characterized in that, The thickness of the oxide film is 500 nanometers to 3000 nanometers.
5. The surface treatment method for copper-containing materials according to claim 1, characterized in that, The hydrated hydrazine solution contains 3% to 10% hydrazine by mass.
6. The surface treatment method for copper-containing materials according to claim 1, characterized in that, The temperature for the second soaking is 50℃~70℃.
7. The surface treatment method for copper-containing materials according to claim 1, characterized in that, The second soaking time is 1 to 4 minutes.
8. A method for processing copper materials, characterized in that, It is obtained by the surface treatment method of the copper-containing material according to any one of claims 1 to 7.
9. A bonding material, characterized in that, It includes a resin and the processed copper material as described in claim 8, wherein the resin is bonded to the processed copper material by an injection molding process.
Citation Information
Patent Citations
Method of bonding copper and resin
US4642161A