A bionic optical film and preparation method thereof

By preparing modified polycarbonate, using raw materials such as nadic acid anhydride and propylene oxide, and introducing unsaturated double bonds and metallic zinc elements, the problem of insufficient strength and toughness of existing bionic optical film materials has been solved, and the light transmittance of the material has been improved. and mechanical properties, suitable for high-end optical film applications.

CN118206786BActive Publication Date: 2024-10-25SHENZHEN FORBEST OPTOELECTRONIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410458061.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-10-25
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

Existing bionic optical film materials have deficiencies in strength and toughness, poor uniformity, and weak interface bonding, which limits their application in optical devices.

Method used

By preparing double-bonded polycarbonate, epoxidized polycarbonate and modified polycarbonate, using raw materials such as nadic anhydride, propylene oxide and tetraaminophthalocyanine zinc, and introducing unsaturated double bonds and metallic zinc elements, the improvement of Translucency and mechanical properties of materials.

Benefits of technology

It significantly improves the strength and toughness of optical films, enhances visible light transmittance, and is suitable for high-end bionic optical film applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118206786B_ABST
    Figure CN118206786B_ABST
Patent Text Reader

Abstract

The present invention relates to a bionic optical film and a preparation method thereof, the preparation method comprising the following steps: (1) preparing double-bonded polycarbonate; (2) preparing epoxidized polycarbonate; (3) preparing modified polycarbonate: weighing tetraaminophthalocyanine zinc, epoxidized polycarbonate and N,N-dimethylformamide, mixing, heating and stirring to react, and obtaining modified polycarbonate; (4) preparing an optical film: dispersing the modified polycarbonate in an organic solvent, fully mixing, coating it on a mold substrate, drying and demoulding, and obtaining a bionic optical film. The present invention prepares a novel optical film material, which is modified on the basis of bionic material polycarbonate. Compared with traditional polycarbonate, the optical film material prepared by the present invention has better strength and toughness, and can also improve its light transmittance to a certain extent, so that it is more suitable for application in high-end bionic optical films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of optical films, and in particular to a bionic optical film and a preparation method thereof. Background Art

[0002] After billions of years of evolution, organisms have not only adapted to survive in nature, but also adapted to a near-perfect degree. Some of the wonderful functions of organisms far exceed human beings' previous designs, and at the same time provide answers to difficult problems for humans. The exploration of some intelligent surfaces in nature provides an effective way to design bionic materials and builds a bridge between biology and other disciplines. From the perspective of materials science, we can further study the structure and function of natural biomaterials, and finally find ways and methods to solve problems by reproducing the principles of the special functions of organisms.

[0003] The compound eyes of moths are composed of an array of nanostructures arranged in an orderly hexagonal pattern. This array is considered to be a homogeneous transparent layer on the surface of the cornea. Each nanostructure protrusion is an anti-reflection unit, which produces low reflectivity, making it look abnormally black and difficult to detect even when flying at night. This is called the moth eye effect. The cornea of ​​butterflies also has similar moth eye nanostructures. The sizes of the nanostructures of the compound eyes of different types of butterflies are different, resulting in different degrees of anti-reflection on the surface. The greater the height of the nanostructure, the lower the reflectivity of its surface. Subwavelength moth eye bionic optical film is a new generation of screen high-definition display technology, which has high screen resolution, strong color saturation, high color reproduction, anti-glare ultra-high definition, eye protection, radiation protection and blue light protection. It effectively suppresses reflected light and increases the transmission of the optical display system, improves the clarity and resolution of the optical display system, suppresses the stray light, glare and ghosting caused by reflection and refraction between the interfaces in the optical system, and suppresses strong light radiation in the blue band.

[0004] With the development of technology, the requirements for optical devices in the fields of optical instruments and optoelectronic systems are getting higher and higher. Among these materials, optical lenses are the main ones, and bionic materials are widely used in optical lenses. However, for current bionic materials, organic-inorganic heterogeneous structures usually have poor uniformity, weak interface bonding, and various defects, which limits the breakthrough of such materials in strength and toughness. Summary of the invention

[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a bionic optical film and a preparation method thereof.

[0006] The purpose of the present invention is achieved by the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a bionic optical film, comprising the following steps:

[0008] (1) Preparation of double-bonded polycarbonate:

[0009] Propylene oxide and nadic anhydride are weighed and mixed into a reaction kettle, and a catalyst is added, and then carbon dioxide is introduced into the reaction kettle, and the temperature and pressure are increased to react. After the reaction is completed, the product is recrystallized and dried to obtain a double-bonded polycarbonate;

[0010] (2) Preparation of epoxidized polycarbonate:

[0011] The double-bonded polycarbonate and chloroform are mixed, stirred at room temperature, and then the catalyst is added, and the stirring is continued for 25-35 hours. After the reaction is completed, the reaction liquid is discharged into ice ethanol and dried to obtain epoxidized polycarbonate;

[0012] (3) Preparation of modified polycarbonate:

[0013] Weighing zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide, mixing them in a reaction container, heating and stirring under the protection of an inert gas, cooling to room temperature, concentrating under reduced pressure, precipitating in ice ethanol, and drying to obtain a modified polycarbonate;

[0014] (4) Preparation of optical films:

[0015] The modified polycarbonate is dispersed in an organic solvent, fully mixed, coated on a mold substrate, and dried and demoulded to obtain a bionic optical film.

[0016] Preferably, in the process of preparing the double-bonded polycarbonate, the mass ratio of propylene oxide to nadic anhydride is 1:0.2-0.28.

[0017] Preferably, in the process of preparing the double-bonded polycarbonate, the catalyst is tetrabutylammonium chloride, and the added amount is 1%-5% of the mass of propylene oxide.

[0018] Preferably, in the process of preparing the double-bonded polycarbonate, after the carbon dioxide is introduced, the pressure inside the reactor is maintained at 4.5-6.5 MPa.

[0019] Preferably, in the process of preparing the double-bonded polycarbonate, the reaction temperature is 75-95° C. and the reaction time is 15-20 h.

[0020] Preferably, in the process of preparing the double-bonded polycarbonate, the recrystallized product is prepared by first dissolving the reaction product in chloroform and then recrystallizing it in ice ethanol.

[0021] Preferably, in the process of preparing the epoxidized polycarbonate, the mass volume ratio of the double-bonded polycarbonate to chloroform is 1 g:(10-20) mL.

[0022] Preferably, in the process of preparing the epoxidized polycarbonate, the catalyst is m-chloroperbenzoic acid, and the mass ratio of the catalyst to the double-bonded polycarbonate is 1:1.2-1.8.

[0023] Preferably, in the process of preparing the epoxidized polycarbonate, the catalyst is gradually added within 1 hour, and stirring is continued for 25-35 hours after the addition is completed.

[0024] Preferably, in the process of preparing the epoxidized polycarbonate, the discharge in the icy ethanol is to centrifuge the reaction solution to collect the supernatant, pour it into the icy ethanol and slowly stir for 10-20 hours, and then collect the lower precipitate.

[0025] Preferably, in the process of preparing the modified polycarbonate, the mass volume ratio of zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide is (0.67-0.84) g: 1 g: (10-20) mL.

[0026] Preferably, in the process of preparing the modified polycarbonate, the reaction temperature is 55-65° C. and the reaction time is 10-20 h.

[0027] Preferably, in the process of preparing the optical film, the organic solvent is ethyl acetate or dichloromethane, and the mass ratio of the modified polycarbonate to the organic solvent is 2-4:10.

[0028] In a second aspect, the present invention provides a bionic optical film prepared by the above-mentioned preparation method.

[0029] The beneficial effects of the present invention are:

[0030] 1. The present invention prepares a new type of optical film material, which is modified on the basis of the bionic material polycarbonate. Compared with the traditional polycarbonate, the optical film material prepared by the present invention has better strength and toughness, and can also improve its light transmittance to a certain extent, so that it is more suitable for application in high-end bionic optical films.

[0031] 2. The present invention uses carbon dioxide, nadic anhydride and propylene oxide as main raw materials to synthesize carbon dioxide-based polyester polycarbonate under high temperature and high pressure. The nadic anhydride introduced into the polycarbonate is an unsaturated anhydride, so it contains unsaturated double bond groups, that is, double-bonded polycarbonate is obtained; then, the double-bonded polycarbonate is oxidized under specific conditions by using meta-chloroperbenzoic acid as an organic peroxy catalyst, and the double bond groups are oxidized to epoxy groups, that is, epoxidized polycarbonate is obtained; then, tetraaminophthalocyanine zinc containing an amino group is reacted with the epoxidized polycarbonate, and the phthalocyanine group and the zinc element are introduced into the polycarbonate by utilizing the combination reaction of the amino group and the epoxy group under the action of temperature increase, so as to obtain a modified polycarbonate.

[0032] 3. The present invention modifies polycarbonate by introducing metal zinc elements and chemical groups such as phthalocyanine through multi-polymerization, which not only enhances the visible light transmittance of the film material, but also greatly improves the strength and toughness performance of the optical film. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0034] Figure 1 Schematic diagram of the product of modified polycarbonate (M-PC) prepared in Example 1 of the present invention;

[0035] Figure 2 It is a schematic diagram of the infrared spectrum of the modified polycarbonate (M-PC) prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0037] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0038] The present invention will be further described below in conjunction with the following examples.

[0039] Example 1

[0040] A method for preparing a bionic optical film comprises the following steps:

[0041] (1) Preparation of double-bonded polycarbonate:

[0042] Propylene oxide (PO) and nadic anhydride (NADI) are weighed and mixed into a vacuum reactor in a mass ratio of propylene oxide to nadic anhydride of 1:0.24. A catalyst tetrabutylammonium chloride (TBAC) is added in an amount of 3% of the mass of propylene oxide. A sufficient amount of carbon dioxide is then introduced into the reactor, and the pressure inside the reactor is maintained at 5.5 MPa and the temperature is maintained at 85°C. The reaction is carried out under heat and pressure for 18 hours. After the reaction is completed, the temperature is lowered to room temperature, the reaction product is dissolved in chloroform, and then recrystallized in ice ethanol. After vacuum drying, double-bonded polycarbonate (D-PC) is obtained.

[0043] (2) Preparation of epoxidized polycarbonate:

[0044] Double-bonded polycarbonate (D-PC) and chloroform are mixed in a reaction container, the mass volume ratio of double-bonded polycarbonate to chloroform is 1g:15mL, inert gas is introduced as protective gas, and the mixture is fully stirred at room temperature. Then, the catalyst m-chloroperbenzoic acid (m-CPBA) is gradually added within 1 hour, and the mass ratio of the catalyst to the double-bonded polycarbonate is 1:1.5. The reaction liquid is continuously stirred during the addition process. After all the catalyst is added, stirring is continued for 30 hours. After the reaction is completed, the reaction liquid is centrifuged to collect the supernatant, poured into ice ethanol and slowly stirred for 15 hours, and the lower precipitate is collected by centrifugation again. After vacuum drying, epoxidized polycarbonate (E-PC) is obtained.

[0045] (3) Preparation of modified polycarbonate:

[0046] Weigh tetraaminophthalocyanine zinc (TAPcZn, C 32 H 20 N 12 Zn), epoxidized polycarbonate (E-PC) and N,N-dimethylformamide (DMF) are mixed in a reaction container, the mass volume ratio of zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide is 0.75g:1g:15mL, under the protection of inert gas, the temperature is raised to 60°C, stirred for 15 hours, then cooled to room temperature, concentrated under reduced pressure, precipitated in ice ethanol, and dried in vacuum to obtain modified polycarbonate (M-PC).

[0047] (4) Preparation of optical films:

[0048] The modified polycarbonate is dispersed in ethyl acetate, with the mass ratio of the modified polycarbonate to the ethyl acetate being 3:10. After being fully mixed, the modified polycarbonate is coated on a mold substrate, and after being dried and demolded, a bionic optical film is obtained.

[0049] Figure 1 This is a schematic diagram of the product of the modified polycarbonate (M-PC) prepared in Example 1.

[0050] Figure 2 The infrared spectrum (FT-IR) of the modified polycarbonate (M-PC) prepared in Example 1 shows that at 2238 cm -1 and 1015cm -1 Typical stretching vibration peaks of phthalocyanine groups appeared at 2238 cm -1 The nitrile group (-CN) of the phthalocyanine group is at 1015 cm -1 The peak at is the skeleton vibration peak of the phthalocyanine group, indicating that the modified polycarbonate (M-PC) prepared in Example 1 successfully introduced the phthalocyanine group into the polycarbonate.

[0051] Example 2

[0052] A method for preparing a bionic optical film comprises the following steps:

[0053] (1) Preparation of double-bonded polycarbonate:

[0054] Weigh propylene oxide (PO) and nadic anhydride (norbornene diacid anhydride, EA) and mix them into a vacuum reactor in a mass ratio of propylene oxide to nadic anhydride of 1:0.2, and add catalyst tetrabutylammonium chloride (TBAC) in an amount of 1% of the mass of propylene oxide. Then, introduce sufficient carbon dioxide into the reactor, maintain the pressure inside the reactor at 4.5 MPa and the temperature at 75°C, and react for 15 hours under heat and pressure. After the reaction is completed, cool to room temperature, dissolve the reaction product in chloroform, and then recrystallize in ice ethanol. After vacuum drying, double-bonded polycarbonate (D-PC) is obtained.

[0055] (2) Preparation of epoxidized polycarbonate:

[0056] Double-bonded polycarbonate (D-PC) and chloroform are mixed in a reaction container, the mass volume ratio of double-bonded polycarbonate to chloroform is 1g:10mL, inert gas is introduced as protective gas, and the mixture is fully stirred at room temperature. Then, the catalyst m-chloroperbenzoic acid (m-CPBA) is gradually added within 1 hour, and the mass ratio of the catalyst to the double-bonded polycarbonate is 1:1.2. The reaction liquid is continuously stirred during the addition process. After all the catalyst is added, stirring is continued for 25 hours. After the reaction is completed, the reaction liquid is centrifuged to collect the supernatant, poured into ice ethanol and slowly stirred for 10 hours, and the lower precipitate is collected by centrifugation again. After vacuum drying, epoxidized polycarbonate (E-PC) is obtained.

[0057] (3) Preparation of modified polycarbonate:

[0058] Weigh tetraaminophthalocyanine zinc (TAPcZn, C 32 H 20 N 12Zn), epoxidized polycarbonate (E-PC) and N,N-dimethylformamide (DMF) are mixed in a reaction container, the mass volume ratio of zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide is 0.67g:1g:10mL, under the protection of inert gas, the temperature is raised to 55°C, stirred for 10 hours, then cooled to room temperature, concentrated under reduced pressure, precipitated in ice ethanol, and dried in vacuum to obtain modified polycarbonate (M-PC).

[0059] (4) Preparation of optical films:

[0060] The modified polycarbonate is dispersed in dichloromethane with a mass ratio of the modified polycarbonate to the dichloromethane being 2:10. After being fully mixed, the modified polycarbonate is coated on a mold substrate. After drying and demolding, a bionic optical film is obtained.

[0061] Example 3

[0062] A method for preparing a bionic optical film comprises the following steps:

[0063] (1) Preparation of double-bonded polycarbonate:

[0064] Propylene oxide (PO) and nadic anhydride (NADI) are weighed and mixed into a vacuum reactor in a mass ratio of propylene oxide to nadic anhydride of 1:0.28. A catalyst tetrabutylammonium chloride (TBAC) is added in an amount of 5% of the mass of propylene oxide. A sufficient amount of carbon dioxide is then introduced into the reactor, and the pressure inside the reactor is maintained at 6.5 MPa and the temperature is maintained at 95°C. The reaction is carried out under heat and pressure for 20 hours. After the reaction is completed, the temperature is lowered to room temperature, and the reaction product is dissolved in chloroform, then recrystallized in ice ethanol, and vacuum dried to obtain double-bonded polycarbonate (D-PC).

[0065] (2) Preparation of epoxidized polycarbonate:

[0066] Double-bonded polycarbonate (D-PC) and chloroform are mixed in a reaction container, the mass volume ratio of double-bonded polycarbonate to chloroform is 1g:20mL, inert gas is introduced as protective gas, and the mixture is fully stirred at room temperature. Then, the catalyst m-chloroperbenzoic acid (m-CPBA) is gradually added within 1 hour, and the mass ratio of the catalyst to the double-bonded polycarbonate is 1:1.8. The reaction liquid is continuously stirred during the addition process. After all the catalyst is added, stirring is continued for 35 hours. After the reaction is completed, the reaction liquid is centrifuged to collect the supernatant, poured into ice ethanol and slowly stirred for 20 hours, and the lower precipitate is collected by centrifugation again. After vacuum drying, epoxidized polycarbonate (E-PC) is obtained.

[0067] (3) Preparation of modified polycarbonate:

[0068] Weigh tetraaminophthalocyanine zinc (TAPcZn, C32 H 20 N 12 Zn), epoxidized polycarbonate (E-PC) and N,N-dimethylformamide (DMF) are mixed in a reaction container, the mass volume ratio of zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide is 0.84g:1g:20mL, under the protection of inert gas, the temperature is raised to 65°C, stirred for 20 hours, then cooled to room temperature, concentrated under reduced pressure, precipitated in ice ethanol, and dried in vacuum to obtain modified polycarbonate (M-PC).

[0069] (4) Preparation of optical films:

[0070] The modified polycarbonate is dispersed in ethyl acetate or dichloromethane, with the mass ratio of the modified polycarbonate to ethyl acetate or dichloromethane being 4:10. After being fully mixed, the modified polycarbonate is coated on a mold substrate, and after drying and demolding, a bionic optical film is obtained.

[0071] Comparative Example 1

[0072] A method for preparing a bionic optical film, which is different from Example 1 in that polycarbonate is prepared in a traditional way, and the prepared polycarbonate (PC) is used as the material of the bionic optical film. The specific method of the polycarbonate includes:

[0073] Weigh propylene oxide (PO) and add it into a vacuum reactor, and add catalyst tetrabutylammonium chloride (TBAC) in an amount of 3% of the mass of propylene oxide. Then, introduce sufficient carbon dioxide into the reactor, maintain the pressure inside the reactor at 5.5 MPa and the temperature at 85°C, and react for 18 hours under heat and pressure. After the reaction is completed, cool to room temperature, dissolve the reaction product in chloroform, and then recrystallize in ice ethanol. After vacuum drying, polycarbonate (PC) is obtained.

[0074] Comparative Example 2

[0075] A method for preparing a bionic optical film, which differs from Example 1 in that double-bonded polycarbonate (D-PC) is prepared as the material of the bionic optical film, and the preparation method is the same as step (1) of Example 1.

[0076] Comparative Example 3

[0077] A method for preparing a bionic optical film, which differs from Example 1 in that epoxidized polycarbonate (E-PC) is prepared as the material of the bionic optical film, and the preparation method is the same as step (1) of Example 1.

[0078] The bionic optical films prepared in Example 1 and Comparative Examples 1-3 were tested and compared in terms of performance, and the results are shown in Table 1:

[0079] Table 1 Performance of different bionic optical films

[0080]

[0081] It can be seen from the test results in Table 1 that the light transmittance of the bionic optical film prepared in Example 1 can reach 91.2%, and the haze is 0.2%, indicating that it has good performance in optical properties; in addition, the tensile strength and impact strength are greatly improved.

[0082] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0083] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a bionic optical film, characterized in that: The following steps are involved: (1) Preparation of double-bonded polycarbonate: Propylene oxide and nadic anhydride are weighed and mixed into a reaction kettle, and a catalyst is added, and then carbon dioxide is introduced into the reaction kettle, and the temperature and pressure are increased to react. After the reaction is completed, the product is recrystallized and dried to obtain a double-bonded polycarbonate; (2) Preparation of epoxidized polycarbonate: The double-bonded polycarbonate and chloroform are mixed, stirred at room temperature, and then the catalyst is added, and the stirring is continued for 25-35 hours. After the reaction is completed, the reaction liquid is discharged into ice ethanol and dried to obtain epoxidized polycarbonate; (3) Preparation of modified polycarbonate: Weighing zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide, mixing them in a reaction container, heating and stirring under the protection of an inert gas, cooling to room temperature, concentrating under reduced pressure, precipitating in ice ethanol, and drying to obtain a modified polycarbonate; (4) Preparation of optical films: The modified polycarbonate is dispersed in an organic solvent, mixed sufficiently, and then coated on a mold substrate, and after drying and demoulding, a bionic optical film is obtained; In the process of preparing the double-bonded polycarbonate, the mass ratio of propylene oxide to nadic anhydride is 1:0.2-0.28; In the process of preparing the epoxidized polycarbonate, the catalyst is m-chloroperbenzoic acid, and the mass ratio of the catalyst to the double-bonded polycarbonate is 1:1.2-1.8; In the process of preparing the modified polycarbonate, the mass volume ratio of zinc tetraaminophthalocyanine, epoxidized polycarbonate and N,N-dimethylformamide is (0.67-0.84) g:1 g:(10-20) mL.

2. The method for preparing a bionic optical film according to claim 1, characterized in that: In the process of preparing the double-bonded polycarbonate, the catalyst is tetrabutylammonium chloride, and the added amount is 1%-5% of the mass of propylene oxide.

3. The method for preparing a bionic optical film according to claim 1, characterized in that: In the process of preparing the double-bonded polycarbonate, after the carbon dioxide is introduced, the pressure inside the reactor is maintained at 4.5-6.5 MPa; the reaction temperature is 75-95° C., and the reaction time is 15-20 h.

4. The method for preparing a bionic optical film according to claim 1, characterized in that: In the process of preparing the epoxidized polycarbonate, the mass volume ratio of the double-bonded polycarbonate and chloroform is 1 g: (10-20) mL.

5. The method for preparing a bionic optical film according to claim 1, characterized in that: During the preparation of the epoxidized polycarbonate, the catalyst is gradually added within 1 hour, and stirring is continued for 25-35 hours after the addition is completed.

6. The method for preparing a bionic optical film according to claim 1, characterized in that: In the process of preparing the modified polycarbonate, the reaction temperature is 55-65° C. and the reaction time is 10-20 hours.

7. The method for preparing a bionic optical film according to claim 1, characterized in that: In the process of preparing the optical film, the organic solvent is ethyl acetate or dichloromethane, and the mass ratio of the modified polycarbonate to the organic solvent is 2-4:

10.