An iron-based catalyst, its preparation method and use

By preparing iron-based catalysts, the stability and cost issues in the preparation of slurry-bed hydrogenation catalysts were solved, achieving efficient lightening of heavy oil and removal of impurities, thereby improving catalytic activity.

CN118204082BActive Publication Date: 2026-11-10PETROCHINA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211620129.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2026-11-10
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

At present, the preparation process of slurry bed hydrogenation catalysts is hampered by unstable raw materials, high preparation costs, complex processes, and poor catalyst stability, resulting in low processing efficiency of heavy or inferior oils and making it difficult to achieve efficient lightweighting.

Method used

The preparation method of the iron-based catalyst includes a first calcination, alkali treatment, precipitation treatment and a second calcination of a mixed raw material system of silicon-containing compounds and iron-based compounds to form a metal-oxygen-iron coordination structure and improve catalytic activity.

Benefits of technology

It significantly improves the light conversion of heavy oil, reduces the content of sulfur, nitrogen, metals, asphaltenes and coke in the light conversion system, and improves the stability and catalytic activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application provides an iron-based catalyst and a preparation method and application thereof. The preparation method comprises the following steps: 1) performing first calcination treatment on a mixed raw material system comprising a silicon-containing compound and an iron-based compound to obtain a first calcination product; 2) performing alkali treatment on the first calcination product to obtain an alkali treatment product; 3) mixing the alkali treatment product, an aqueous solution of an auxiliary metal salt and an aqueous solution of a precipitant, and performing precipitation treatment on the mixed system to obtain a precipitation product; and 4) performing second calcination treatment on the precipitation product to obtain the iron-based catalyst. The alkali treatment comprises: performing water bath reaction of the first calcination product in an aqueous alkali solution, wherein the temperature of the water bath reaction is 40-95 DEG C, and the time is 0.5-4 h. The preparation method is simple and easy to operate, and the prepared iron-based catalyst has excellent catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a catalyst, and more particularly to an iron-based catalyst, its preparation method, and its application, belonging to the field of petrochemical technology. Background Technology

[0002] In recent years, with the increasing production of heavy or low-quality oils, their high viscosity and density, high carbon / hydrogen atom ratio, high heteroatom content, high metal content, and high gum / asphalt content have posed significant challenges to the development of petroleum processing. Hydrogenation technology, as an important means of processing heavy or low-quality oils, has received increasing attention and development.

[0003] A slurry bed reactor, also known as a suspended bed, is a reactor in which gas passes through a liquid (slurry) layer containing suspended solid particles in a bubbling manner to achieve a gas-liquid-solid reaction. It offers advantages such as strong feedstock adaptability, simple process, high feedstock oil conversion depth, and high light oil yield. Therefore, it is suitable for processing various heavy or low-quality oils, including those with high sulfur content, high carbon residue, high viscosity, high metal content, and high asphaltene content. In slurry bed hydrogenation processes, the slurry bed hydrogenation catalyst is the core technology, and its preparation method has become a focus of research and development.

[0004] At present, the preparation of slurry bed hydrogenation catalysts is generally hampered by problems such as unstable raw materials, high preparation costs, complex preparation processes, and processes that are not conducive to catalyst stability. Therefore, these problems not only hinder the improvement of catalyst activity, but also impede the efficient processing and utilization of heavy or low-quality oils, resulting in incalculable energy losses. Summary of the Invention

[0005] This invention provides a method for preparing an iron-based catalyst. The method is simple and easy to operate, and the prepared iron-based catalyst has excellent catalytic activity. It can significantly improve the conversion of heavy oil to lighter oil and reduce the content of sulfur, nitrogen, metals, asphaltenes and coke in the lighter oil system.

[0006] This invention provides an iron-based catalyst with excellent catalytic activity, which can significantly improve the light conversion of heavy oil and reduce the content of sulfur, nitrogen, metals, asphaltenes and coke in the light conversion system.

[0007] This invention provides a method for hydrogenating heavy oil, which can significantly improve the light conversion of heavy oil and reduce the content of sulfur, nitrogen, metals, asphaltenes and coke in the light conversion system.

[0008] This invention provides a method for preparing an iron-based catalyst, comprising the following steps:

[0009] 1) A mixed raw material system including silicon-containing compounds and iron-based compounds is subjected to a first calcination treatment to obtain a first calcination product;

[0010] 2) The first roasted product is subjected to alkali treatment to obtain an alkali-treated product;

[0011] 3) Mix the alkali-treated product, the aqueous solution of the auxiliary metal salt, and the aqueous solution of the precipitant, and perform precipitation treatment on the mixed system to obtain the precipitated product;

[0012] 4) The precipitated product is subjected to a second calcination treatment to obtain the iron-based catalyst;

[0013] The alkali treatment includes: subjecting the first calcined product to a water bath reaction in an alkaline aqueous solution, wherein the temperature of the water bath reaction is 40~95℃ and the time is 0.5~4h.

[0014] In the preparation method described above, in step 1), the molar ratio of silicon to iron in the mixed raw material system is (0.1~10):1.

[0015] In the preparation method described above, the mass ratio of the first calcined product to water in the alkaline aqueous solution is 1:(5~100), and the alkali concentration in the alkaline aqueous solution is 0.01~2 mol / L.

[0016] In the preparation method described above, the precipitation treatment is carried out at a temperature of 40~95℃ for a time of 1~24h.

[0017] In the preparation method described above, the molar ratio of metallic iron in the iron-based compound to the auxiliary metal in the aqueous solution of the auxiliary metal salt is 1:(0.1~20).

[0018] In the preparation method described above, the molar ratio of the precipitant to the total metal in the aqueous precipitant solution is (1~6):1, and the total metal includes the iron element in the iron-based compound and the auxiliary metal element in the aqueous solution of the auxiliary metal salt.

[0019] In the preparation method described above, the heating rate of the first calcination treatment is 3~10℃ / min, and the calcination temperature of the first calcination treatment is 200~800℃; and / or,

[0020] The heating rate of the second calcination treatment is 3~10℃ / min, and the calcination temperature of the second calcination treatment is 200~800℃.

[0021] This invention provides an iron-based catalyst, which is obtained by any of the preparation methods described above.

[0022] The iron-based catalyst described above comprises, by mass percentage, 10-95% metal oxide and 5-90% silicon oxide, wherein the metal oxide includes iron oxide and auxiliary metal oxide.

[0023] The present invention also provides a method for hydrogenating heavy oil, using the iron-based catalyst described above.

[0024] The preparation method of the iron-based catalyst of the present invention involves calcining a mixed raw material system of silicon-containing compounds and iron-based compounds and then subjecting it to alkali treatment. This process forms an appropriate number of structural vacancies on the surface of silicon oxide, guiding the auxiliary metal salt into these vacancies and ultimately forming an auxiliary metal-oxygen-iron coordination structure. This results in a strong interaction between the auxiliary metal and the active component iron, thereby obtaining an iron-based catalyst with significant lightening catalytic activity and excellent performance in desulfurization, denitrification, demetallization, asphalt removal, and coking inhibition. Detailed Implementation

[0025] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0026] The first aspect of this invention provides a method for preparing an iron-based catalyst, comprising the following steps:

[0027] 1) A mixed raw material system including silicon-containing compounds and iron-based compounds is subjected to a first calcination treatment to obtain a first calcination product;

[0028] 2) The first roasted product is subjected to alkali treatment to obtain an alkali-treated product;

[0029] 3) Mix the alkali-treated product, the aqueous solution of the auxiliary metal salt, and the aqueous solution of the precipitant, and perform precipitation treatment on the mixed system to obtain the precipitated product;

[0030] 4) The precipitated product is subjected to a second calcination treatment to obtain the iron-based catalyst.

[0031] The mixed raw material system in step 1) includes a silicon-containing compound as a structural aid source and an iron-based compound as an active component source for the iron-based catalyst. During the first calcination treatment, the volatile components in both the silicon-containing compound and the iron-based compound continuously volatilize and decrease, yielding a first calcined product comprising silicon oxide and iron oxide. The iron oxide referred to in this invention is iron oxide FeO. x , x>0.

[0032] By way of example, the silicon-containing compounds of the present invention include inorganic silicon and organosilicon solutions, such as silica sol, alkaline silica sol, nano-inorganic silicon solution, water glass, and at least one of tetraethyl orthosilicate, silicon acetate, triethoxysilane, methyldiethoxysilane, and dimethyldiethoxysilane.

[0033] By way of example, the iron-based compounds of the present invention are specifically iron salts or ferrous salts, such as at least one of ferric nitrate, ferric sulfate, ferrous sulfate, ferric chloride, ferrous chloride and ferric phosphate.

[0034] In step 2), the first calcined product is subjected to a water bath reaction in an alkaline aqueous solution, and the temperature of the water bath reaction is controlled at 40~95℃ for 0.5~4h, finally obtaining the alkaline-treated product.

[0035] To avoid the residual alkali in the alkali-treated product from affecting the subsequent preparation process, the alkali-treated system can be repeatedly filtered and washed after the alkali treatment is completed. The washed product is then dried (drying temperature for example, 60~140℃, drying time for example, 4~24h, further, drying temperature for example, 80~120℃) to obtain the alkali-treated product.

[0036] The aforementioned alkaline aqueous solution refers to an aqueous solution in which an alkali is dissolved. This invention does not limit the type of alkali in the alkaline aqueous solution; it can be an inorganic alkali and / or an organic alkali. Exemplarily, inorganic alkalis include at least one of sodium hydroxide, potassium hydroxide, and ammonia; organic alkalis include at least one of triethylamine, urea, pyridine, potassium methoxide, potassium ethoxide, and sodium ethoxide. When the alkali comprises two or more specific compounds, this invention does not limit the mass ratio between the various compounds.

[0037] Subsequently, in step 3), a precipitant is used to cause the auxiliary metal ions in the aqueous solution of the auxiliary metal salt, as well as the free ferric ions or ferrous ions that were not completely oxidized to iron oxide in step 1), to undergo a precipitation reaction to obtain the precipitated product.

[0038] The aforementioned aqueous solution of a metal-coefficient salt refers to an aqueous solution in which a metal-coefficient salt is dissolved or dispersed. This invention does not limit the type of metal-coefficient, and it can be at least one of zinc, alkali metals, and rare earth elements; nor does this invention limit the type of anion in the metal-coefficient salt, which can be any volatile anion, such as chloride ions, sulfate ions, nitrate ions, phosphate ions, etc.

[0039] The aforementioned aqueous solution of the precipitant refers to an aqueous solution in which the precipitant is dissolved. This invention does not limit the type of precipitant, as long as it can cause metal ions to precipitate in the form of a compound. For example, the precipitant includes at least one of NaOH, KOH, Na₂CO₃, K₂CO₃, Na₂S, (NH₄)₂S, urea, and ammonia water.

[0040] In one embodiment, the residual amount of precipitant in the precipitate product can be further reduced by post-treatment of the precipitation reaction system. Exemplarily, the post-treatment includes repeatedly filtering and washing the precipitation reaction system with water, followed by drying the washed product (drying temperature, for example, 60-140°C, drying time, for example, 4-24 hours, further, drying temperature, for example, 80-120°C) to obtain the precipitate product.

[0041] Finally, the precipitated product is subjected to a second calcination treatment to obtain the iron-based catalyst of the present invention. In the second calcination treatment, the auxiliary metal precipitate and iron salt precipitate formed in step 3) are oxidized to gradually generate auxiliary metal oxides and iron oxide.

[0042] The preparation method of this invention is simple and easy to operate, and can use stable and low-cost raw materials. Therefore, the preparation of iron-based catalysts has the advantages of low raw material and operating costs, which helps to improve the competitiveness of production enterprises. Furthermore, the iron-based catalyst prepared according to the method of this invention has high catalytic activity. It can not only achieve the lightening of heavy or inferior oils through hydrogenation processes, but also reduce the content of sulfur, nitrogen, metals, and asphaltenes in the products, and suppress coking during the hydrogenation process. The inventors speculate that the reason may be that during alkali treatment, the iron-oxygen-silicon coordination structure and some silicon-based oxides formed in the first roasting product are etched under the action of alkali, forming a suitable amount of structural vacancies. Since the auxiliary metal ions account for most of the ions to be precipitated, the structural vacancies formed during alkali treatment are basically completely occupied by the auxiliary metal precipitation during the precipitation process, and the auxiliary metal replaces the silicon atoms in the aforementioned iron-oxygen-silicon coordination structure, forming an iron-oxygen-auxiliary metal coordination structure. Therefore, a strong interaction occurs between the auxiliary metal and the active metal iron, thereby enhancing the catalytic activity of the iron-based catalyst.

[0043] Further, in step 1), the silicon-iron molar ratio in the mixed raw material system is (0.1~10):1. Specifically, the silicon element in the silicon-iron molar ratio refers to the silicon element in the silicon-containing compound, and the iron element in the silicon-iron molar ratio refers to the iron element in the iron-based compound. This ratio is beneficial for achieving efficient dispersion of active metallic iron, thereby forming more iron-oxygen-silicon coordination structures, and thus improving the catalytic activity of the iron-based catalyst.

[0044] In step 1), to ensure a more uniform mixing of the silicon compound and the iron-based compound, the mixed raw material system includes a dispersing solvent, such as water and / or ethanol, in addition to the silicon compound and the iron-based compound. In practice, for example, at least one of the iron-based compound and the silicon-containing compound may be prepared into a solution using a dispersing solvent, and then the two may be mixed to obtain the mixed raw material system; or, the iron-based compound, the silicon-containing compound, and the dispersing solvent may be directly mixed to obtain the mixed raw material system. Generally, the mass ratio of the dispersing solvent to the iron-based compound is (0.01~20):1. It is understood that when the mixed raw material system includes a dispersing solvent, to ensure the efficient execution of the first calcination treatment, the mixed raw material system needs to be dried before the first calcination treatment, for example, at 60~120℃ for 4~48 hours.

[0045] During the alkali treatment process, the catalytic activity of the iron-based catalyst can be further optimized by controlling the mass ratio of water to the first calcined product in the alkali aqueous solution. Specifically, the mass ratio of the first calcined product to water in the alkali aqueous solution is 1:(5~100), and the alkali concentration in the alkali aqueous solution is 0.01~2 mol / L.

[0046] This invention does not limit the temperature and time of precipitation treatment. When the precipitation treatment temperature is 40~95℃ and the time is 1~24h, it is beneficial to promote the positive progress of precipitation treatment. Furthermore, in order to make the precipitation treatment more complete, the precipitation treatment can be carried out in a water bath; even further, during the precipitation treatment in the water bath, the system needs to be continuously stirred, and after the precipitation treatment is completed, the system temperature can be appropriately reduced (the reduced system temperature is still 40~95℃) to allow the system to stand and age for 2~12h.

[0047] In one specific embodiment, when the molar ratio of metallic iron in the iron-based compound to the auxiliary metal in the aqueous solution of the auxiliary metal salt is 1:(0.1~20), it helps to further enhance the catalytic activity of the iron-based catalyst.

[0048] It should be noted that when the aqueous solution of a multi-metallic salt is a mixture of aqueous solutions of multiple multi-metallic salts, the multi-metallic salt in the above molar ratio refers to the total amount of multi-metallic salt in all multi-metallic salts.

[0049] Furthermore, the molar ratio of precipitant to total metal in the precipitant aqueous solution is (1~6):1, where the total metal includes iron from the iron-based compound and auxiliary metal from the auxiliary metal salt aqueous solution. Specifically, during the precipitation process, the catalytic activity of the iron-based catalyst can be improved by controlling the ratio between the precipitant and total metal. On the one hand, when there is too little precipitant, it is not conducive to the complete precipitation of metal ions, making it difficult to form sufficient active components of metallic iron and auxiliary metal. On the other hand, when there is too much precipitant, in addition to increasing costs, it also leads to excessive residues of precipitant and related products on the final iron-based catalyst, affecting the catalytic contact between the active components and the feedstock.

[0050] Furthermore, the inventors have discovered that when the heating rate of the first calcination treatment is 3~10℃ / min and the calcination temperature of the first calcination treatment is 200~800℃; and / or, when the heating rate of the second calcination treatment is 3~10℃ / min and the calcination temperature of the second calcination treatment is 200~800℃, it is beneficial to remove volatile components and form target structural components.

[0051] It should be noted that both the first and second calcination processes of the present invention are carried out in an air atmosphere. Furthermore, the heating rate in both the first and second calcination processes is 3~6℃ / min.

[0052] It is understandable that the time for the first and second calcination processes will vary when different silicon-containing compounds and iron-based compounds are selected, as well as different first and second calcination temperatures. Specifically, the time for the first and second calcination processes is 2 to 8 hours, each independently.

[0053] A second aspect of the present invention provides an iron-based catalyst, which is obtained by the above-described preparation method.

[0054] The iron-based catalyst of this invention can be used for the lightening of heavy or inferior oils, and is particularly suitable for slurry-bed hydrogenation systems. Heavy or inferior oils refer to various primary and secondary processed residues and their deasphalted oils with boiling points above 350°C. Exemplarily, this includes at least one of crude oil, atmospheric residue, vacuum residue, coal tar, deasphalted oil, and heavy oils extracted from oil sands or shale.

[0055] In the process of using the iron-based catalyst of the present invention to lighten heavy or inferior oils, the iron-based catalyst of the present invention can be used directly or after pre-sulfurization treatment. When pre-sulfurization treatment is required, the present invention does not limit the specific process parameters of the pre-sulfurization treatment; a pre-sulfurization process of conventional hydrotreating catalysts in the art can be used, and the pre-sulfurized oil or pre-sulfurizing agent used can also be a conventionally used pre-sulfurized oil or pre-sulfurizing agent in the art. In one specific embodiment, the pre-sulfurization treatment temperature is 200~450℃, the pressure is 1~10MPa, the pre-sulfurization treatment time is 4~48 hours, and the liquid hourly space velocity is 0.5~10h. -1 The hydrogen-to-oil volume ratio is 100-800; furthermore, the pre-sulfurization treatment temperature is 280-380℃, the pressure is 2-6MPa, the pre-sulfurization treatment time is 6-24 hours, and the liquid hourly space velocity is 1-4h. -1 The hydrogen-to-oil volume ratio is 200-500.

[0056] The iron-based catalyst of this invention for the lightening treatment of heavy or inferior oil mainly refers to the hydrotreating of heavy or inferior oil, including but not limited to hydrorefining, hydromodification, hydrocracking and hydroisomerization; more specifically, hydrotreating includes hydrodesulfurization, hydronitrogenation, hydrodemetallization, and hydrosaturation of aromatics.

[0057] In one specific embodiment, the iron-based catalyst comprises an oxide structure promoter, an oxide of active metallic iron (iron oxide), and a metal-supporting oxide. The iron-based catalyst comprises, by mass percentage, 10-95% metal oxide and 5-90% silicon oxide (oxide structure promoter), wherein the metal oxide includes iron oxide and the metal-supporting oxide.

[0058] The iron-based catalyst of this invention is beneficial for the lightening of heavy or inferior oils, especially in desulfurization, demetallization, denitrification and deasphalting.

[0059] The present invention also provides a method for hydrogenating heavy oil using the above-mentioned iron-based catalyst.

[0060] The specific hydrogenation method of this invention is basically the same as the existing hydrogenation methods for heavy oil in the art, wherein the hydrogenation treatment temperature is 200~500℃, the pressure is 2~25MPa, and the liquid hourly space velocity is 0.1~3h. -1 The hydrogen-to-oil volume ratio is 500–2000; furthermore, the hydrotreating temperature is 350–450°C, the pressure is 4–18 MPa, and the liquid hourly space velocity is 0.2–1.5 h⁻¹. -1 The hydrogen-to-oil volume ratio is 800-1300.

[0061] In one specific embodiment, the mass of the iron-based catalyst, calculated as iron, is 1 to 20 wt% of the mass of the heavy oil.

[0062] This hydrogenation method enables efficient hydrogenation of heavy oils.

[0063] The iron-based catalyst and its preparation method of the present invention will be described in detail below through specific embodiments.

[0064] Example 1

[0065] The preparation method of the iron-based catalyst in this embodiment includes the following steps:

[0066] 1) Mix 32.44 g of ferric chloride, silica sol (the Si:Fe molar ratio of silica sol and ferric chloride is 0.25:1) and 5 g of deionized water evenly. The resulting mixed raw material system is dried at 120℃ for 6 h, and then heated at a rate of 5℃ / min and calcined at 400℃ in air atmosphere for 3 h to obtain the first calcined product.

[0067] 2) Then the first calcined product was added to a 0.5 mol / L potassium hydroxide aqueous solution (the mass ratio of the first calcined product to the water in the potassium hydroxide aqueous solution was 1:20), treated at 80℃ water bath temperature for 1 h, filtered, washed with water, and dried at 120℃ for 4 h to obtain the alkali-treated product.

[0068] 3) The alkali-treated product and the cerium nitrate aqueous solution (cerium nitrate is dissolved in 250 mL of deionized water, and the Fe:Ce molar ratio of ferric chloride and cerium nitrate is 1:0.25) are added to a sodium hydroxide solution obtained by dissolving 10 g of sodium hydroxide in 80 mL of deionized water and mixed evenly; wherein, the molar ratio of sodium hydroxide to total metals is 1:1;

[0069] 4) Stir the mixture in a water bath at 80°C for 4 hours, then cool it down to 60°C and let it stand for 12 hours to age. Filter to obtain the precipitate.

[0070] 5) The precipitate was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 500°C in air for 2 hours at a rate of 5°C / min to obtain the iron-based catalyst A1.

[0071] Example 2

[0072] The preparation method of the iron-based catalyst in this embodiment includes the following steps:

[0073] 1) Mix 32.44g of ferric chloride and tetraethyl orthosilicate (the Si:Fe molar ratio of tetraethyl orthosilicate and ferric chloride is 0.38:1) evenly. The resulting mixed raw material system is dried at 120℃ for 8h and then heated at a rate of 5℃ / min. After calcination at 500℃ in air atmosphere for 2h, the first calcined product is obtained.

[0074] 2) Then the first calcined product was added to a 0.2 mol / L triethylamine aqueous solution (the mass ratio of the first calcined product to water in the triethylamine aqueous solution was 1:10), treated at 80℃ water bath temperature for 2 h, filtered while hot, washed with water, and dried at 120℃ for 4 h to obtain the alkali-treated product.

[0075] 3) The alkali-treated product and zinc chloride aqueous solution (zinc chloride is dissolved in 250 mL of deionized water, and the Fe:Zn molar ratio of ferric chloride and zinc chloride is 1:3) are added to 121.53 g of ammonia aqueous solution (mass percentage is 30%) and mixed evenly; wherein, the molar ratio of ammonia to total metal is 1.25:1;

[0076] 4) Stir the mixture in an 80°C water bath for 2 hours, then cool it to 40°C and let it stand for 12 hours to age. Filter to obtain the precipitate.

[0077] 5) The precipitated product was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 500°C in air atmosphere for 4 hours at a rate of 3°C / min to obtain iron-based catalyst A2.

[0078] Example 3

[0079] The iron-based catalyst preparation method in this embodiment includes the following steps:

[0080] 1) Mix 40.25g ferric sulfate, 6.82g ferrous sulfate, silicon acetate (the Si:Fe molar ratio of silicon acetate, ferric sulfate, and ferrous sulfate is 0.8:1) and 5g ethanol evenly. The resulting mixed raw material system is dried at 100℃ for 12h, and then heated at a rate of 10℃ / min to 350℃ in air atmosphere for 4h to obtain the first calcined product.

[0081] 2) Then the first calcined product was added to a 1.0 mol / L sodium hydroxide aqueous solution (the mass ratio of the first calcined product to the water in the sodium hydroxide aqueous solution was 1:8), treated at a water bath temperature of 90℃ for 2 hours, filtered while hot, washed with water, and dried at 120℃ for 6 hours to obtain the alkali-treated product.

[0082] 3) The alkali-treated product and magnesium sulfate aqueous solution (magnesium sulfate dissolved in 500 mL of deionized water, with the Fe:Mg molar ratio of ferrous sulfate, ferrous sulfate and magnesium sulfate being 1:1.2) are then added to 126.22 g of ammonia aqueous solution (mass percentage of 30%) and mixed thoroughly; wherein the molar ratio of ammonia to total metals is 2:1.

[0083] 4) Stir the mixture in a water bath at 70°C for 3 hours, then cool it down to 60°C and let it stand for 4 hours to age. Filter to obtain the precipitate.

[0084] 5) The precipitate was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 500°C in air atmosphere for 3 hours at a rate of 10°C / min to obtain iron-based catalyst A3.

[0085] Example 4

[0086] The preparation method of the iron-based catalyst in this embodiment includes the following steps:

[0087] 1) Mix 20.2g of ferric nitrate nonahydrate, silicon acetate (the Si:Fe molar ratio of silicon acetate and ferric nitrate nonahydrate is 6:1) and 15g of ethanol evenly. The resulting mixed raw material system is dried at 80℃ for 12h and then heated at a rate of 3℃ / min to 350℃ and calcined in air atmosphere for 4h to obtain the first calcined product.

[0088] 2) Then the first calcined product was added to a 1.0 mol / L sodium hydroxide aqueous solution (the mass ratio of the first calcined product to the water in the sodium hydroxide aqueous solution was 1:100), treated at a water bath temperature of 90℃ for 3 hours, filtered while hot, washed with water, and dried at 120℃ for 6 hours to obtain the alkali-treated product.

[0089] 3) The alkaline treatment product and zinc sulfate aqueous solution (zinc sulfate dissolved in 500 mL of deionized water, and the Fe:Zn molar ratio of ferric nitrate nonahydrate to zinc sulfate is 1:5) are added to a urea solution obtained by dissolving 108 g of urea in 100 mL of deionized water and mixed evenly; wherein, the molar ratio of urea to total metals is 6:1.

[0090] 4) Stir the mixture in a water bath at 80°C for 3 hours, then cool it down to 60°C and let it stand for 4 hours to age. Filter to obtain the precipitate.

[0091] 5) The precipitated product was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 400°C in air atmosphere for 3 hours at a rate of 6°C / min to obtain iron-based catalyst A4.

[0092] Example 5

[0093] The preparation method of the iron-based catalyst in this embodiment is basically the same as that in Example 3. The difference is that the heating rate of calcination in steps 1) and 5) in this embodiment is 20℃ / min.

[0094] Example 6

[0095] The iron-based catalyst preparation method in this embodiment includes the following steps:

[0096] 1) A mixture of 10.02 g ferric sulfate, 15.2 g ferrous sulfate, and tetraethyl orthosilicate (with a Si:Fe molar ratio of 10:1 for tetraethyl orthosilicate, ferric sulfate, and ferrous sulfate) was dried at 100 °C for 12 h and then calcined at 450 °C in air for 4 h at a rate of 10 °C / min to obtain the first calcined product.

[0097] 2) Then the first calcined product was added to a 1.0 mol / L sodium hydroxide aqueous solution (the mass ratio of the first calcined product to the water in the sodium hydroxide aqueous solution was 1:10), treated at 85℃ water bath temperature for 3 h, filtered while hot, washed with water, and dried at 120℃ for 6 h to obtain the alkali-treated product.

[0098] 3) The alkali-treated product and zinc sulfate aqueous solution (zinc sulfate dissolved in 500 mL of deionized water, and the Fe:Zn molar ratio of ferrous sulfate, ferrous sulfate and zinc sulfate is 1:10) are added to 481.25 g of ammonia aqueous solution (mass percentage is 30%) and mixed evenly; wherein, the molar ratio of ammonia to total metal is 3:1;

[0099] 4) Stir the mixture in a water bath at 70°C for 3 hours, then cool it down to 60°C and let it stand for 4 hours to age. Filter to obtain the precipitate.

[0100] 5) The precipitated product was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 550°C in air atmosphere for 3 hours at a rate of 10°C / min to obtain iron-based catalyst A6.

[0101] Example 7

[0102] The mixture of 1.62 g of ferric chloride and silica sol (with a Si:Fe molar ratio of 3:1 between silica sol and ferric chloride) was dried at 120 °C for 6 h, then heated at a rate of 5 °C / min and calcined at 500 °C in air for 3 h to obtain the first calcined product.

[0103] 2) Then the first calcined product was added to an ammonia solution with a concentration of 2.0 mol / L (the mass ratio of the first calcined product to water in the ammonia solution was 1:15), treated at 80℃ water bath temperature for 1 h, filtered, washed with water, and dried at 120℃ for 4 h to obtain the alkali-treated product.

[0104] 3) The alkaline treatment product and zinc nitrate aqueous solution (zinc nitrate is dissolved in 200 mL of deionized water, and the Fe:Zn molar ratio of ferric chloride and zinc nitrate is 1:20) are added to a potassium hydroxide solution obtained by dissolving 47 g of potassium hydroxide in 200 mL of deionized water and mixed evenly; wherein, the molar ratio of potassium hydroxide to total metals is 4:1.

[0105] 4) Stir the mixture in a water bath at 80°C for 4 hours, then cool it down to 60°C and let it stand for 12 hours to age. Filter to obtain the precipitate.

[0106] 5) The precipitated product was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 500°C in air atmosphere for 2 hours at a rate of 5°C / min to obtain iron-based catalyst A7.

[0107] Comparative Example 1

[0108] This comparative example provides a comparative catalyst for the slurry-bed hydrotreating of heavy oil, and its preparation method includes the following steps:

[0109] 1) Mix 32.44g of ferric chloride and zinc chloride aqueous solution (zinc chloride was dissolved in 250mL of deionized water, and the Fe:Zn molar ratio of ferric chloride and zinc chloride was 1:0.25) to obtain a mixed system;

[0110] 2) While stirring, slowly add the sodium hydroxide solution (obtained by dissolving 12g of sodium hydroxide in 80mL of deionized water) to the above mixture; wherein, the molar ratio of sodium hydroxide to total metal is 1.2:1;

[0111] 3) Stir the reaction in an 80°C water bath for 4 hours, then cool it down to 60°C and let it stand for 24 hours to age. Filter to obtain the precipitate.

[0112] 4) The precipitate was washed with deionized water while hot until the pH value was about 7. Then it was dried in an oven at 120°C for 12 hours. The temperature was then increased at a rate of 5°C / min and calcined at 500°C in air for 2 hours to obtain iron-based catalyst B1.

[0113] Comparative Example 2

[0114] The preparation method of the iron-based catalyst in this embodiment includes the following steps:

[0115] 1) Mix 20.2g of ferric nitrate nonahydrate, silicon acetate (the Si:Fe molar ratio of silicon acetate and ferric nitrate nonahydrate is 6:1) and 15g of ethanol evenly. The resulting mixed raw material system is dried at 80℃ for 12h and then heated at a rate of 3℃ / min to 350℃ and calcined in air atmosphere for 4h to obtain the first calcined product.

[0116] 2) Then, the first roasting product and the zinc sulfate aqueous solution (zinc sulfate dissolved in 500 mL of deionized water, and the Fe:Zn molar ratio of ferric nitrate nonahydrate to zinc sulfate is 1:5) are added to the urea solution obtained by dissolving 108 g of urea in 100 mL of deionized water and mixed evenly; wherein, the molar ratio of urea to total metals is 6:1;

[0117] 3) Stir the mixture in an 80°C water bath for 3 hours, then cool it to 60°C and let it stand for 4 hours to age. Filter to obtain the precipitate.

[0118] 4) The precipitate was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 400°C in air for 3 hours at a rate of 6°C / min to obtain iron-based catalyst B2.

[0119] Comparative Example 3

[0120] The preparation method of the iron-based catalyst in this embodiment includes the following steps:

[0121] 1) Mix 40.25g ferric sulfate, 6.82g ferrous sulfate and 5g ethanol evenly. The resulting mixed raw material system is dried at 100℃ for 12h and then heated at a rate of 10℃ / min to 350℃ in air atmosphere for 4h to obtain the first calcined product.

[0122] 2) Then the first calcined product was added to a 1.0 mol / L sodium hydroxide aqueous solution (the mass ratio of the first calcined product to the water in the sodium hydroxide aqueous solution was 1:8), treated at a water bath temperature of 90℃ for 2 hours, filtered while hot, washed with water, and dried at 120℃ for 6 hours to obtain the alkali-treated product.

[0123] 3) The alkali-treated product and magnesium sulfate aqueous solution (magnesium sulfate dissolved in 500 mL of deionized water, with the Fe:Mg molar ratio of ferrous sulfate, ferrous sulfate and magnesium sulfate being 1:1.2) are then added to 126.22 g of ammonia aqueous solution (mass percentage of 30%) and mixed thoroughly; wherein the molar ratio of ammonia to total metals is 2:1.

[0124] 4) Stir the mixture in a water bath at 70°C for 3 hours, then cool it down to 60°C and let it stand for 4 hours to age. Filter to obtain the precipitate.

[0125] 5) The precipitate was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 500°C in air for 3 hours at a rate of 10°C / min to obtain iron-based catalyst B3.

[0126] Comparative Example 4

[0127] The preparation method of the iron-based catalyst in this embodiment includes the following steps:

[0128] 1) Mix 32.44 g of ferric chloride, silica sol (the Si:Fe molar ratio of silica sol and ferric chloride is 0.25:1) and 5 g of deionized water evenly, then add cerium nitrate aqueous solution (cerium nitrate is obtained by dissolving in 50 mL of deionized water, and the Fe:Ce molar ratio of ferric chloride and cerium nitrate is 1:0.25). The resulting mixed raw material system is dried at 120 °C for 6 h, and then heated at a rate of 5 °C / min and calcined at 400 °C in air atmosphere for 3 h to obtain the first calcined product.

[0129] 2) Then the first calcined product was added to a 0.5 mol / L potassium hydroxide aqueous solution (the mass ratio of the first calcined product to the water in the potassium hydroxide aqueous solution was 1:20), treated at 80℃ water bath temperature for 1 h, filtered, washed with water, and dried at 120℃ for 4 h to obtain the alkali-treated product.

[0130] 3) Add the alkali-treated product to 10g of sodium hydroxide dissolved in 280mL of deionized water and mix thoroughly; wherein the molar ratio of sodium hydroxide to total metal is 1:1;

[0131] 4) Stir the mixture in a water bath at 80°C for 4 hours, then cool it down to 60°C and let it stand for 12 hours to age. Filter to obtain the precipitate.

[0132] 5) The precipitated product was washed with deionized water until the pH value was approximately 7, then dried in an oven at 120°C, and then calcined at 500°C in air atmosphere for 2 hours at a rate of 5°C / min to obtain iron-based catalyst B4.

[0133] Experimental Example 1

[0134] This experiment demonstrates the application of iron-based catalysts A1-A3, A5-A6, and B1, B3-B4 in slurry-bed hydrotreating of mixed residue oil (whose properties are shown in Table 1). All iron-based catalysts underwent pre-sulfurization treatment before application at a temperature of 350℃, a pressure of 4 MPa, a time of 8 hours, and a liquid hourly space velocity (LISH) of 1.5 h⁻¹. -1 The hydrogen-to-oil volume ratio is 300.

[0135] The hydrotreating process was carried out in a 0.5L high-temperature and high-pressure slurry-bed reactor. The operating conditions for the hydrotreating process were: a temperature of 430℃, a pressure of 16MPa, and a reaction space velocity of 0.5h⁻¹. -1 The hydrogen-to-oil volume ratio was 900, the mixed residue oil was 150g, and the catalyst mass was 10wt% of the mixed residue oil mass. After hydrotreating, the hydrotreating system was tested, and the results are shown in Table 2.

[0136] Table 1

[0137]

[0138] Table 2

[0139]

[0140] Experimental Example 7

[0141] In this experimental example, iron-based catalysts A2, A4, A7, B1, and B2 were used to perform slurry bed hydrotreating on the mixed residue oil in Table 1, and none of the iron-based catalysts were pre-sulfurized before application.

[0142] The hydrotreating process was carried out in a 0.5L high-temperature and high-pressure slurry-bed reactor. The operating conditions for the hydrotreating process were: a temperature of 430℃, a pressure of 16MPa, and a reaction space velocity of 0.5h⁻¹. -1 The hydrogen-to-oil volume ratio was 900, the feedstock oil was 150g, and the catalyst mass was 15wt% of the mixed residue oil mass. After hydrotreating, the hydrotreating system was tested, and the results are shown in Table 3.

[0143] Table 3

[0144]

[0145] As can be seen from the data in Tables 2 and 3, the iron-based catalyst prepared by the method of this invention exhibits superior desulfurization, demetallization, denitrogenation, deasphalting, and lightening effects on heavy oil, whether pre-sulfurized or not. Compared to the comparative example, the iron-based catalyst prepared by this invention demonstrates superior reactivity. Therefore, the iron-based catalyst of this invention has promising application prospects in slurry-bed hydrotreating processes.

[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an iron-based catalyst, characterized in that, Includes the following steps: 1) A mixed raw material system including silicon-containing compounds and iron-based compounds is subjected to a first calcination treatment to obtain a first calcination product; 2) The first roasted product is subjected to alkali treatment to obtain an alkali-treated product; 3) Mix the alkali-treated product, the aqueous solution of the auxiliary metal salt, and the aqueous solution of the precipitant, and perform precipitation treatment on the mixed system to obtain the precipitated product; The auxiliary metal is at least one of zinc, magnesium, and the rare earth element cerium; 4) The precipitated product is subjected to a second calcination treatment to obtain the iron-based catalyst; The alkali treatment includes: subjecting the first calcined product to a water bath reaction in an alkaline aqueous solution, wherein the temperature of the water bath reaction is 40~95℃ and the time is 0.5~4h.

2. The preparation method according to claim 1, characterized in that, In step 1), the molar ratio of silicon to iron in the mixed raw material system is (0.1~10):

1.

3. The preparation method according to claim 1, characterized in that, The mass ratio of the first calcined product to water in the alkaline aqueous solution is 1:(5~100), and the alkali concentration in the alkaline aqueous solution is 0.01~2 mol / L.

4. The preparation method according to any one of claims 1-3, characterized in that, The precipitation treatment is carried out at a temperature of 40~95℃ for 1~24h.

5. The preparation method according to claim 4, characterized in that, The molar ratio of metallic iron in the iron-based compound to the auxiliary metal in the aqueous solution of the auxiliary metal salt is 1:(0.1~20).

6. The preparation method according to claim 4, characterized in that, The molar ratio of precipitant to total metal in the aqueous precipitant solution is (1~6):1, and the total metal includes iron in the iron-based compound and auxiliary metal in the aqueous solution of the auxiliary metal salt.

7. The preparation method according to claim 1, characterized in that, The heating rate of the first calcination treatment is 3~10℃ / min, and the calcination temperature of the first calcination treatment is 200~800℃; and / or, The heating rate of the second calcination treatment is 3~10℃ / min, and the calcination temperature of the second calcination treatment is 200~800℃.

8. An iron-based catalyst, characterized in that, It is obtained by the preparation method according to any one of claims 1-7.

9. The iron-based catalyst according to claim 8, characterized in that, The metal oxides comprise 10-95% by mass and 5-90% by mass, including iron oxide and auxiliary metal oxides.

10. A method for hydrogenating heavy oil, characterized in that, The iron-based catalyst described in claim 9 is used.

Citation Information

Patent Citations

  • Residual oil suspended bed hydrocracking catalyst as well as preparation method and application thereof

    CN114602472A

  • Promoted, attrition resistant, silica supported precipitated iron catalyst

    US20090075814A1