A rare earth doped micro-nano laser enhanced by plasmon resonance and its construction method

Through surface plasmon resonance enhancement of rare earth doped micro-nano lasers, combined with high-quality resonance cavity, the problem of micro-nano lasers being strictly restricted on pump light sources and environment is solved, and a continuous optical pump laser output with low threshold value at room temperature is achieved. Improves the efficiency and stability of micro-nano lasers.

CN118198845BActive Publication Date: 2024-11-15HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410365577.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-15
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

The existing micro-nano lasers are harsh on pump light sources and operating environments, limiting their applications in high-density photoelectric integration and biological cell sensing, especially traditional gain dielectric materials fail due to high-power photoquenching and photobleaching. Moreover, rare earth doping gain media have problems such as narrow intrinsic absorption cross-section, low ion doping concentration and low luminescent quantum yield.

Method used

The surface plasmon resonance enhancement of rare earth doped micro-nano laser is used to enhance the energy absorption and reflection of light waves on the surface of gold nanoparticles, combined with high-quality resonance cavity, and achieve efficient absorption and luminescence of rare earth ions, lower the laser pumping threshold, and By adjusting the coupling strength and resonant cavity mode of nanocrystals and gold nanoparticles, the coupling efficiency of optical microcavities is improved.

Benefits of technology

The continuous optical pump laser output with a low threshold at room temperature is realized, which reduces the size and threshold of the laser, improves the efficiency and stability of the micro-nano laser, and is suitable for the field of micro-nano lasers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118198845B_ABST
    Figure CN118198845B_ABST
Patent Text Reader

Abstract

A rare earth doped micro-nano laser enhanced by plasma excitation resonance and a construction method thereof, which relates to a micro-nano laser and a construction method thereof. It aims to solve the problem that the existing micro-nano laser has strict restrictions on the pump light source and the operating environment. The micro-nano laser of the present invention is based on β-NaYF 4 :20Yb,2Er@NaYF 4 A micro-nano laser with nanocrystals and polyethyleneimine-modified nanogold particles as gain media, polystyrene microspheres as resonant cavities, and gain media loaded on the surface of polystyrene microspheres; preparation method: first prepare nanocrystals and remove oleic acid ligands, then couple nanocrystals and nanogold particles with a whispering gallery resonant cavity to obtain a micro-nano laser. It controls the energy transfer pathway through cross-relaxation of activator ions to achieve energy enrichment at 551nm, and achieves low-threshold laser output through the resonance of the resonant cavity, which can be used in chip optical interconnection, integrated optical circuits, micro devices, chemical detection and biosensing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plasma excitation resonance enhanced rare earth doped micro-nano laser and a construction method thereof. Background Art

[0002] Micro-nano lasers have broad application prospects in many fields such as high-density optoelectronic integration and biological cell sensing. These emerging applications have put forward new requirements for the size, threshold and pumping environment of micro-nano lasers. However, as the size of the laser decreases, its pumping threshold will increase exponentially, resulting in a very serious accumulation of thermal effects, causing traditional gain medium materials to fail due to high-power light quenching and photobleaching. At present, the reported micro-nano lasers generally use pulsed light pumping in a low-temperature operating environment to avoid thermal damage, but this harsh condition severely limits the development and application of micro-nano lasers. Therefore, it is urgent to develop a new method to enhance the luminescence of the gain medium through plasmon resonance and efficiently couple with the resonant cavity, so as to construct a room temperature continuous light pumped low-threshold micro-nano laser.

[0003] Compared with traditional gain medium materials (inorganic quantum dots, organic dyes, semiconductor materials, etc.), rare earth-doped gain medium has many advantages such as a wide luminescence range, unique photostability, and a long fluorescence lifetime. It is a new type of gain medium material with superior performance. However, rare earth ions have problems such as narrow intrinsic absorption cross-section, low ion doping concentration, and low luminescence quantum yield. The present application uses surface plasmon resonance to overcome the challenges of rare earth-doped gain media. When the pump light is irradiated to the surface of gold nanoparticles, the interaction between the light wave and the plasma wave causes the energy of the light wave to be absorbed or reflected. This leads to an enhancement of the local electromagnetic field around the metal nanoparticles, which greatly improves the absorption efficiency of the photons by the adjacent rare earth ions and enhances the luminescence. Combined with a high-quality resonant cavity, stimulated radiation can occur and a high-quality laser signal can be output. For example, in the article "Ultralow-threshold, continuous-wave upconverting lasing from subwavelength plasmons" on pages 1172-1176 of Nature Materials, issue 18 of 2019, Fernandez-Bravo et al. designed an ultra-stable directional emission plasma nanoarray upconversion laser. Rare earth-doped nanoparticles (~14nm) were deposited on the surface of the plasma nanoarray for microcavity resonance to prepare a laser with an ultra-low threshold of 70W / cm 2Continuous-wave upconversion lasers (one order of magnitude lower than other small lasers). However, the size of the silver nanorod arrays reaches several hundred micrometers or even larger and is confined to the substrate. Similarly, in the article "Self-Sufficient and Highly Efficient Gold Sandwich Upconversion Nanocomposite Lasers for Stretchable and Bio-applications" on pages 19840-19854 of the 12th volume, issue 17, 2020 of *ACS Applied Materials & Interfaces*, Chen et al. proposed a new laser emission scheme using gold sandwich upconversion nanocomposites (Au-UCNP-Au) with an ultra-low threshold under 980 nm continuous-wave excitation. The electromagnetic hotspots based on local surface plasmon resonance and the enhanced scattering coefficient facilitate the formation of a coherent closed loop through multiple scattering, which is the reason for the generation of stimulated emission at 545 nm. Due to the unique light-trapping structure, random lasing action was observed at an extremely low threshold (~0.06 kW / cm 2 ), but the random laser modes and output directions are difficult to control. SUMMARY OF THE INVENTION

[0004] The present invention aims to solve the technical problem of the harsh restrictions of existing micro-nano lasers on pump light sources and operating environments, and provides a plasmon resonance-enhanced rare-earth-doped micro-nano laser and a method for constructing the same.

[0005] The plasmon resonance-enhanced rare-earth-doped micro-nano laser of the present invention is a micro-nano laser with β-NaYF4:Yb,Er@NaYF4 nanocrystals and polyethyleneimine-modified gold nanoparticles (PEI-AuNPs) as the gain medium and polystyrene microspheres as the resonant cavity; the gain medium is loaded on the surface of the polystyrene microspheres; the chemical general formula of the β-NaYF4:Yb,Er@NaYF4 nanocrystals is NaY (0.8-x) F4:0.2Yb,xEr@NaYF4, 0 < x ≤ 0.08; the size of the PEI-AuNPs is 50-70 nm.

[0006] Furthermore, the chemical general formula of the β-NaYF4:Yb,Er@NaYF4 nanocrystals is NaY (0.8-x) F4:0.2Yb,xEr@NaYF4, 0.005 ≤ x ≤ 0.040.

[0007] Furthermore, the thickness of the inert NaYF4 shell of the β-NaYF4:Yb,Er@NaYF4 nanocrystal is 1 to 6 nm.

[0008] Furthermore, the gain medium loaded on the surface of the polystyrene microsphere is a single layer.

[0009] The rare earth doped micro-nano laser enhanced by plasmon resonance of the present invention has structural advantages. Firstly, β-NaYF4:Yb,Er@NaYF4 nanocrystals and PEI-AuNPs are selected as gain media. NaYF4 is a most common fluoride matrix material with low phonon energy (<400cm -1 ), low non-radiative relaxation and high radiative emission rate, as well as good physicochemical stability. The strong electromagnetic field of the plasmonic nanostructure can strongly enhance the multiphoton upconversion process. However, the surface plasmon resonance of a single nanoparticle usually has a low mode quality. Due to internal energy transfer, the overlapping energy spectrum of UCNPs and multiple narrow bands lead to a decrease in the output efficiency of a single target mode. Microspherical whispering gallery modes (WGM) resonators have both the stability of Fabry-Perot microcavities and the high quality factor of plasmonic elementary resonance microcavities. They can enhance the light absorption in different spectral ranges by regulating a variety of resonance modes, thereby achieving the capture and enhancement of light emission at a specific wavelength or a wide spectral range. The composite of PEI-AuNPs and β-NaYF4:Yb,Er@NaYF4 nanocrystals with WGM microcavities can achieve their efficient coupling in optical microcavities and emit lasers.

[0010] The micro-nano laser enhanced by the plasma excitation resonance of the present invention has the advantages in principle. By adjusting the rare earth ion Er in β-NaYF4:Yb,Er@NaYF4 3+ The concentration of the nanoparticles can be cross-relaxed to control the enrichment of particles at a specific energy level, achieving a population inversion. Surface plasmon resonance enhanced upconversion luminescence is one of the most effective methods. By changing the thickness of the inert shell of the coated NaYF4, the coupling strength between the nanocrystals and PEI-AuNPs can be adjusted. The micro-nano optical resonant cavity is the key to achieving stimulated radiation amplification. Polystyrene microspheres are selected as the resonant cavity. The microcavity size, material refractive index, surface state and other factors have an extremely good effect on the evanescent field and resonant cavity mode, which is very consistent with the rare earth doped gain medium.

[0011] First, the activator ion Er in the nanocrystal is 3+ Concentration regulation to achieve 4 S 3 / 2The energy at the luminescent energy level is transiently enriched, and the number of particles at a specific energy level is inverted under low-power pumping. Gold nanoparticles can absorb the light emitted by nanocrystals, produce plasma exciton resonance enhancement, and couple the two with the optical microcavity to minimize scattering, collection and other losses, reduce the laser pumping threshold, and achieve continuous light-pumped laser output on a micro-nano scale.

[0012] By coupling highly efficient rare earth doped nanocrystals and PEI-AuNPs with a whispering gallery resonator, the present invention designs a highly efficient micro-nano laser enhanced by continuous light pumping at room temperature and plasma exciton resonance. This new type of micro-nano laser has a small size and a low threshold, and can achieve highly efficient laser output at room temperature. The invention provides a feasible method for reducing the threshold of micro-nano lasers and provides a new idea for the construction of highly efficient micro-nano lasers.

[0013] The preparation method of the above-mentioned rare earth doped micro-nano laser enhanced by plasmon resonance is carried out according to the following steps:

[0014] 1. Preparation of β-NaYF4:Yb,Er nanocrystals by coprecipitation method; the general chemical formula of β-NaYF4:Yb,Er nanocrystals is NaY (0.8-x) F4:0.2Yb,xEr@NaYF4,0 <x≤0.08;

[0015] Second, the NaYF4 inert shell layer was coated on β-NaYF4:Yb,Er nanocrystals by hot injection method to obtain β-NaYF4:Yb,Er@NaYF4 nanocrystals;

[0016] 3. Removal of oleic acid ligands on the surface of β-NaYF4:Yb,Er@NaYF4 nanocrystals;

[0017] 4. PEI-AuNPs with a particle size of 40 to 70 nm and β-NaYF4:Yb,Er@NaYF4 nanocrystals with oleic acid ligand removed are used as gain media to couple with polystyrene microspheres in a whispering gallery resonator to obtain a micro-nano laser enhanced by plasmon resonance.

[0018] Furthermore, the preparation method of β-NaYF4:Yb,Er nanocrystals described in step 1 is carried out according to the following steps:

[0019] (1) First, press NaY (0.8-x)F4: 0.2Yb,xEr@NaYF4, with a stoichiometric ratio of 0 < x ≤ 0.08, weigh YCl3·6H2O, YbCl3·6H2O, and ErCl3·6H2O as raw materials. Then add oleic acid and 1-octadecene, purge with argon to remove oxygen, stir and heat the reaction solution to 120 - 160 °C and hold for 20 - 40 minutes to fully dissolve and mix the raw materials and remove moisture; at room temperature, add a methanol solution containing NaOH and NH4F, and continue to stir for 20 - 40 minutes;

[0020] (2) Heat the solution to 80 - 100 °C and hold for 20 - 40 minutes; remove methanol, then raise the temperature to 290 - 310 °C and hold for 0.5 - 1 hour, then stop the reaction and cool to room temperature;

[0021] (3) Add ethanol to the reaction solution, centrifuge at a speed of 6000 - 9000 rpm for 5 - 10 minutes to collect the product; purify the product with ethanol 2 - 3 times, and then disperse it in cyclohexane to obtain a cyclohexane dispersion of β-NaYF4:Yb,Er nanocrystals.

[0022] Furthermore, in step one (1), the ratio of the total amount of substance of YCl3·6H2O, YbCl3·6H2O, and ErCl3·6H2O to the volume of oleic acid is 1 mmol : (5 - 8) mL.

[0023] Furthermore, in step one (1), the ratio of the total amount of substance of YCl3·6H2O, YbCl3·6H2O, and ErCl3·6H2O to the volume of 1-octadecene is 1 mmol : (15 - 20) mL.

[0024] Furthermore, in step one (1), the ratio of the total amount of substance of YCl3·6H2O, YbCl3·6H2O, and ErCl3·6H2O to the amount of substance of NaOH in the methanol solution is 1 : (2 - 3).

[0025] Furthermore, in step one (1), the ratio of the total amount of substance of YCl3·6H2O, YbCl3·6H2O, and ErCl3·6H2O to the amount of substance of NH4F in the methanol solution is 1 : (3.2 - 5).

[0026] Furthermore, the preparation method of the β-NaYF4:Yb,Er@NaYF4 nanocrystals described in step two is carried out according to the following steps:

[0027] (1) YCl3·6H2O, NaOH and NH4F are weighed as raw materials according to the stoichiometric ratio of NaYF4, YCl3·6H2O is added to oleic acid and 1-octadecene, argon is passed to remove oxygen, the reaction solution is stirred and heated to 120-160°C for 20-40 minutes to fully dissolve and mix the raw materials, and water is removed to obtain a YCl3 solution; NaOH and NH4F are dissolved in methanol, and the methanol solution containing NaOH and NH4F is added to the YCl3 solution at room temperature, and stirring is continued for 20-40 minutes. The resulting solution is cooled to room temperature to serve as a precursor;

[0028] (2) adding a mixed solution of oleic acid and 1-octadecene to a cyclohexane dispersion of β-NaYF4:Yb,Er nanocrystals, passing argon to remove oxygen, stirring and heating the reaction solution to 160-165° C. for 20-40 minutes to fully disperse the raw materials and remove moisture; continuing to heat the reaction solution to 285-305° C., and then injecting a precursor into the reaction solution. Depending on the thickness of the shell layer, the number of times the precursor is added is 1-5 times, and each time the precursor is added, it is aged for 6-9 minutes. After the aging is completed, the reaction is stopped and cooled to room temperature;

[0029] (3) adding ethanol to the reaction solution, and collecting the product by centrifugation at 6000-9000 rpm for 5-10 min; the product is purified 2-3 times with ethanol, and then dispersed in cyclohexane to obtain a cyclohexane dispersion of β-NaYF4:Yb,Er@NaYF4 nanocrystals.

[0030] Furthermore, in step 2 (2), the ratio of the amount of β-NaYF4:Yb,Er nanocrystals in the cyclohexane dispersion of β-NaYF4:Yb,Er nanocrystals to the volume of oleic acid is 1 mmol:(10-14) mL;

[0031] Furthermore, in step 2 (2), the ratio of the amount of β-NaYF4:Yb,Er nanocrystals in the cyclohexane dispersion of β-NaYF4:Yb,Er nanocrystals to the volume of octadecene is 1 mmol:(28-30) mL;

[0032] Furthermore, in step 2 (2), when hot-injecting the shell, the amount of injection will cause the reaction solution to produce temperature fluctuations. Larger temperature fluctuations will make the morphology of the nanocrystals uneven, so the amount of precursor solution injected each time is 0.6% to 10% of the reaction solution. According to Ostwald ripening, as the nanocrystals grow, the growth accelerates, and the injection amount needs to be increased and the injection time is shortened to 6 to 9 minutes. If the ripening time is too short, the crystal growth will be incomplete, and if the time is too long, the nanocrystals will tend to grow into rods.

[0033] Furthermore, the thickness of the nanocrystal inert shell is 1 to 6 nm. The thickness of the nanocrystal inert shell will affect the coupling strength of the plasmon resonance of the remaining gold nanoparticles. The strongest coupling cannot be achieved when the luminescent center of the nanocrystal is too far or too close to the gold nanoparticle. By controlling the thickness of the inert shell to 2 to 4 nm, the optimal resonance distance is achieved.

[0034] Furthermore, the method for removing the oleic acid ligand on the surface of the gain medium β-NaYF4:Yb,Er@NaYF4 nanocrystal described in step 3 is carried out according to the following steps:

[0035] (1) According to the mass ratio of nitrosotetrafluoroborate (NOBF4) to volume of N-dimethylformamide (DMF) of 1 mg: (0.13-0.2) mL, NOBF4 was dissolved in DMF, and ultrasonicated for 2 minutes to completely dissolve it, thereby obtaining a mixed solution of NOBF4 and DMF;

[0036] (2) A mixed solution of NOBF4 and DMF, a cyclohexane dispersion of β-NaYF4:Yb,Er@NaYF4 nanocrystals and N-N-dimethylformamide were mixed, and the mixture was shaken for 8 to 12 minutes to remove the oleic acid ligands on the surface of β-NaYF4:Yb,Er@NaYF4 nanocrystals. Cyclohexane and toluene were then added, and the mixture was allowed to stand for 15 to 25 minutes. The mixture was centrifuged at 8000 to 10000 rpm for 8 to 10 minutes, and the β-NaYF4:Yb,Er@NaYF4 nanocrystals after the ligands were eliminated were collected and dispersed in DMF to obtain a dispersion of β-NaYF4:Yb,Er@NaYF4 nanocrystals after the ligands were eliminated.

[0037] Furthermore, the NOBF4 concentration in the NOBF4 and DMF mixed solution described in step three (1) is 0.02-0.03M; if the amount of NOBF4 added is too little, the surface ligands of the nanoparticles will not be completely removed, and some oleic acid molecules will adhere to the surface of the nanoparticles, making the nanoparticles partially hydrophobic; if the amount of NOBF4 added is too much, the oleic acid molecules on the surface of the nanoparticles will be completely removed, but the excess NOBF4 will etch the surface of the nanoparticles, affecting the lattice of the nanoparticles, thereby causing a decrease in luminescence performance.

[0038] Furthermore, the ratio of the volume of the NOBF4 and DMF mixed solution described in step 3 (2) to the volume of the cyclohexane dispersion of β-NaYF4:Yb,Er@NaYF4 nanocrystals is 1:(4-6);

[0039] Furthermore, the method for preparing a rare earth doped micro-nano laser by coupling the gain medium with a whispering gallery resonant cavity described in step 4 is carried out according to the following steps:

[0040] (1) First, 3 to 10 μL of polystyrene microspheres with a solid content of 10% were dispersed in 500 to 2000 μL of deionized water (DI) and ultrasonicated for 5 minutes, and then 5 to 8 μL of β-NaYF4:Yb,Er@NaYF4 nanocrystal dispersion with a concentration of 6 to 8 mg / mL and 100 μL of PEI-AuNPs dispersion with a concentration of 0.05 to 0.08 mg / mL were added, and mixed evenly to obtain a mixed solution; wherein the particle size of PEI-AuNPs in the PEI-AuNPs dispersion was 50 to 70 nm;

[0041] (2) The mixed solution is shaken in a constant temperature shaking box at 25°C at a speed of 500-800 rpm for 1-3 hours. The positively charged β-NaYF4:Yb,Er@NaYF4 nanocrystals and PEI-AuNPs are adsorbed on the surface of the negatively charged polystyrene microspheres under the action of electrostatic force and self-assembled into a homogeneous film layer. Among them, the shaking rate and time will strongly affect the loading amount and loading state of rare earth-doped nanoparticles and PEI-AuNPs on the surface of polystyrene microspheres. Shaking at a speed of 500-800 rpm for 1-3 hours can form a monolayer load without agglomeration of nanoparticles.

[0042] (3) The product is collected by centrifugation at 4000-6000 rpm for 5 minutes, and then washed with ethanol and water for 2-3 times to remove excess rare earth doped nanoparticles and PEI-AuNPs, thereby obtaining a rare earth doped micro-nano laser enhanced by plasmon resonance. The rare earth doped micro-nano laser enhanced by plasmon resonance is dispersed in water or ethanol for later use.

[0043] In the rare earth doped micro-nano laser prepared by coupling the gain medium with the whispering gallery resonant cavity, the rare earth doped nanoparticles and PEI-AuNPs are uniformly wrapped on the surface of the microspheres, and the coupled microspheres are redispersed in water or ethanol for further use. By adjusting the concentration ratio of the microsphere resonant cavity and the rare earth doped nanoparticles, the surface state and thickness of the load layer can be precisely controlled. If the number of adsorbed nanoparticles is too large, the nanoparticles will agglomerate on the surface of the microsphere to form multilayer nanoparticles, and the surface is relatively rough overall; if the number of adsorbed nanoparticles is too small, the surface of the resonant cavity will not be completely covered by nanoparticles, affecting the coupling effect, and both will affect the propagation and loss of light in the resonant cavity through scattering and reflection; by adjusting the concentration ratio of the microsphere resonant cavity and PEI-AuNPs, the loading amount of PEI-AuNPs can be accurately controlled. If the PEI-AuNPs loading is too small, only a small part of the nanocrystals can produce plasma excitation resonance enhancement with PEI-AuNPs, and if the loading is too large, the luminescent center is reduced, the luminescent intensity is reduced, or agglomeration occurs on the surface of the microsphere, making the surface relatively rough. The concentration ratio of the microsphere resonant cavity, rare earth-doped nanoparticles and PEI-AuNPs defined in the present invention can obtain a gain medium layer with a single layer loading and non-agglomerated nanoparticles, produce plasma excitation resonance enhancement, and reduce the threshold of the rare earth-doped micro-nano laser.

[0044] The rare earth doped micro-nano laser enhanced by plasma excitation resonance of the present invention, the Er in the nanocrystal loaded by the micro-nano laser 3+ It plays the role of laser output and generates localized plasma exciton resonance with PEI-AuNPs to generate enhanced luminescence. The micro-nano laser can control the energy transfer pathway by cross-relaxation of the activator ions to achieve energy enrichment at 551nm, and achieve the purpose of low-threshold laser output through the resonance of the polystyrene microsphere resonator. The rare earth doped micro-nano laser of the present invention can be used in the field of micro-nano lasers. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The β-NaY obtained in step 1 of Example 1 0.78 F4: Transmission electron microscope photo of 0.2Yb, 0.02Er nanocrystals;

[0046] Figure 2 The β-NaY obtained in step 2 of Example 1 0.78 F4: Transmission electron micrograph of 0.2Yb, 0.02Er@NaYF4 nanocrystals;

[0047] Figure 3 The ligand-eliminated β-NaY obtained in step 3 in Example 1 0.78 F4: Transmission electron microscopy image of 0.2Yb,0.02Er@NaYF4 nanoparticles;

[0048] Figure 4 is a transmission electron microscopy photograph of PEI-AuNPs in step 3 of Example 1;

[0049] Figure 5 is a scanning electron microscope photograph of the rare earth doped micro-nano laser enhanced by plasmon resonance obtained in step 4 in Example 1;

[0050] Figure 6 β-NaY prepared in step 2 of Example 1 0.78 F4: Emission spectrum of 0.2Yb, 0.02Er@NaYF4 nanocrystals under 980nm laser excitation;

[0051] Figure 7 This is the laser output spectrum of the plasma resonance enhanced micro-nano laser obtained in Example 1.

[0052] Figure 8 This is a scanning electron microscope photograph of the plasma resonance enhanced micro-nano laser obtained in step 4 in Example 2.

[0053] Fig. 9 This is the laser output spectrum of the plasma resonance enhanced micro-nano laser obtained in Example 2. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and examples, but the present invention is not limited to the scope of the examples.

[0055] Embodiment 1: The method for constructing the rare earth doped micro-nano laser enhanced by plasma resonance of this embodiment is carried out according to the following steps:

[0056] 1. Preparation of β-NaY 0.78 F4: 0.2Yb, 0.02Er nanocrystals:

[0057] (1) First, press β-NaY 0.78 F4: 0.2Yb, 0.02Er stoichiometric ratio: 0.78mmol YCl3·6H2O, 0.2mmol YbCl3·6H2O and 0.02mmol ErCl3·6H2O were weighed as raw materials, and the raw materials were added into a 50mL three-necked flask containing 6mL oleic acid and 15mL 1-octadecene, and the reaction solution was heated to 160°C for 30 minutes to fully dissolve the chloride and remove the water; cooled to room temperature, 10mL methanol solution containing 2.5mmol NaOH and 4mmol NH4F was added to the reaction solution, and stirred for 30 minutes; in this step, methanol provides an effective solvent for the addition of NaOH and NH4F, which is removed in the subsequent synthesis step;

[0058] (2) heating the solution to 100°C and maintaining it for 30 minutes, then heating it to 300°C and maintaining it for 1 hour, stopping the reaction, and cooling it to room temperature;

[0059] (3) Add ethanol to the reaction solution, centrifuge at 6000 rpm for 5 minutes to collect the product, purify it with ethanol three times, and disperse the product in cyclohexane to obtain β-NaY 0.78 F4: 0.2Yb, 0.02Er nanocrystals in cyclohexane dispersion.

[0060] 2. Preparation of β-NaY 0.78 F4:0.2Yb,0.02Er@NaYF4 nanocrystals:

[0061] (1) 0.3034 g of YCl3·6H2O, 0.100 g of NaOH and 0.148 g of NH4F were weighed as raw materials, and YCl3·6H2O was added to 6 mL of oleic acid and 15 mL of 1-octadecene, and argon was passed to remove oxygen. The reaction solution was stirred and heated to 150°C for 30 minutes to fully dissolve and mix the raw materials, and the water was removed to obtain a YCl3 solution; NaOH and NH4F were dissolved in 10 mL of methanol, and the methanol solution containing NaOH and NH4F was added to the YCl3 solution at room temperature, and stirring was continued for 30 minutes. The resulting solution was cooled to room temperature to serve as a precursor;

[0062] (2) Take 0.5 mL of β-NaY prepared in step 1 0.78 F4: 0.2Yb, 0.02Er nanocrystal cyclohexane dispersion, add 4.3mL oleic acid and 10.7mL 1-octadecene mixed solution, pass argon to remove oxygen, stir the reaction solution and heat to 160°C for 30 minutes to fully disperse the raw materials and remove moisture; quickly heat to 300°C, according to the designed coating 2nm NaYF4, inject the precursor 4 times, the injection amount is 0.10mL, 0.25mL, 0.25mL, 0.40mL, the aging time is 8, 7, 7, 8 minutes, respectively, wait for the aging to be completed, stop the reaction, and cool to room temperature;

[0063] (3) Add ethanol to the reaction solution, centrifuge at 6000 rpm for 5 minutes to collect the product, purify it with ethanol three times, and disperse the product in cyclohexane to obtain β-NaY 0.78 F4: 0.2Yb, 0.02Er@NaYF4 nanocrystals in cyclohexane dispersion;

[0064] 3. Removal of β-NaY 0.78 F4:0.2Yb,0.02Er@NaYF4 surface oleic acid ligand:

[0065] (1) First, 0.013 g of nitrosotetrafluoroborate (NOBF4) was dissolved in 2.5 mL of N-dimethylformamide (DMF), and the mixture was completely dissolved by ultrasonication for 2 minutes to obtain a mixed solution of NOBF4 and DMF;

[0066] (2) Mix the NOBF4 and DMF solution, 2 mL of β-NaY 0.78 F4: 0.2Yb, 0.02Er@NaYF4 nanocrystal cyclohexane dispersion was mixed with 2.5mL DMF, shaken for 10 minutes to remove the oleic acid ligand on the surface of the nanocrystal, 10mL cyclohexane and 10mL toluene were added, and the mixture was allowed to stand for 20 minutes. The nanoparticles after ligand elimination were collected by centrifugation at 10000rpm for 10 minutes, and then dispersed in DMF to obtain β-NaY 0.78 F4: 0.2Yb, 0.02Er@NaYF4 nanoparticle dispersion;

[0067] 4. Preparation of rare earth doped micro-nano laser by coupling gain medium with whispering gallery resonator:

[0068] (1) First, 10 μL of polystyrene microspheres with a solid content of 10% were dispersed in 1000 μL of deionized water and ultrasonicated for 5 minutes, and then 7 μL of β-NaY 0.78 F4: 0.2Yb, 0.02Er@NaYF4 nanoparticle dispersion and 100uL of 0.05mg / mL PEI-AuNPs dispersion with a particle size of 60nm to obtain a mixed solution;

[0069] (2) The mixed solution was shaken at 750 rpm for 2 h at 25 °C in a constant temperature shaker, and the positively charged β-NaYF4:Yb,Er@NaYF4 nanocrystals and PEI-AuNPs were assembled and adsorbed on the negatively charged surface of the polystyrene microspheres in the microsphere resonator cavity through electrostatic force;

[0070] (3) The product was collected by centrifugation at 5000 rpm for 5 minutes, and then washed with ethanol and water for 3 times to remove excess rare earth doped nanoparticles and PEI-AuNPs, thereby obtaining a rare earth doped micro-nano laser enhanced by plasmon resonance. The rare earth doped micro-nano laser enhanced by plasmon resonance was dispersed in water for later use.

[0071] β-NaY prepared in step 1 of this embodiment 0.78 F4: Transmission electron microscope photo of 0.2Yb, 0.02Er nanocrystals Figure 1 As shown, the β-NaY prepared in step 2 0.78 Transmission electron microscope photo of F4:0.2Yb,0.02Er@NaYF4 nanocrystals Figure 2 As shown, the β-NaY obtained by step 3 to eliminate the ligand 0.78 F4: 0.2Yb, 0.02Er@NaYF4 nanoparticles transmission electron microscope photos Figure 3 As shown, the transmission electron micrograph of the purchased 60nm PEI-AuNPs is shown in Figure 4 As shown, the scanning electron microscope photo of the rare earth doped micro-nano laser enhanced by plasmon resonance obtained in step 4 is shown in Figure 5 As shown. Figures 1 to 3 It can be seen that the β-NaY synthesized in this example 0.78 F4:0.2Yb,0.02Er@NaYF4 nanocrystals are uniform hexagonal nanoparticles with a size of 26nm, and the particle size does not change significantly after removing the surface ligands; the rare earth doped micro-nano laser enhanced by plasmon resonance is a single-layer self-assembled β-NaY 0.78 F4: polystyrene microcavity with 0.2Yb, 0.02Er@NaYF4 nanocrystals and 60nm PEI-AuNPs gain medium. The diameter of the polystyrene microspheres is 5μm, and the nanoparticles are loaded as a single layer on the surface of the resonant cavity. The nanoparticles do not agglomerate.

[0072] β-NaY prepared in step 2 of this embodiment 1 0.78 The emission spectrum of F4:0.2Yb,0.02Er@NaYF4 nanocrystals is shown in the figure. Figure 6 It can be seen that the nanoparticles emit fluorescence signals in multiple wavelengths, and the emission wavelengths are mainly located at 523nm, 551nm and 660nm. 3+ β-NaY with 2% content 0.78 F4:0.2Yb,0.02Er@NaYF4 nanocrystals have the highest fluorescence emission intensity at 551nm.

[0073] The laser output spectrum of the rare earth doped micro-nano laser enhanced by plasmon resonance obtained in step 4 of this embodiment 1 is as follows: Figure 7 As shown, the micro-nano laser has multi-mode laser output, realizing the construction of room temperature, continuous light pumped low threshold rare earth doped micro-nano laser.

[0074] Embodiment 2: The method for constructing the rare earth doped micro-nano laser enhanced by plasmon resonance of this embodiment is carried out according to the following steps:

[0075] 1. Preparation of β-NaY 0.78 F4: 0.2Yb, 0.02Er nanocrystals, the steps and parameters are the same as those in Example 1;

[0076] 2. Preparation of β-NaY 0.78F4: 0.2Yb, 0.02Er@NaYF4 nanocrystals: the steps and parameters are the same as those in Example 1;

[0077] 3. Removal of β-NaY 0.78 F4: 0.2Yb, 0.02Er@NaYF4 surface oleic acid ligand, the steps and parameters are the same as those in Example 1;

[0078] 4. Preparation of rare earth doped micro-nano laser by coupling gain medium with whispering gallery resonator:

[0079] (1) First, 10 μL of polystyrene microspheres with a solid content of 10% were dispersed in 1000 μL of deionized water and ultrasonicated for 5 minutes, and then 7 μL of β-NaY 0.78 F4: 0.2Yb, 0.02Er@NaYF4 nanoparticle dispersion and 200uL 0.05mg / mL PEI-AuNPs dispersion with a particle size of 60nm to obtain a mixed solution;

[0080] (2) The mixed solution was shaken at 500 rpm for 4 h at 25 °C in a constant temperature shaker, and the positively charged β-NaYF4:Yb,Er@NaYF4 nanocrystals and 60 nm PEI-AuNPs were assembled and adsorbed on the negatively charged surface of the microsphere resonant cavity polystyrene microspheres through electrostatic force;

[0081] (3) The product was collected by centrifugation at 6000 rpm for 5 minutes, and then washed with ethanol and water for 3 times respectively to remove excess rare earth doped nanoparticles and PEI-AuNPs, thereby obtaining a rare earth doped micro-nano laser enhanced by plasmon resonance. The rare earth doped micro-nano laser enhanced by plasmon resonance is a microsphere resonator after loading a gain medium, and the rare earth doped micro-nano laser enhanced by plasmon resonance is redispersed in water.

[0082] The scanning electron microscope photo of the rare earth doped micro-nano laser enhanced by plasmon resonance obtained in step 4 of this embodiment 2 is shown in FIG8. Figure 8 It can be seen that rare earth-doped nanoparticles and 60nm PEI-AuNPs gain medium particles are wrapped on the surface of the microspheres. The nanoparticles are evenly loaded on the surface of the resonant cavity and can be well coupled with the resonant cavity, thus forming a high-efficiency micro-nano laser.

[0083] The laser output spectrum of the rare earth doped micro-nano laser enhanced by plasmon resonance obtained in step 4 of this embodiment 2 is as follows: Fig. 9 As shown, from Fig. 9 It can be seen that the micro-nano laser has multi-mode laser output, realizing the construction of room temperature, continuous light pumped low threshold rare earth doped micro-nano laser.

Claims

1. A rare earth doped micro-nano laser enhanced by plasmon resonance, characterized in that: The laser is a micro-nano laser with β-NaYF4:Yb,Er@NaYF4 nanocrystals and polyethyleneimine-modified gold nanoparticles as the gain medium and polystyrene microspheres as the resonant cavity; the gain medium is loaded on the surface of the polystyrene microspheres; the chemical general formula of the β-NaYF4:Yb,Er@NaYF4 nanocrystals is NaY (0.8-x) F4:0.2Yb,xEr@NaYF4, where 0 < x ≤ 0.08; the size of the PEI-AuNPs is 50 - 70 nm.

2. The rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 1, characterized in that: The general chemical formula of β-NaYF4:Yb,Er@NaYF4 nanocrystals is NaY (0.8-x) F4:0.2Yb,xEr@NaYF4, 0.005≤x≤0.

04.

3. The rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 1 or 2, characterized in that: The thickness of the inert NaYF4 shell of β-NaYF4:Yb,Er@NaYF4 nanocrystals is 1 to 6 nm.

4. The rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 1 or 2, characterized in that: The gain medium is loaded on the surface of polystyrene microspheres in the form of a monolayer.

5. A method for preparing a rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 1, characterized in that: The method proceeds as follows:

1. Preparation of β-NaYF4:Yb,Er nanocrystals by coprecipitation method; the general chemical formula of β-NaYF4:Yb,Er nanocrystals is NaY (0.8-x) F4:0.2Yb,xEr,0 <x≤0.08; Second, the NaYF4 inert shell layer was coated on the β-NaYF4:Yb,Er nanocrystals by hot injection method to obtain β-NaYF4:Yb,Er@NaYF4 nanocrystals; 3. Removal of oleic acid ligands on the surface of β-NaYF4:Yb,Er@NaYF4 nanocrystals; 4. PEI-AuNPs with a particle size of 40 to 70 nm and β-NaYF4:Yb,Er@NaYF4 nanocrystals with oleic acid ligand removed are used as gain media to couple with polystyrene microspheres in a whispering gallery resonator to obtain a micro-nano laser enhanced by plasmon resonance.

6. The method for preparing a rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 5, characterized in that: The preparation method of β-NaYF4:Yb,Er nanocrystals described in step 1 is carried out according to the following steps: (1) First, according to the stoichiometric ratio of NaY (0.8-x) F4:0.2Yb,xEr, where 0 < x ≤ 0.08, weigh YCl3·6H2O, YbCl3·6H2O and ErCl3·6H2O as raw materials. Then add oleic acid and 1-octadecene, purge with argon to remove oxygen, stir and heat the reaction solution to 120 - 160 °C and keep it for 20 - 40 minutes to fully dissolve and mix the raw materials and remove moisture; add a methanol solution containing NaOH and NH4F at room temperature and continue stirring for 20 - 40 minutes; (2) heating the solution to 80-100°C and maintaining it for 20-40 minutes; removing methanol, then heating it to 290-310°C and maintaining it for 0.5-1 hour, stopping the reaction, and cooling it to room temperature; (3) adding ethanol to the reaction solution, and collecting the product by centrifugation at a speed of 6000-9000 rpm for 5-10 min; the product is purified 2-3 times with ethanol, and then dispersed in cyclohexane to obtain a cyclohexane dispersion of β-NaYF4:Yb,Er nanocrystals.

7. The method for preparing a rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 5 or 6, characterized in that: The preparation method of β-NaYF4:Yb,Er@NaYF4 nanocrystals described in step 2 is carried out according to the following steps: (1) YCl3·6H2O, NaOH and NH4F are weighed as raw materials according to the stoichiometric amount of NaYF4, YCl3·6H2O is added to oleic acid and 1-octadecene, argon is passed to remove oxygen, the reaction solution is stirred and heated to 120-160°C for 20-40 minutes to fully dissolve the raw materials, and water is removed to obtain a YCl3 solution; NaOH and NH4F are dissolved in methanol, and the methanol solution containing NaOH and NH4F is added to the YCl3 solution at room temperature, and stirring is continued for 20-40 minutes. The resulting solution is cooled to room temperature to serve as a precursor; (2) adding a mixed solution of oleic acid and octadecene to the cyclohexane dispersion of β-NaYF4:Yb,Er nanocrystals prepared in step 1, passing argon to remove oxygen, stirring and heating the reaction solution to 160-165° C. for 20-40 minutes to fully disperse the raw materials and remove moisture; continuing to heat the reaction solution to 285-305° C., and then injecting the precursor into the reaction solution. The number of times the precursor is added is 1-5 times according to the thickness of the shell layer. After each addition of the precursor, ripening is carried out for 6-9 minutes. After the ripening is completed, the reaction is stopped and cooled to room temperature; (3) adding ethanol to the reaction solution, and collecting the product by centrifugation at 6000-9000 rpm for 5-10 min; the product is purified 2-3 times with ethanol, and then dispersed in cyclohexane to obtain a cyclohexane dispersion of β-NaYF4:Yb,Er@NaYF4 nanocrystals.

8. The method for preparing a rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 5 or 6, characterized in that: The method for removing the oleic acid ligand on the surface of β-NaYF4:Yb,Er@NaYF4 nanocrystals described in step 3 is carried out according to the following steps: (1) NOBF4 was dissolved in N-dimethylformamide at a ratio of 1 mg of nitrosoborate to (0.13-0.2) mL of N-dimethylformamide, and the mixture was completely dissolved by ultrasonication for 2 minutes to obtain a mixed solution of NOBF4 and DMF; (2) The mixed solution of NOBF4 and DMF, the cyclohexane dispersion of β-NaYF4:Yb,Er@NaYF4 nanocrystals and DMF were mixed, and the mixture was shaken for 8 to 12 minutes to remove the oleic acid ligands on the surface of β-NaYF4:Yb,Er@NaYF4 nanocrystals. Cyclohexane and toluene were then added, and the mixture was allowed to stand for 15 to 25 minutes. The mixture was centrifuged at 8000 to 10000 rpm for 8 to 10 minutes, and the β-NaYF4:Yb,Er@NaYF4 nanocrystals after the ligands were eliminated were collected and dispersed in DMF to obtain the β-NaYF4:Yb,Er@NaYF4 nanocrystal dispersion after the ligands were eliminated.

9. The method for preparing a rare earth doped micro-nano laser enhanced by plasmon resonance according to claim 5 or 6, characterized in that: The method for preparing a rare earth doped micro-nano laser by coupling the gain medium with a whispering gallery resonant cavity described in step 4 is carried out according to the following steps: (1) First, 3 to 10 μL of polystyrene microspheres with a solid content of 10% are dispersed in 500 to 2000 μL of deionized water and ultrasonicated for 5 minutes, and then 5 to 8 μL of β-NaYF4:Yb,Er@NaYF4 nanocrystal dispersion with a concentration of 6 to 8 mg / mL and 100 μL of PEI-AuNPs dispersion with a concentration of 0.05 to 0.08 mg / mL are added, and mixed evenly to obtain a mixed solution; wherein the particle size of PEI-AuNPs in the PEI-AuNPs dispersion is 50 to 70 nm; (2) The mixed solution was shaken in a constant temperature shaking box at 25°C at a speed of 500-800 rpm for 1-3 hours. The positively charged β-NaYF4:Yb,Er@NaYF4 nanocrystals and PEI-AuNPs were adsorbed on the surface of the negatively charged polystyrene microspheres under the action of electrostatic force and self-assembled into a homogeneous film layer. (3) The product was collected by centrifugation at 4000-6000 rpm for 5 minutes, and then washed with ethanol and water for 2-3 times to remove excess rare earth-doped nanoparticles and PEI-AuNPs, thereby obtaining a rare earth-doped micro-nano laser enhanced by plasmon resonance.