A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume and a preparation method thereof
By using polymeric bromine flame retardant and antimony trioxide in PBT/PET alloy materials, combining phosphate and silicone flame retardant to form an insulating and dense layer, the existing materials have been solved at high temperatures, and the GWIT low and smoke are low at high temperatures. The problem is that high flame retardant and low smoke emissions are achieved.
Patent Information
- Application Number
- CN202410328647.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Existing flame retardant PBT/PET alloy materials have lower GWIT and produce more smoke and toxic gases when burned at high temperatures, which poses a threat to the human body and the environment.
The polymerized bromine flame retardant and antimony trioxide are combined with phosphate and silicone flame retardant to form an insulating and dense silicon dioxide layer, which inhibits combustion and generates an inorganic thermal insulation protection layer, and reduces smoke generation. and improve flame retardant effect.
It achieves high GWIT, low smoke output, and low harmful flame retardant effects, improves physical and mechanical properties and environmental performance, and meets environmental protection requirements.
Smart Images

Figure BDA0004752818850000061 
Figure BDA0004752818850000071 
Figure BDA0004752818850000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and more specifically, to a flame-retardant PBT and PET alloy material with high GWIT and low smoke volume and a preparation method thereof. Background Art
[0002] Polybutylene terephthalate (PBT) is a polymer made of terephthalic acid and butanediol through a polycondensation reaction. Currently, glass fiber reinforced PBT materials have been widely used in lighting fixtures, cooling fans, connectors, coil skeletons, electrical housings and other electronic and electrical components. With the development of technology, people have higher and higher requirements for the performance of PBT modified materials, and at the same time, cost pressure has forced changes. In this case, glass fiber reinforced PBT and PET alloy materials with better performance have come into being. Polyethylene terephthalate (PET) has good heat resistance and low cost, and PET can effectively prevent the exposure of glass fibers in the glass fiber reinforced PBT system, achieving a high gloss effect on the product surface.
[0003] When glass fiber reinforced PBT / PET alloy is used in rail transportation, building materials, cables and other industries, flame retardancy is indispensable. By adopting a bromine-antimony compound system, it has the advantages of high flame retardant efficiency and good flame retardant effect. However, conventional flame retardant PBT / PET plastics can only meet the V0 flame retardant requirements of UL-94. For the IEC glow wire test, its glow wire ignition temperature (GWIT) is relatively low, usually only about 750°C. With the upgrading of electronic components products, higher requirements are put forward for the GWIT of PBT / PET.
[0004] The Chinese invention patent document with application number CN202011588124.8 in the prior art discloses a high GWIT flame-retardant PBT / PET alloy material, which includes the following components by weight: 13 to 48 parts of PBT resin, 5 to 40 parts of PET resin, 8 to 10 parts of brominated flame retardant, 0.5 to 1 part of antimony trioxide, 3 to 6 parts of calcium hydroxide, and 25 to 35 parts of alkali-free glass fiber.
[0005] With regard to the above-mentioned related technologies, the inventors found that although the GWIT of PBT and PET alloy materials can reach 850°C, the use of strong alkali calcium hydroxide has irritating and corrosive effects, which will cause harm to the human body during use. In addition, the use of brominated flame retardants and antimony trioxide in combination will produce more smoke and toxic gases during combustion, posing a great threat to human life safety and the living environment. Summary of the invention
[0006] In order to reduce the smoke emission during combustion of PBT / PET composite materials and improve the flame retardant effect, the present application provides a flame retardant PBT and PET alloy material with high GWIT and low smoke emission and a preparation method thereof.
[0007] In the first aspect, the present application provides a flame retardant PBT and PET alloy material with high GWIT and low smoke volume, adopting the following technical solution:
[0008] A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume comprises the following raw materials in parts by weight: 20-45 parts of PBT resin, 5-15 parts of PET resin, 2-4.8 parts of toughening agent, 30-35 parts of alkali-free glass fiber, 9-11 parts of polymeric bromine flame retardant, 0.5-2 parts of antimony trioxide, 9-10 parts of flame retardant synergist, 0.1-0.3 parts of antioxidant, and 0.2-0.6 parts of lubricant, wherein the flame retardant synergist comprises phosphate and silicone flame retardant in a mass ratio of 0.5-1:1.
[0009] By adopting the above technical scheme, a polymeric brominated flame retardant and antimony trioxide are used in combination. The polymeric brominated flame retardant has a high molecular weight, good compatibility with PBT and PET, excellent light and heat stability, good fluidity, and good process adaptability. It does not produce halogenated dibenzodioxanes and halogenated dibenzopyrans during combustion, has good safety in use, and has comprehensively improved physical and mechanical properties, environmental properties, and stability. Antimony trioxide and the polymeric brominated flame retardant work together to extinguish flames in a gaseous state. The phosphate in the flame retardant synergist forms polymetaphosphoric acid during the combustion process, which has great The strong dehydration effect dehydrates and carbonizes the polymer, changes the mode of the polymer combustion process, and forms a carbon layer on its surface to isolate the air, thereby exerting a stronger flame retardant effect. When burning, the silicone flame retardant will generate an inorganic thermal insulation protective layer containing Si-O bonds and Si-C bonds, which is unique to silicone. It not only prevents the decomposition products generated by combustion from escaping, but also inhibits the thermal decomposition of polymer materials, achieving the effects of high flame retardancy, low smoke emission, and low harmfulness, thereby preparing PBT and PET alloy materials with low smoke emission, high GWIT, good flame retardancy, high mechanical strength, and meeting environmental protection requirements.
[0010] Optionally, the organosilicon-based flame retardant includes polyborosiloxane, phenyl silicone resin and polytetrafluoroethylene in a mass ratio of 1:1-1.5:0.1-0.3.
[0011] By adopting the above technical scheme, during the combustion process of the alloy material, the phenyl silicone resin is first enriched from the inside of the material to the combustion surface, forming a large number of Si-C bonds at about 350°C, and combining with the O element to form Si-O bonds at about 450°C, and finally forming an insulating and dense silicon dioxide layer on the surface of the alloy material. As a mesh structure protective layer, the gas generated by the combustion cannot escape from the protective layer, causing the carbon layer to expand violently. The large volume carbon layer formed by the expansion has an excellent heat insulation effect, effectively blocking the thermal effect of external radiation on the material, reducing the heat of the alloy material, thereby achieving the dual effects of flame retardancy, smoke suppression and toxicity reduction, and expansion and smoke suppression. In addition, as the silicon element continues to migrate to the outer layer, the surface of the carbon layer becomes denser, thereby achieving a good flame retardant and smoke suppression effect. Polyborosiloxane is a polymer obtained by introducing boron into the Si-O skeleton of polysiloxane, and is a new type of high-density polysiloxane in element-modified polysiloxane. As one of the sub-materials, due to the presence of high bond energy such as Si-O bond and BO bond on the main chain of the molecule, it has better high temperature resistance and adhesion. During the combustion process of the alloy, the silicon element will gradually enrich on the surface of the alloy with the combustion, increase the quality of the carbon layer, prevent dripping, inhibit the transfer of heat and oxygen and the formation of flammable volatile products and their diffusion to the combustion zone, and prevent the alloy material from continuing to burn, thereby improving the flame retardancy of the PBT / PET alloy. Moreover, the addition of polyborosiloxane with flexible chain segments can further improve the impact strength of the alloy material and enhance the mechanical properties. Polytetrafluoroethylene has good fluidity and dispersibility. After mixing with the alloy material, it can show good handling performance and can form fibers to achieve an anti-drip effect. Moreover, it has stable chemical properties and good thermal stability. When used with phenyl silicone resin and polyborosiloxane, it can achieve better flame retardancy and reduce smoke emission.
[0012] Optionally, the polyborosiloxane is pretreated as follows:
[0013] Nickel sulfate and graphite powder are added to ethanol, ultrasonically dispersed for 20-30 minutes, dried and mixed with polyborosiloxane, and placed at 0.05-0.08 MPa for 10-12 hours. The mass ratio of polyborosiloxane, nickel sulfate and graphite powder is 1:0.1-0.3:0.05-0.2.
[0014] By adopting the above technical scheme, nickel sulfate can expand at a lower temperature to form a carbon layer, and can increase the density and continuity of the carbon layer, hinder the transfer of external heat, reduce the heat release of the material, reduce the release of combustible gas and smoke particles, and play a flame retardant effect. When the alloy material burns, the graphite powder can form a covering layer on the surface of the composite material as the matrix decomposes, and wrap on the carbon layer, and work together with nickel sulfate to further prevent the alloy material matrix from contacting with the air. On the other hand, it also alleviates the release of decomposition gas, improves flame retardancy, and reduces the smoke release rate and heat release.
[0015] Optionally, 0.5-1 parts by weight of a nucleating agent is also added to the flame retardant PBT and PET alloy material.
[0016] By adopting the above technical scheme, PBT and PET alloy materials are prone to produce sticky films during the injection molding process, which leads to tearing of the parts. Adding nucleating agents to the alloy materials can further refine the crystal structure, improve the crystallinity and increase the crystallization rate, so that the alloy materials can be easily solidified and demolded at high temperatures, shortening the processing cycle and improving the quality of parts.
[0017] Optionally, the preparation method of the nucleating agent is as follows:
[0018] The biomass and sodium silicate are mixed evenly at a mass ratio of 6-8:1, heated to 500-600°C, kept warm for 2-4 hours, washed with deionized water, and dried to obtain biochar;
[0019] The biochar is immersed in silica gel at 0.06-0.08 MPa for 8-10 hours, dried at 60-80° C. for 10-30 minutes, ground and sieved to obtain a nucleating agent.
[0020] By adopting the above technical scheme, biomass and sodium silicate are mixed and pyrolyzed. The main elements in biomass are carbon, followed by oxygen, hydrogen and nitrogen. The addition of sodium silicate increases the silicon content in biochar and reduces the carbon content. When preparing biochar, after being pyrolyzed, the carbon component undergoes intense pyrolysis, exposing the silicon located in the internal structure, so that the surface of the formed biochar is loaded with smooth crystalline silicon oxide particles, the specific surface area and porosity are increased, and the adsorption amount is improved, thereby reducing the amount of smoke released. Then the biochar is immersed in silica sol. The silica sol loaded in the biochar can absorb heat and shrink, play a physical barrier and structural support role, and block the transfer of heat, oxygen and gaseous products. The oxygen-containing functional groups on the silica sol are connected to the hydroxyl groups on the biochar through hydrogen bonds, and the oxygen-containing groups on the silica sol form hydrogen bonds with the polymer, thereby limiting the thermal vibration of the polymer, increasing the energy required for the decomposition of the polymer chain, and improving the thermal stability.
[0021] Optionally, the phosphate is at least one of ammonium polyphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, sodium phosphate, magnesium phosphate and antimony phosphate.
[0022] Optionally, the polymeric brominated flame retardant is selected from at least one of brominated epoxy resin, brominated polystyrene, decabromodiphenyl ether, hexabromocyclododecane, octabromoether and decabromodiphenyl ether.
[0023] Optionally, the toughening agent is a glycidyl acrylate grafted elastomer.
[0024] By adopting the above technical solution, the toughening agent can improve the compatibility between PET resin and PBT resin, improve impact strength and elongation, etc., and improve the toughness of the alloy material.
[0025] Optionally, the lubricant is selected from at least one of calcium stearate, magnesium stearate, pentaerythritol ester and ethylene bis stearamide.
[0026] In the second aspect, the present application provides a method for preparing a flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, using the following technical solution:
[0027] A method for preparing a flame-retardant PBT and PET alloy material with high GWIT and low smoke volume comprises the following steps:
[0028] The polymeric brominated flame retardant, antimony trioxide, a flame retardant synergist, an antioxidant and a lubricant are uniformly mixed to prepare a powder additive;
[0029] The PET resin, the PBT resin and the toughening agent are mixed evenly, the powder additive is added, the alkali-free glass fiber is added through side feeding, and the mixture is extruded and granulated after mixing.
[0030] By adopting the above technical solution, the alkali-free glass fiber is added into the extruder through side feeding and blended with other raw materials, which can prevent the alkali-free glass fiber from agglomerating in the blend and improve the surface quality of the alloy material.
[0031] Optionally, the PET resin and the PBT resin are pre-dried in vacuum at 100-120° C. for 2-3 hours.
[0032] In summary, this application has the following beneficial effects:
[0033] 1. Since the present application adopts PBT resin and PET resin as base materials, adds polymeric bromine flame retardant and antimony trioxide to improve the GWIT and flame retardant effect of the alloy material, adds phosphate and silicone flame retardant as flame retardant synergists, can further improve the flame retardant effect of the alloy material, and form an insulating protective layer to isolate the air, prevent the decomposition products generated by combustion from escaping, inhibit the thermal decomposition of the polymer material, and achieve the purpose of high flame retardancy, low smoke emission and low harmfulness.
[0034] 2. In the present application, phenyl silicone resin, polyborosiloxane and polytetrafluoroethylene are preferably used as silicone-based flame retardants. When the alloy material burns, phenyl silicone resin and polyborosiloxane can gradually form an insulating and dense silica layer, which prevents the internal combustible gas from escaping, thereby presenting an excellent dual effect of smoke suppression and toxicity reduction and expansion flame retardancy. Polytetrafluoroethylene can cooperate with phenyl silicone resin and polyborosiloxane to produce a coordinated effect of flame retardancy and smoke suppression. In addition, polyborosiloxane with flexible chain segments can further increase the impact strength of the alloy material and improve the mechanical properties.
[0035] 3. In the present application, nickel sulfate and graphite powder are preferably used to pretreat polyborosiloxane, which can form a covering layer on the dense layer of silica or the combined material while the dense layer of silica is formed on the polyborosiloxane, thereby further preventing the transfer of heat and the release of decomposition gas, improving flame retardancy and reducing smoke generation.
[0036] 4. In the present application, it is preferred to add a nucleating agent to the alloy material to improve the demoulding effect of the alloy material, so that the surface of the alloy product is smooth and of high quality. The nucleating agent is made of biochar modified by sodium silicate and then impregnated with silica sol, so that the surface of the biochar is loaded with more fine particles, the specific surface area is increased, the interface effect with the alloy material is enhanced, the adsorption force is increased, and the smoke emission can be reduced. In addition, the impregnated silica sol can absorb heat and shrink to form a barrier, thereby improving the shielding effect against heat and decomposition gases. DETAILED DESCRIPTION
[0037] The following examples further illustrate the present application in detail.
[0038] Preparation Examples 1-4 of Nucleating Agents
[0039] Preparation Example 1: 80 g of biomass and sodium silicate were mixed evenly in a mass ratio of 8:1, heated to 600° C. at a rate of 10° C. / min in a muffle furnace, kept warm for 2 h, ground, sieved through a 60-mesh sieve, washed with deionized water 4 times, and dried at 80° C. for 24 h to obtain biochar, where the biomass was rice straw;
[0040] The prepared biochar was immersed in a silica gel with a concentration of 35 wt %, immersed at 0.08 MPa for 8 h, dried at 80° C. for 10 min, ground, and passed through a 500-mesh sieve to obtain a nucleating agent. The silica sol was prepared by mixing 35 g of silica particles with deionized water.
[0041] Preparation Example 2: 60 g of biomass and sodium silicate were mixed evenly in a mass ratio of 8:1, heated to 500° C. at a rate of 10° C. / min in a muffle furnace, kept warm for 4 h, ground, sieved through a 60-mesh sieve, washed with deionized water 4 times, and dried at 80° C. for 24 h to obtain biochar, where the biomass was rice straw;
[0042] The prepared biochar was immersed in a silica gel with a concentration of 35 wt %, immersed at 0.06 MPa for 10 h, dried at 60° C. for 30 min, ground, and passed through a 500-mesh sieve to obtain a nucleating agent. The silica sol was prepared by mixing 35 g of silica particles with deionized water.
[0043] Preparation Example 3: 80 g of biomass and sodium silicate were evenly mixed in a mass ratio of 8:1, heated to 600°C at a rate of 10°C / min in a muffle furnace, kept warm for 2 hours, ground, sieved through a 60-mesh sieve, washed with deionized water 4 times, dried at 80°C for 24 hours, ground, sieved through a 500-mesh sieve, to obtain a nucleating agent, and the biomass was rice straw.
[0044] Preparation Example 4: The biomass is heated to 600°C at a rate of 10°C / min in a muffle furnace, kept warm for 2 hours, ground, sieved through a 60-mesh sieve, washed 4 times with deionized water, and dried at 80°C for 24 hours to obtain biochar, where the biomass is rice straw; the obtained biochar is immersed in a silica gel with a concentration of 35wt%, immersed at 0.08MPa for 8 hours, dried at 80°C for 10 minutes, ground, sieved through a 500-mesh sieve, and a nucleating agent is obtained. The silica sol is prepared by mixing 35g of silica particles with deionized water.
[0045] Preparation Example 5
[0046] Preparation Example 5 of polyborosiloxane: Octamethylcyclotetrasiloxane and boric acid are used for synthesis. The preparation method is as follows: 14.83 g of octamethylcyclotetrasiloxane, 1.04 g of tetraethyl silicate, 1 ml of hydrochloric acid, 0.733 g of boric acid and 40 ml of diethylene glycol dimethyl ether solvent are added into a round-bottom flask. Tetraethyl silicate serves as a branching center to promote the reaction between boric acid and polysiloxane. The mixture is reacted at 70°C for 4 h under magnetic stirring, and the temperature is raised to 120°C. The reaction is continued for 2 h. The solvent is removed by filtration and reduced pressure distillation to obtain polyborosiloxane.
[0047] Example
[0048] Example 1: A flame retardant PBT and PET alloy material with high GWIT and low smoke volume, the raw material dosage is shown in Table 1, wherein the intrinsic viscosity of the PET resin is 0.76 dl / g, selected from Songhan Plastics, the brand is CR-8839T, the intrinsic viscosity of the PBT resin is 1.0 dl / g, selected from Suzhou Damai Plastics Co., Ltd., the brand is 1100-211M, the length of the alkali-free glass fiber is 5 μm, the polymerized brominated flame retardant is brominated polystyrene, selected from Zhongshan Yuanda New Materials, the product number is 7010, and the antioxidant is a weight ratio of The ratio of antioxidant 1010 and antioxidant 168 is 1:0.5, the lubricant is ethylene bis stearamide, the toughening agent is acrylate glycidyl ester grafted elastomer, selected from Shanghai Xichen Industrial Co., Ltd., the item number is G60-65, the flame retardant synergist includes phosphate and silicone flame retardant in a mass ratio of 1:1, the phosphate is ammonium polyphosphate, the silicone flame retardant includes polyborosiloxane, phenyl silicone resin and polytetrafluoroethylene in a mass ratio of 1:1.5:0.3, the polyborosiloxane is prepared by Preparation Example 5, and the phenyl silicone resin is selected from Wacker, Germany, the model is 603, polytetrafluoroethylene is selected from Dongguan Maoke Plastic Raw Materials Co., Ltd., with the brand name L-5.
[0049] The method for preparing the flame-retardant PBT and PET alloy materials with high GWIT and low smoke volume comprises the following steps: uniformly mixing a polymeric brominated flame retardant, antimony trioxide, a flame retardant synergist, an antioxidant and a lubricant to obtain a powder additive;
[0050] PET resin and PBT resin are dried at 120℃ for 2h, then mixed with toughening agent, added with powder additive, added with alkali-free glass fiber through side feeding, extruded and granulated after mixing, the temperature of each zone of the extruder is: Zone 1: 180℃; Zone 2: 230℃; Zone 3: 230℃; Zone 4: 230℃; Zone 5: 230℃; Zone 6: 220℃; Zone 7: 240℃; Zone 8: 240℃; Zone 9: 240℃; Head: 245℃, the extruded material strips are cooled to room temperature through the water tank and granulated by the pelletizer. The length-to-diameter ratio of the twin-screw extruder is 40:1, and two vacuum sections are installed on the 5th and 7th sections of the equipment to realize double vacuum control, so as to improve and control the odor of the modified product and the volatilization of its harmful substances. After granulation, it is cooled in 40-degree water temperature and immediately separated from the water to prevent hydrolysis during the production process and affect the material properties.
[0051] Table 1
[0052]
[0053]
[0054] Example 2-5: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume. The difference from Example 1 is that the amounts of raw materials used are as shown in Table 1.
[0055] Example 6: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume. The difference from Example 1 is that the brominated flame retardant is brominated epoxy resin selected from Shanghai Shengduan Trading, with a brand name of NPEB-400.
[0056] Example 7: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume. The difference from Example 1 is that the flame retardant synergist includes phosphate and silicone flame retardant in a mass ratio of 0.5:1, the phosphate is ammonium polyphosphate, and the silicone flame retardant includes polyborosiloxane, phenyl silicone resin and polytetrafluoroethylene in a mass ratio of 1:1:0.1.
[0057] Example 8: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, which differs from Example 1 in that polytetrafluoroethylene is not added.
[0058] Example 9: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 1 in that the organosilicon flame retardants are all phenyl silicone resins.
[0059] Example 10: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 1 in that polyborosiloxane is used instead of phenyl silicone resin.
[0060] Example 11: A flame retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 1 in that the polyborosiloxane is pretreated as follows:
[0061] Nickel sulfate and graphite powder were added into ethanol, the mass of ethanol was 3 times of the total mass of nickel sulfate and graphite powder, ultrasonically dispersed for 30 minutes, dried and mixed with polyborosiloxane, and placed under 0.08 MPa for 10 hours. The mass ratio of polyborosiloxane, nickel sulfate and graphite powder was 1:0.3:0.2.
[0062] Example 12: A flame retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 1 in that the polyborosiloxane is pretreated as follows:
[0063] Nickel sulfate and graphite powder were added into ethanol, the mass of ethanol was 3 times of the total mass of nickel sulfate and graphite powder, ultrasonically dispersed for 20 minutes, dried and mixed with polyborosiloxane, and placed under 0.05 MPa for 12 hours. The mass ratio of polyborosiloxane, nickel sulfate and graphite powder was 1:0.1:0.05.
[0064] Example 13: A flame retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 1 in that the polyborosiloxane is pretreated as follows:
[0065] Nickel sulfate was added into ethanol, the mass of ethanol being 3 times of the mass of nickel sulfate, and ultrasonically dispersed for 20 minutes. After drying, the mixture was mixed with polyborosiloxane and placed under 0.05 MPa for 12 hours. The mass ratio of polyborosiloxane to nickel sulfate was 1:0.1.
[0066] Example 14: A flame retardant PBT and PET alloy material with high GWIT and low smoke yield, which is different from Example 1 in that the polyborosiloxane is pretreated as follows:
[0067] Graphite powder was added into ethanol, the mass of ethanol being 3 times of the mass of graphite powder, and ultrasonically dispersed for 20 minutes. After drying, the mixture was mixed with polyborosiloxane and placed under 0.05 MPa for 12 hours. The mass ratio of polyborosiloxane to graphite powder was 1:0.05.
[0068] Example 15: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume. The difference from Example 11 is that the PET resin and the PBT resin are dried at 120°C for 2 hours and then mixed evenly with 1 kg of nucleating agent and toughening agent. The nucleating agent is prepared by Preparation Example 1, and the other parameters are the same as those of Example 10.
[0069] Example 16: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume. The difference from Example 11 is that the PET resin and the PBT resin are dried at 120°C for 2 hours and then mixed evenly with 0.5 kg of nucleating agent and toughening agent. The nucleating agent is prepared by Preparation Example 2. The other parameters are the same as those of Example 10.
[0070] Example 17: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 15 in that the nucleating agent is made from Preparation Example 3.
[0071] Example 18: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 15 in that the nucleating agent is made from Preparation Example 4.
[0072] Comparative Example
[0073] Comparative Example 1-4: A flame-retardant PBT and PET alloy material with high GWIT and low smoke volume, which is different from Example 1 in that the amount of raw materials used is as shown in Table 2.
[0074] Table 2
[0075]
[0076]
[0077] Embodiment 5: A flame retardant PBT and PET alloy material with high GWIT, comprising the following components by weight percentage: 40.5% PBT resin, 20% PET resin, 8% brominated epoxy resin, 0.5% antimony trioxide, 3% calcium hydroxide, and 25% alkali-free glass fiber, wherein the PBT resin is selected from Changchun Chemical Industry of Taiwan, China, with the brand name PBT1200211M, the PET resin is selected from Yizheng Chemical Fiber of Sinopec, with the brand name PET FG600, the particle size of calcium hydroxide is 5 μm, and the brominated epoxy resin is selected from Israel Chemical Group, with the brand name: Powder-F-2100; The preparation method of the flame retardant PBT and PET alloy material with high GWIT is as follows: 1) Dry the PBT at 135° C. for 4 hours and set aside;
[0078] 2) PBT resin, PET resin, brominated flame retardant, antimony trioxide and calcium hydroxide are mixed evenly and added into a twin-screw extruder. Alkali-free glass fiber is fed from the side of the extruder. The mixture is plasticized, mixed and extruded at 240° C. and cooled and granulated to obtain flame-retardant PBT and PET alloy materials with high GWIT.
[0079] Performance testing
[0080] PBT and PET alloy materials were prepared according to the methods in the examples and comparative examples, and performance tests were performed according to the following methods. The test results are recorded in Table 3.
[0081] 1. GWIT: Tested in accordance with IEC 60695-2-12-2014 "Glow Wire Flammability Test".
[0082] 2. UL-94: When the thickness of the sample is 1.6 mm, the flame retardancy is tested in accordance with UL-94.
[0083] 3. Impact strength: Tested in accordance with GB / T1843-2008 "Determination of impact strength of plastic cantilever beam".
[0084] 4. TSP (smoke release): Tested in accordance with ISO 5660-1 "Combustion heat release rate".
[0085] 5. Demolding effect: Demolding performance is divided into the following four levels according to the time required for complete demolding: (1) Poor - sticking to the mold; (2) Medium - manual assisted demolding; (3) Good - basically able to demold automatically, occasionally requiring manual assistance; (4) Excellent - completely automatic demolding.
[0086] Table 3
[0087]
[0088]
[0089] It can be seen from the data in Table 3 that in Examples 1-5, different raw material amounts are used, brominated epoxy resin is used as a brominated flame retardant, and it is used in combination with antimony trioxide, and a synergistic flame retardant composed of phosphate and silicone resin is added. The PBT and PET alloy materials prepared in this way have high GWIT, good flame retardancy, low smoke emission, good mechanical properties, and are alloy materials that meet environmental protection requirements.
[0090] Example 6 uses brominated epoxy resin as a polymeric brominated flame retardant. Compared with Example 1, the PBT and PET alloy materials prepared in Preparation Example 6 have low smoke emission, good flame retardancy, high impact strength, and similar properties to Example 1.
[0091] In Example 7, different ratios of phosphate and silicone flame retardant are used, and the usage ratio of polyborosiloxane, phenyl silicone resin and polytetrafluoroethylene in the silicone flame retardant is different from that in Example 1. Table 3 shows that the PBT and PET alloy materials prepared in Example 7 have flame retardancy, mechanical properties and low smoke volume similar to those in Example 1.
[0092] In Example 8, polytetrafluoroethylene was not added to the organosilicon flame retardant, and the organosilicon flame retardant was phenyl silicone resin and polyborosiloxane. In Example 9, the organosilicon flame retardant was only phenyl silicone resin, and polytetrafluoroethylene and polyborosiloxane were not added. Table 3 shows that the impact strength of the PBT and PET alloy materials prepared in Example 9 decreased, the flame retardant effect weakened, and the smoke emission increased. In Example 8, the smoke emission of the PBT and PET alloy materials increased, and the GWIT was also reduced.
[0093] In Example 10, the organosilicon flame retardants are polyborosiloxane and polytetrafluoroethylene. Compared with Example 1, the flame retardant properties of the PBT and PET alloy materials prepared in Example 10 are reduced, the heat resistance is weakened, and the smoke generation is increased.
[0094] Compared with Example 1, Example 11 and Example 12 also use nickel sulfate and graphite powder to pretreat the polyborosiloxane. The impact strength of the PBT and PET alloy materials prepared in this way is increased, and the smoke emission is further reduced. It can be seen that pretreating the polyborosiloxane can further increase the mechanical strength and environmental protection of the alloy material.
[0095] When pretreating polyborosiloxane in Example 13 and Example 14, graphite powder and nickel sulfate were not added, respectively. Table 3 shows that compared with Example 11 and Example 12, the impact strength of the PBT and PET alloy materials prepared in Example 13 and Example 14 decreased, and the smoke generation increased.
[0096] Compared with Example 11, Example 15 and Example 16 further added a nucleating agent, and the nucleating agent was prepared from Preparation Example 1 and Preparation Example 2, respectively. Table 3 shows that the smoke emission of the PBT and PET alloy materials prepared in Example 15 and Example 16 is further reduced, and the impact resistance is enhanced, and the demolding effect is improved.
[0097] Compared with Example 15, Example 17 and Example 18 use the nucleating agents prepared in Preparation Example 3 and Preparation Example 4, respectively. In Preparation Example 3, only sodium silicate is mixed with biomass for sintering without impregnation with silica gel. In Preparation Example 4, only the biochar prepared by calcining biomass is impregnated in silica gel. The smoke emission of the PBT and PET alloy materials prepared in Example 17 and Example 18 increases, and the impact strength decreases.
[0098] Compared with Example 1, the amount of raw materials in Comparative Examples 1-4 is changed, no flame retardant synergist is added in Comparative Example 1, the amount of polymeric brominated flame retardant in Comparative Example 2 is reduced, the amount of antimony trioxide in Comparative Example 3 is increased, and the amounts of PET and PBT are changed, and the amount of flame retardant synergist in Comparative Example 4 is reduced. It can be seen from the data in Table 3 that although the PBT and PET alloy materials prepared in Comparative Example 1 have good flame retardant effects, the GWIT is reduced and the smoke emission is large. The GWIT of Comparative Example 2 is reduced and the flame retardant effect is poor. The impact strength of Comparative Example 3 is reduced and the GWIT is deteriorated. In Comparative Example 4, the GWIT is reduced and the smoke emission is increased, indicating that changing the amount of raw materials will affect the comprehensive performance of PBT and PET alloy materials.
[0099] Comparative Example 5 is a PBT and PET alloy material containing antimony trioxide and brominated epoxy resin in the prior art. Although it has high GWIT and flame retardant effects, it has a large amount of smoke, is not environmentally friendly, and has poor demoulding effect.
[0100] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A flame retardant PBT and PET alloy material with high GWIT and low smoke volume, characterized in that: The invention comprises the following raw materials in parts by weight: 20-45 parts of PBT resin, 5-15 parts of PET resin, 2-4.8 parts of toughening agent, 30-35 parts of alkali-free glass fiber, 9-11 parts of polymeric brominated flame retardant, 0.5-2 parts of antimony trioxide, 9-10 parts of flame retardant synergist, 0.1-0.3 parts of antioxidant, and 0.2-0.6 parts of lubricant, wherein the flame retardant synergist comprises phosphate and silicone flame retardant in a mass ratio of 0.5-1:1; The organosilicon flame retardant comprises polyborosiloxane, phenyl silicone resin and polytetrafluoroethylene in a mass ratio of 1:1-1.5:0.1-0.
3.
2. The flame retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 1, characterized in that: The polyborosiloxane is pretreated as follows: Nickel sulfate and graphite powder are added to ethanol, ultrasonically dispersed for 20-30 minutes, dried and mixed with polyborosiloxane, and placed at 0.05-0.08 MPa for 10-12 hours. The mass ratio of polyborosiloxane, nickel sulfate and graphite powder is 1:0.1-0.3:0.05-0.
2.
3. The flame retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 1, characterized in that: 0.5-1 weight portion of nucleating agent is also added to the flame retardant PBT and PET alloy material.
4. The flame retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 3, characterized in that: The preparation method of the nucleating agent is as follows: The biomass and sodium silicate are mixed evenly at a mass ratio of 6-8:1, heated to 500-600°C, kept warm for 2-4 hours, washed with deionized water, and dried to obtain biochar; The biochar is immersed in silica gel at 0.06-0.08 MPa for 8-10 hours, dried at 60-80° C. for 10-30 minutes, ground and sieved to obtain a nucleating agent.
5. The flame retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 1, characterized in that: The phosphate is at least one of ammonium polyphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, sodium phosphate, magnesium phosphate and antimony phosphate.
6. The flame retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 1, characterized in that: The polymeric brominated flame retardant is selected from at least one of brominated epoxy resin, brominated polystyrene, decabromodiphenyl ether, hexabromocyclododecane, octabromoether and decabromodiphenyl ether.
7. The flame retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 1, characterized in that: The toughening agent is a glycidyl acrylate grafted elastomer.
8. The method for preparing the flame-retardant PBT and PET alloy material with high GWIT and low smoke yield according to any one of claims 1 to 7, characterized in that: The following steps are involved: The polymeric brominated flame retardant, antimony trioxide, a flame retardant synergist, an antioxidant and a lubricant are uniformly mixed to prepare a powder additive; The PET resin, the PBT resin and the toughening agent are mixed evenly, the powder additive is added, the alkali-free glass fiber is added through side feeding, and the mixture is extruded and granulated after mixing.
9. The method for preparing the flame-retardant PBT and PET alloy material with high GWIT and low smoke yield according to claim 8, characterized in that: The PET resin and the PBT resin are vacuum dried at 100-120° C. for 2-3 hours in advance.