A microcrystalline glass and its preparation method, and microcrystalline glass products
By adjusting the crystal phase composition and processing technology of glass-ceramics, the problems of fogging and poor weather resistance after chemical strengthening of glass-ceramics have been solved, resulting in glass-ceramics with high hardness, drop resistance and good light transmittance, which are suitable for displays, electronic smart terminals and photovoltaic power generation devices.
Patent Information
- Application Number
- CN202410255780.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-11-22
AI Technical Summary
Existing microcrystalline glass is prone to fogging after chemical strengthening, and its weather resistance is not ideal, especially in high temperature and high humidity environments, which affects its performance.
By adjusting the crystal phase composition of the glass-ceramic, ensuring that the content of LiAlSi4O10 is greater than that of other crystal phases, the ratio of LiAlSi4O10 to Li2Si2O5 is ≥1.13, controlling the average crystal particle size to ≤50nm, optimizing the component ratio to improve transmittance and weather resistance, and employing nucleation, crystallization, and chemical strengthening treatments.
It achieves high hardness, good drop resistance and excellent weather resistance in microcrystalline glass. The glass surface is not prone to fogging, it is suitable for high temperature and high humidity environments, and maintains good light transmittance.
Smart Images

Figure CN118206287B_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No. 202211470006.6, entitled "A microcrystalline glass and its preparation method, and microcrystalline glass products", filed on November 22, 2022. Technical Field
[0002] This invention relates to the field of glass-ceramics, and more particularly to a glass-ceramic, its preparation method, and glass-ceramic products. Background Technology
[0003] With the development of display technology, glass is frequently used to protect display devices. Studies have shown that 70% of electronic product damage is caused by accidental drops. The cover glass used for protecting electronic products on the market is generally high-alumina silicate glass. High alumina content is beneficial for improving stress strength and stress layer depth after ion exchange, but this glass has relatively poor drop resistance.
[0004] The performance of glass-ceramics depends on the ratio of crystalline phase to glassy phase and the size of the grains. Introducing nucleating agents into the glass formulation or adjusting the oxide ratio can form one or more crystalline phases during subsequent heat treatment. This results in glass exhibiting both high transparency and high strength, improving properties such as average hardness and fracture toughness. The microcrystalline phase in glass-ceramics can hinder microcrack propagation paths, contributing to overall improvements in scratch resistance, impact resistance, and drop resistance. However, glass-ceramics have poor weather resistance and are prone to aging, especially in high-temperature and high-humidity environments, where surface fogging can occur, affecting their performance. Summary of the Invention
[0005] The main objective of this invention is to provide a microcrystalline glass, a preparation method thereof, and microcrystalline glass products, thereby solving the technical problem that the surface of microcrystalline glass obtained after chemical strengthening is prone to fogging in the prior art.
[0006] To achieve the above objectives, the present invention provides a microcrystalline glass with a crystallinity ≥55% and a crystalline phase comprising LiAlSi4O. 10 and Li2Si2O5, wherein the LiAlSi4O 10 Its content is greater than that of any other crystalline phase;
[0007] The LiAlSi4O 10 The ratio of the content of [certain substances] to the content of Li2Si2O5 is ≥1.13;
[0008] The microcrystalline glass contains the following components by weight percentage:
[0009] 69%–75% SiO2;
[0010] 6%–12% Al2O3;
[0011] 1.7%–3.5% P2O5;
[0012] 8%–13% Li₂O;
[0013] 0.1%–3% Na₂O;
[0014] 2% to 5% ZrO2.
[0015] Optionally, the crystalline phase of the glass-ceramic may further include at least one of Li2SiO3, Li3PO4, and β-spodumene.
[0016] Optionally, the microcrystalline glass contains the following components by weight percentage:
[0017] 71%–74% SiO2;
[0018] 7%–10% Al2O3;
[0019] 2%–3.5% P2O5;
[0020] 10%–12% Li₂O;
[0021] 0.5%–2% Na₂O;
[0022] 2.5% to 4.5% ZrO2.
[0023] Further, optionally, the microcrystalline glass also contains the following components by weight percentage:
[0024] K2O: 0-1%;
[0025] B2O3: 0-1%;
[0026] CaO: 0-1%;
[0027] MgO: 0–1%;
[0028] ZnO: 0-1%;
[0029] Y2O3: 0-1%;
[0030] Clarifying agent: 0-1%.
[0031] Optionally, the average grain size of the crystals in the microcrystalline glass is ≤50nm;
[0032] And / or, the average transmittance of the microcrystalline glass in the range of 380 nm to 780 nm is ≥90.5%.
[0033] And / or, the average transmittance of the microcrystalline glass at wavelengths of 380-780 nm is ≥90.5% after undergoing the double 85 test.
[0034] Optionally, the b-value of the microcrystalline glass is ≤0.45, wherein the b-value is the absolute value of the yellow-blue value when the thickness of the microcrystalline glass is 0.6 mm.
[0035] And / or, the haze of the microcrystalline glass is ≤0.25.
[0036] And / or, the drop height of the microcrystalline glass is ≥1.6m.
[0037] Furthermore, to achieve the above objectives, the present invention also provides a method for preparing microcrystalline glass, the method comprising the following steps:
[0038] S10 involves weighing and mixing glass raw materials, then melting, clarifying, homogenizing, shaping, and annealing to obtain raw glass sheets.
[0039] S20, the raw glass plate is subjected to nucleation treatment, then crystallization treatment, and then cooled to obtain basic microcrystalline glass;
[0040] S30, the basic microcrystalline glass is chemically strengthened to obtain the microcrystalline glass.
[0041] Optionally, the nucleation treatment temperature is 530℃~580℃, and the nucleation treatment time is 0.5h~1.5h.
[0042] Optionally, the crystallization treatment temperature is 640℃~740℃, and the crystallization treatment time is 2~4h.
[0043] Optionally, the chemical enhancement treatment includes a bath salt containing 10 wt% to 40 wt% NaNO3 and 59 wt% to 90 wt% KNO3; and / or 0 wt% to 0.2 wt% LiNO3.
[0044] Optionally, the temperature for chemical strengthening is 450℃~520℃, and the time for chemical strengthening is 4~8h.
[0045] In addition, the present invention also provides a microcrystalline glass product, which includes the microcrystalline glass as described above. The microcrystalline glass product can be applied to the fields of displays, electronic smart terminals and photovoltaic power generation devices to play a protective role.
[0046] The beneficial effects that this invention can achieve are:
[0047] Compared with the prior art, the crystallinity of the microcrystalline glass of the present invention is ≥55%, and its crystalline phase includes LiAlSi4O. 10And Li₂Si₂O₅. LiAlSi₄O 10 The content of LiAlSi4O is greater than the content of any other crystal phase. 10 The ratio of the content of [unspecified substance] to the content of Li2Si2O5 is ≥1.13, the average particle size of the crystal is ≤50nm, the average transmittance of the microcrystalline glass in the wavelength range of 380nm~780nm is ≥90.5%, the b-value is ≤0.45, the haze is ≤0.25, and the drop height is ≥1.6m.
[0048] By adjusting the crystal phase composition of glass-ceramics and controlling the differences in structure between the glass phase and the crystal phase, the formation of voids is reduced, thus avoiding the formation of Na+ voids during chemical strengthening. + Aggregates within the voids of the microcrystalline and glassy phases, making it difficult to form compressive stress. At the same time, the chemically strengthened microcrystalline glass has good hardness and drop resistance, as well as excellent weather resistance, is not prone to aging, does not easily fog up on the glass surface, has good light transmittance, and can adapt to high temperature and high humidity environments. It can be widely used in fields such as displays, electronic smart terminals, and photovoltaic power generation devices.
[0049] The preparation method of the present invention is easy to process and has low processing cost, which can save time and energy for heat treatment. Attached Figure Description
[0050] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0051] Figure 1 This is a schematic flowchart of the preparation method of microcrystalline glass in Embodiment 1 of the present invention.
[0052] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0053] It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0054] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0055] In this invention, descriptions involving "first," "second," etc., are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of that feature. Furthermore, the technical solutions of the various embodiments can be combined with each other, but only on the basis of being achievable by those skilled in the art. If the combination of technical solutions is contradictory or impossible to implement, such a combination should be considered non-existent and not within the scope of protection claimed by this invention.
[0056] Because the crystal content in glass-ceramics is high (>60%), structural differences exist between the glass phase and the crystalline phase, resulting in structural vacancies. During chemical strengthening, on the one hand, Na... + They tend to agglomerate in the cavities of the microcrystalline and glassy phases, making it difficult to form compressive stress. On the other hand, microcrystalline glass has poor weather resistance and is prone to aging, especially in high temperature and high humidity environments, where the glass surface is prone to fogging, affecting its performance.
[0057] In view of this, the present invention provides a microcrystalline glass, which has high hardness, good drop resistance and excellent weather resistance, is not easy to age, the glass surface is not easy to fog up, has good light transmittance, and can adapt to high temperature and high humidity environments.
[0058] The crystallinity of the microcrystalline glass of this invention is ≥55%, and its crystalline phase includes LiAlSi4O. 10 and Li2Si2O5, wherein the LiAlSi4O 10 Its content is greater than that of any other crystal phase.
[0059] The LiAlSi4O 10 The ratio of the content of [agent] to the content of [Li2Si2O5] is ≥1.13.
[0060] The microcrystalline glass of the present invention includes, but is not limited to, the crystal phases described above, and may also include at least one of Li2SiO3, Li3PO4, and β-spodumene.
[0061] By adjusting the crystal phase composition of glass-ceramics and controlling the differences in structure between the glass phase and the crystal phase, the formation of voids is reduced, thus avoiding the formation of Na+ voids during chemical strengthening. + Aggregates within the voids of the microcrystalline and glassy phases, making it difficult to form compressive stress. It can also solve problems such as the poor weather resistance of microcrystalline glass, easy aging, fogging on the glass surface, and incompatibility with high temperature and high humidity environments.
[0062] The microcrystalline glass of the present invention contains the following components by weight percentage:
[0063] 69%–75% SiO2;
[0064] 6%–12% Al2O3;
[0065] 1.7%–3.5% P2O5;
[0066] 8%–13% Li₂O;
[0067] 0.1%–3% Na₂O;
[0068] 2% to 5% ZrO2.
[0069] More preferably, the microcrystalline glass of the present invention contains the following components:
[0070] 71%–74% SiO2;
[0071] 7%–10% Al2O3;
[0072] 2%–3.5% P2O5;
[0073] 10%–12% Li₂O;
[0074] 0.5%–2% Na₂O;
[0075] 2.5% to 4.5% ZrO2.
[0076] The SiO2 in the glass-ceramic of this invention is a component constituting the glass framework. SiO2 can serve as the main body of the glass network structure, endowing the base glass and the glass-ceramic with better chemical stability, mechanical properties, and forming properties. During the glass microcrystallization process, it provides a source of SiO2 for the formation of crystalline phases. Excessive SiO2 content during glass microcrystallization promotes the formation of quartz and quartz solid solutions. Therefore, considering all factors, the preferred mass percentage of SiO2 is 69%–75%, more preferably 71%–74%. In some embodiments, the SiO2 content is 69%, 70%, 71%, 72%, 73%, 74%, or 75%.
[0077] In this invention, the Al2O3 in the microcrystalline glass is a network intermediate oxide. The non-bridging oxygen forms an aluminum-oxygen tetrahedron with Al, which has a larger volume than the silicon-oxygen tetrahedron, creating larger gaps in the glass structure. This facilitates ion exchange, resulting in better chemical strengthening and improved mechanical properties. However, Al2O3 is an extremely refractory oxide, which rapidly increases the high-temperature viscosity of the glass, making glass clarification and homogenization more difficult and significantly increasing the concentration of bubble defects. Excessive Al2O3 content can significantly increase the glass microcrystallization temperature, inhibiting the crystallization ability of the base glass and hindering the formation of Li2Si2O5, thus promoting the crystallization process of LiAlSi4O3. 10Excessive formation, even of the LiAlSi2O6 crystalline phase within the base glass, reduces glass transmittance. Therefore, considering all factors, the mass percentage content of Al2O3 is preferably 6% to 12%, more preferably 7% to 10%. In some embodiments, the mass percentage content of Al2O3 is 6%, 7%, 8%, 9%, 10%, 11%, or 12%.
[0078] In the microcrystalline glass of this invention, P2O5 and Li2O react to form the Li3PO4 crystalline phase, thereby inducing the reaction of Li2O and SiO2 in the glass to form Li2SiO3, ultimately generating the Li2Si2O5 crystalline phase. If the P2O5 content is too high, it will promote the precipitation of lithium metasilicate during crystallization, resulting in insufficient glass phase and an inability to form a sufficient amount of Li2Si2O5 crystalline phase. It will also promote the precipitation of the quartz phase, making it difficult to obtain crystallized glass with high transmittance. Therefore, considering all factors, the preferred mass percentage of P2O5 is 1.7% to 3.5%, more preferably 2% to 3.5%. In some embodiments, the mass percentage of P2O5 is 1.7%, 1.9%, 2%, 2.2%, 2.4%, 2.5%, 2.7%, 3%, 3.3%, or 3.5%.
[0079] The Li₂O in the microcrystalline glass of this invention, being a network exogenous oxide, reduces the viscosity of the glass, promoting its melting and clarification. It also promotes the formation of Li₃PO₄ during the basic microcrystallization process, which in turn facilitates the formation of Li₂Si₂O₅ and LiAlSi₄O₅ crystalline phases during crystallization. 10 Crystal phase. However, excessively high Li₂O content leads to excessively low glass viscosity, making it difficult to obtain a chemically stable glass composition. It also results in excessively low compressive stress during ion strengthening and increases raw material costs. Therefore, considering all factors, the preferred mass percentage content of Li₂O is 8%–13%, more preferably 10%–12%. In some embodiments, the mass percentage content of Li₂O is 8%, 9%, 10%, 11%, 12%, 13%, 12.5%, 11.7%, 9.6%, or 8.4%.
[0080] The Na₂O in the microcrystalline glass of this invention can significantly reduce the viscosity of the base glass, promoting its melting and clarification, while simultaneously lowering the glass crystallization temperature. This facilitates the crystallization of the glass to react with K₂O in molten potassium nitrate salt. + To strengthen the glass and generate high compressive stress on its surface, thus increasing its strength, the glass must contain a sufficient amount of sodium (Na). +It is present. Therefore, taking all factors into consideration, the mass percentage content of Na2O is preferably 0.1% to 3%, more preferably 0.5% to 2%. In some embodiments, the mass percentage content of Na2O is 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1%, 1.4%, 1.5%, 1.8%, 2%, 2.2%, 2.6%, 2.5%, 2.8%, or 3%.
[0081] The ZrO2 in the microcrystalline glass of this invention has a high zirconium ion potential energy, and ZrO2 tends to promote the crystallization of lithium feldspar crystals. ZrO2 also helps to reduce the grain size during crystallization, thereby improving the glass transmittance. Excessive ZrO2 content leads to the presence of unmelted ZrO2 in the glass, resulting in uneven crystallization. Therefore, considering all factors, the preferred ZrO2 mass percentage is 2% to 5%, more preferably 2.5% to 4.5%. In some embodiments, the ZrO2 mass percentage is 2%, 2.2%, 2.5%, 2.6%, 2.9%, 3%, 3.2%, 3.5%, 3.9%, 4%, 4.1%, 4.5%, 4.7%, 4.9%, or 5%.
[0082] The microcrystalline glass of the present invention comprises, but is not limited to, the above-mentioned components, and may also include at least one of K2O, B2O3, CaO, MgO, ZnO, Y2O3, and a clarifying agent. These components are beneficial for lowering the melting temperature of the microcrystalline glass, regulating the properties of the glass forming material, and simultaneously regulating ion exchange to improve the stress strength and depth of the strengthened glass. However, excessive content may generate other impurity phases. Therefore, preferably, the addition amounts of each component, calculated by mass percentage, are as follows:
[0083] K2O: 0-1%;
[0084] B2O3: 0-1%;
[0085] CaO: 0-1%;
[0086] MgO: 0–1%;
[0087] ZnO: 0-1%;
[0088] Y2O3: 0-1%;
[0089] Clarifying agent: 0-1%.
[0090] The clarifying agent can be selected from those that are well-known to the public. Preferably, the clarifying agent includes at least one of SnO2 and CeO2.
[0091] In some embodiments, the glass-ceramic comprises 74% SiO2, 9.4% Al2O3, 2% P2O5, 8.8% Li2O, 2.8% Na2O and 3% ZrO2 by weight percentage.
[0092] In some embodiments, the glass-ceramic comprises 72.5% SiO2, 9.1% Al2O3, 2.1% P2O5, 9.5% Li2O, 2.9% Na2O, 2.9% ZrO2 and 1% B2O3 by weight percentage.
[0093] In some embodiments, the glass-ceramic comprises, by weight percentage, 73.6% SiO2, 8.2% Al2O3, 2.5% P2O5, 8.5% Li2O, 1.4% Na2O, 3.9% ZrO2, 0.8% K2O, 0.3% B2O3 and 0.8% Y2O3.
[0094] By adjusting the ratio of the above components, the obtained microcrystalline glass has the following properties:
[0095] The average grain size of the crystals is ≤50nm;
[0096] Average transmittance ≥90.5% in the 380nm–780nm range;
[0097] After undergoing the double 85 test, the average transmittance of the microcrystalline glass in the wavelength range of 380-780nm is ≥90.5%.
[0098] b value ≤ 0.45, where b value is the absolute value of the yellow-blue value when the thickness of the microcrystalline glass is 0.6 mm;
[0099] Haze ≤ 0.25;
[0100] The drop height is ≥1.6m.
[0101] The present invention also provides a method for preparing the microcrystalline glass as described above, comprising the following steps:
[0102] S10 involves weighing and mixing glass raw materials, then melting, clarifying, homogenizing, shaping, and annealing to obtain raw glass sheets.
[0103] S20 involves nucleating the raw glass plate, followed by crystallization, and then cooling to obtain the basic microcrystalline glass.
[0104] S30, the basic microcrystalline glass is chemically strengthened to obtain the microcrystalline glass.
[0105] In step S10, the raw glass sheet can also be cut according to size requirements. Furthermore, the glass raw materials can be formulated according to the component ratios of the microcrystalline glass of the present invention.
[0106] This step does not limit the method of forming the raw glass sheet; any method known to those skilled in the art can be selected, such as float glass forming, overflow forming, calendering, slot pull-down forming, or frit casting.
[0107] In some embodiments, the thickness of the raw glass obtained by the above process is 0.3 to 2 mm.
[0108] In step S20, the nucleation treatment temperature is preferably 530℃~580℃, and the nucleation treatment time is preferably 0.5h~1.5h. Specifically, in some embodiments, the nucleation treatment temperature can be 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 555℃, 565℃, or 575℃; and the nucleation treatment time can be 0.5h, 0.8h, 1.0h, 1.2h, 1.3h, or 1.5h.
[0109] The preferred temperature for crystallization is 640℃ to 740℃. The preferred crystallization time is 2 to 4 hours. Specifically, in some embodiments, the crystallization temperature can be 640℃, 650℃, 670℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 705℃, 715℃, 725℃, or 695℃; the crystallization time can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 2.8 hours, or 3.8 hours.
[0110] The nucleation and crystallization treatments described above can adjust the concentration of LiAlSi4O in the crystalline phase of the glass-ceramic. 10 Its content is greater than that of any other crystal phase.
[0111] In some embodiments, LiAlSi4O 10 The content of [something] is greater than that of Li2Si2O5.
[0112] In some embodiments, LiAlSi4O 10 The ratio of the content of to the content of Li2Si2O5 is ≥1.13.
[0113] In step S20, the base microcrystalline glass can also be trimmed, machined by CNC machine tool, or subjected to rough grinding or polishing.
[0114] In step S30, before chemical strengthening, the base glass-ceramic can be pretreated as follows: the base glass-ceramic is placed at 350–400°C for 20–40 minutes. Specifically, in some embodiments, the holding temperature can be 350°C, 370°C, 380°C, 390°C, or 400°C; the holding time can be 20 minutes, 25 minutes, 28 minutes, 30 minutes, 35 minutes, 38 minutes, or 40 minutes.
[0115] The chemical strengthening treatment in this step includes a bath salt, specifically, the base microcrystalline glass is placed in the bath salt for chemical strengthening treatment.
[0116] In some embodiments, the temperature and time for chemical fortification are 450°C to 520°C and 4 to 8 hours, respectively. Specifically, the temperature for chemical fortification can be 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, or 520°C, and the time for chemical fortification can be 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours, or 8 hours.
[0117] In some embodiments, the bath salt comprises 10 wt% to 40 wt% NaNO3 and 59 wt% to 90 wt% KNO3; and / or 0 wt% to 0.2 wt% LiNO3. It is understood that in some embodiments, the bath salt comprises 10 wt% to 40 wt% NaNO3 and 59 wt% to 90 wt% KNO3; in some embodiments, the bath salt comprises 10 wt% to 40 wt% NaNO3, 59 wt% to 90 wt% KNO3, and 0 wt% to 0.2 wt% LiNO3.
[0118] The microcrystalline glass obtained after the above chemical strengthening treatment has high hardness and good drop resistance, compressive stress and weather resistance. The glass surface is not prone to fogging, can adapt to high temperature and high humidity environments, and maintains good light transmittance.
[0119] In some embodiments, after the chemical strengthening treatment is completed, the glass-ceramic can be cleaned and dried to avoid residual contaminants affecting the strengthening effect.
[0120] The microcrystalline glass obtained by the technical solution of the present invention has excellent physical, chemical and mechanical properties. Microcrystalline glass products containing the microcrystalline glass described above have the same beneficial effects and can be widely used in the fields of displays, electronic smart terminals and photovoltaic power generation devices to play a protective role.
[0121] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention and are not intended to limit the present invention.
[0122] Example 1
[0123] Reference Figure 1 The method for preparing the microcrystalline glass of the present invention includes the following steps:
[0124] S10 involves weighing the glass raw materials, mixing them, melting them at 1380℃, then clarifying, homogenizing, shaping, annealing, and finally cutting them to obtain a 0.6mm thick plain glass sheet.
[0125] S20: The raw glass from step S10 is nucleated at 530°C for 0.5 h, then crystallized at 640°C for 2 h, and then cooled to room temperature to obtain the basic microcrystalline glass.
[0126] S30, the basic microcrystalline glass from step S20 is placed at 370°C for 30 minutes to complete the pretreatment, and then immersed in a salt bath at 450°C for chemical strengthening for 4 hours. The bath salts used in the salt bath include 0.2wt% LiNO3 + 40wt% NaNO3 + 59.8wt% KNO3.
[0127] Example 2
[0128] According to the proportion of glass raw materials in component 1 of Example 1 in Table 1, raw glass was prepared according to the preparation method in step S10 of Example 1. Then, eight groups of basic glass crystals were prepared according to the conditions in step S20 of Example 2 in Table 2. The properties of the obtained basic glass crystals are shown in Table 2.
[0129] Example 3
[0130] According to the proportion of glass raw materials in component 1 of Example 1 in Table 1, raw glass was obtained by preparing it according to the preparation method in step S10 of Example 1. Basic glass was prepared according to condition 1 of Example 2 in step S20 of Table 2. The basic glass was prepared according to the conditions in step S30 of Table 3 to obtain 5 groups of glass. The properties of the 5 groups of glass are shown in Table 3.
[0131] Comparative Example 1
[0132] According to the proportion of glass raw materials in Comparative Component 1 in Table 1, glass raw materials were weighed and prepared according to the preparation method of steps S10 to S30 in Example 1. The properties are shown in Table 1.
[0133] Comparative Example 2
[0134] According to the proportion of glass raw materials in component 1 of Example 1 in Table 1, the raw glass was prepared according to the preparation method in step S10 of Example 1, and the basic glass was prepared according to the conditions of comparative example 2 in step S20 of Table 2. The properties of the basic glass are shown in Table 2.
[0135] Comparative Example 3
[0136] Five groups of microcrystalline glasses were prepared by following the preparation conditions of step S30 in Table 3, based on the basic microcrystalline glass obtained in Comparative Example 2.
[0137] Performance testing
[0138] Performance tests were conducted on the products of the embodiments and comparative examples, and the results are shown in Tables 1 and 2. Unless otherwise specified, the test methods for each test item are conventional methods in the art. Details are as follows:
[0139] (1) Crystal phase and crystallinity: The crystal phase is determined by comparing the XRD diffraction peaks with the database spectrum. The crystallinity is obtained by calculating the proportion of the diffraction intensity of the crystal phase in the overall spectrum intensity using the Rietveld method.
[0140] (2) Average grain size: The average grain size was determined using a scanning electron microscope (SEM). The microcrystalline glass was surface-treated in HF acid and then chromium-sprayed onto the surface. The surface was scanned under a scanning electron microscope (SEM) to observe the diameter of the grains. The average diameter of all grain profiles was summed and divided by the number of grains in the SEM image.
[0141] (3) The color b value was tested using a Datacolor 650 ultra-high precision desktop spectrophotometer.
[0142] (4) Visible light transmittance was tested using a spectrophotometer in accordance with standard ISO13468-1:1996.
[0143] (5) Double 85 test: The test temperature is set to 85℃ and the humidity is set to 85%. The reliability test is conducted on the test sample for 1000 hours.
[0144] (6) Drop performance of the whole machine sandpaper: The test was conducted by a mobile phone controlled drop tester. The specific test conditions were: 80 grit sandpaper, 195g total weight, 60cm base height, increasing by 10cm, once per height, until it broke.
[0145] In this paper, unless otherwise stated, the products of each embodiment and comparative example after ion exchange were tested using a Japanese Orihara FSM-6000LE+SLP1000 surface stress analyzer. Here, CS refers to the compressive stress value of the surface of the tempered glass; CS-30 refers to the compressive stress value at a depth of 30 micrometers after the tempered glass sample was strengthened with mixed salt; and DOC refers to the ion exchange depth of the compressive stress layer of the tempered glass.
[0146] Table 1. Composition ratios and properties of the microcrystalline glass in Example 1 and Comparative Example 1.
[0147]
[0148]
[0149] Table 2. Preparation conditions of step S20 in Example 2 and Comparative Example 2 and the properties of their base glass-ceramics.
[0150]
[0151]
[0152] Table 3. Preparation conditions and microcrystalline glass properties of step S30 in Example 3.
[0153]
[0154] Table 4 Comparative Example 3: Preparation conditions of step S30 and its properties of the glass-ceramic.
[0155]
[0156] As shown in the table above, the microcrystalline glass obtained by using the technical solution of this invention in the embodiments of this invention has a crystallinity ≥55%, an average crystal particle size ≤50nm, and a crystalline phase of LiAlSi4O. 10 The content is greater than that of Li2Si2O5, and the crystal phase is LiAlSi4O 10 The ratio of the content of [unspecified substance] to the content of Li2Si2O5 is ≥1.13, the b-value is ≤0.45, the average transmittance in the range of 380nm to 780nm is ≥90.5%, and the haze is ≤0.25. Moreover, after chemical strengthening treatment, the surface of the microcrystalline glass is clean after the double 85 test, it is not easy to fog up, maintains good transmittance, has good weather resistance, is not easy to age, can resist high temperature and high humidity environments, and also has high hardness, excellent compressive stress and drop resistance.
[0157] In Comparative Example 1, the excessive addition of P2O5 in the microcrystalline glass, reaching 4%, led to the degradation of LiAlSi4O 10 The content of [unspecified substance] is less than that of Li2Si2O5. The b-value and haze of the microcrystalline glass are relatively large, at 0.75 and 0.55% respectively. The transmittance of 0.6mm microcrystalline glass at 560nm is only 89.2%. After the double 85 test, the glass surface becomes hazy, and the transmittance of 0.6mm microcrystalline glass at 560nm is only 65.3%.
[0158] Comparative Example 2 had an excessively long nucleation time, which did not meet the requirements for preparing the microcrystalline glass of this invention. Before chemical strengthening, the crystal phase of the obtained basic microcrystalline glass contained LiAlSi4O. 10 The content of is equal to the content of Li2Si2O5.
[0159] Comparative Example 3 is a microcrystalline glass obtained by chemically strengthening the basic microcrystalline glass obtained in Comparative Example 2. After the microcrystalline glass was subjected to the double 85 test, the glass surface showed a fogging phenomenon, and the transmittance of 560nm of the 0.6mm microcrystalline glass was less than 70%. The microcrystalline glass had poor weather resistance, was prone to aging, and was not suitable for high temperature and high humidity environments.
[0160] The above are merely preferred embodiments of the present invention and do not limit the scope of the patent. Any equivalent structural or procedural transformations made based on the description and drawings of the present invention, or direct or indirect applications in other related technical fields, are similarly included within the scope of patent protection of the present invention.
Claims
1. A microcrystalline glass, characterized in that, The microcrystalline glass has a crystallinity of ≥55% and its crystalline phase includes LiAlSi4O. 10 and Li2Si2O5, wherein the LiAlSi4O 10 Its content is greater than that of any other crystalline phase; The LiAlSi4O 10 The ratio of the content of [certain substances] to the content of Li2Si2O5 is ≥1.33; The microcrystalline glass contains the following components by weight percentage: 69%~75% SiO2; 6%–12% Al2O3; 1.7%–3.5% P2O5; 8%–13% Li₂O; 0.1%–3% Na₂O; 2%–4.5% ZrO2; The average grain size of the crystals in the microcrystalline glass is ≤50nm; After undergoing the double 85 test, the average transmittance of the microcrystalline glass in the wavelength range of 380-780nm is ≥90.5%. The haze of the microcrystalline glass is ≤0.25; The conditions for the dual 85 experiment are as follows: the test temperature is set to 85℃, the humidity is set to 85%, and the reliability test is conducted on the test sample for 1000 hours.
2. The microcrystalline glass according to claim 1, characterized in that, The crystal phase of the microcrystalline glass also includes at least one of Li2SiO3, Li3PO4, and β-spodumene.
3. The microcrystalline glass according to claim 1, characterized in that, The microcrystalline glass contains the following components by weight percentage: 71%~74% SiO2; 7%–10% Al2O3; 2%–3.5% P2O5; 10%–12% Li₂O; 0.5%–2% Na₂O; 2.5% to 4.5% ZrO2.
4. The microcrystalline glass according to any one of claims 1 to 3, characterized in that, The microcrystalline glass also contains the following components by weight percentage: K2O: 0-1%; B2O3: 0–1%; CaO: 0-1%; MgO: 0–1%; ZnO: 0–1%; Y2O3: 0–1%; Clarifying agent: 0-1%.
5. The microcrystalline glass according to claim 1, characterized in that, The b-value of the microcrystalline glass is ≤0.45, wherein the b-value is the absolute value of the yellow-blue value when the thickness of the microcrystalline glass is 0.6 mm; And / or, the drop height of the microcrystalline glass is ≥1.6m.
6. A method for preparing the microcrystalline glass according to any one of claims 1 to 5, characterized in that, Includes the following steps: Weigh the glass raw materials, mix them, melt, clarify, homogenize, shape, and anneal to obtain raw glass sheets; The raw glass plate is subjected to nucleation treatment, followed by crystallization treatment, and then cooled to obtain basic microcrystalline glass; The basic glass-ceramic is chemically strengthened to obtain the glass-ceramic.
7. The method for preparing microcrystalline glass according to claim 6, characterized in that, The nucleation treatment temperature is 530℃~580℃, and the nucleation treatment time is 0.5h~1.5h; And / or, the crystallization treatment temperature is 640℃~740℃, and the crystallization treatment time is 2~4h.
8. The method for preparing microcrystalline glass according to claim 6, characterized in that, The chemical enhancement treatment includes a bath salt containing 10wt% to 40wt% NaNO3, 59wt% to 90wt% KNO3, and 0wt% to 0.2wt% LiNO3.
9. The method for preparing microcrystalline glass according to claim 6, characterized in that, The chemical strengthening temperature is 450℃~520℃, and the chemical strengthening time is 4~8h.
10. A microcrystalline glass product, characterized in that, The microcrystalline glass product includes the microcrystalline glass according to any one of claims 1 to 5, and the microcrystalline glass product is used in the fields of display screens, electronic smart terminals and photovoltaic power generation devices.
Citation Information
Patent Citations
Glass composition, microcrystalline glass as well as preparation method and application of microcrystalline glass
CN114195392A
Glass composition, microcrystalline glass as well as preparation method and application of microcrystalline glass
CN114195394A
Glass-ceramics, preparation method thereof, and glass-ceramics product
CN115716709B