Methods for recycling valuable metals from waste batteries

By combining mechanical activation and piezoelectric effects in used batteries, the problems of high energy consumption and serious pollution in the recycling of used batteries in the existing technology are solved, efficient and environmentally friendly recycling of valuable metals is achieved, the process flow is simplified and the process is improved. The metal recovery rate.

CN118207419BActive Publication Date: 2024-10-22SHENZHEN AUTOMOTIVE RES INST BEIJING INST OF TECH (SHENZHEN RES INST OF NAT ENG LAB FOR ELECTRIC VEHICLES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410315072.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-10-22
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

Existing methods for recycling valuable metals from used batteries have problems such as high energy consumption, serious pollution, low metal recovery rate, complex processes, and non-environmental protection, especially the high energy consumption caused by the fire process and the use of acids and bases in the wet process. resulting in water and soil pollution.

Method used

Using a method that combines mechanical activation and piezoelectric effect in physics, piezoelectric material is added to used battery black powder and mechanical stress and ultrasonic treatment are applied to form a piezoelectric effect and reduce the reducing agent and acid used in the chemical reaction. Efficient leaching of valuable metals. This method includes pre-soaking treatment and ultrasonic treatment in the water immersion stage, and utilizes the conversion of mechanical energy-electrical energy-chemical energy to preferentially extract lithium and reduce the loss of metallic lithium.

Benefits of technology

It realizes the clean, efficient and low-energy recovery of valuable metals from used batteries, improves the metal recovery rate, simplifies the process, reduces the risk of environmental pollution, and is suitable for the recycling of many types of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118207419B_ABST
    Figure CN118207419B_ABST
Patent Text Reader

Abstract

The present application discloses a method for recovering valuable metals from waste batteries, comprising: adding piezoelectric material to waste battery black powder and mixing evenly to obtain a mixture; adding water and a promoter to the mixture to obtain a pre-impregnation system, and applying mechanical stress treatment to the pre-impregnation system; adding water to the pre-impregnation system after mechanical stress treatment to obtain a water immersion system, and applying ultrasound to the water immersion system; solid-liquid separation to obtain a leachate and a leachate residue, wherein the leachate is a lithium-containing solution. According to the present application, a simple, clean, efficient, high-comprehensive recovery value and low-energy consumption recycling method for waste battery electrodes can be provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of waste battery recycling and resource utilization, and in particular to a method for recycling valuable metals in waste batteries. Background Art

[0002] With the rapid development of the new energy industry, the demand for batteries has also shown a sharp growth trend, but the battery life is limited. For example, the service life of lithium batteries is usually about 5 to 8 years, which is accompanied by the generation of a large number of waste batteries. If these waste batteries cannot be recycled in time, they will not only pose a safety hazard, but also easily cause environmental pollution. In addition, batteries contain a large number of valuable metal elements, such as lithium, nickel, cobalt, manganese, etc. If they are not recycled in time, a large amount of valuable metal resources will be wasted, which is not conducive to sustainable development.

[0003] At present, the recycling methods of metal elements in waste batteries are mainly pyrometallurgical processes and hydrometallurgical processes. The pyrometallurgical process is to put the electrode material into an electric arc furnace and process it at a high temperature of more than 1000℃. The plastic and organic solvents in it are burned, and the metal and its compounds undergo redox reactions. Different metals have different melting points and condensation points. They are collected through the process of metal vapor volatilization, cooling and condensation. Low-boiling-point nickel, cobalt and manganese metals are mainly recovered. Finally, the remaining residual metals are screened, pyrolyzed, magnetically separated or chemically separated to recover lithium, aluminum, iron and other metals. Although the pyrometallurgical process is simple and mature, the process flow is short, the operation is relatively simple, and there is no need for sorting in advance. It can recycle a mixture of multiple types of batteries. However, its recycling process consumes a lot of energy, produces more CO2 or other harmful gases, and the pressure of incineration tail gas treatment is high, which is easy to cause air pollution; some metal lithium and other metals are difficult to recover in the slag, and the metal recovery rate is low. The product alloy needs to be further processed with hydrometallurgical processes to achieve the purification of different metals. The hydrometallurgical process is to dissolve the electrode materials of waste lithium batteries through acid or alkali, leach the metal components in the electrode active substances, and after the leachate is purified by impurities, separate the metal ions and form corresponding inorganic salts or oxides, such as cobalt sulfate, nickel sulfate, cobalt chloride, lithium carbonate, etc., through ion exchange, extraction or precipitation, which can be directly used in the production and recycling of batteries. Conventional hydrometallurgical processes can recover almost all high-value metal elements in batteries, but the disadvantages are that there are many metal ion components in the solution, the operation procedures are complicated, and the process flow is long; the process uses a large amount of acid and alkali, and the wastewater treatment is difficult, which is easy to cause water and soil pollution, and improper treatment is easy to cause secondary pollution; it is suitable for waste batteries with relatively single components. When the components change significantly, the process needs to be adjusted.

[0004] In summary, there is an urgent need to provide a cleaner, more efficient and less energy-consuming method for recycling used batteries. Summary of the invention

[0005] The purpose of this application is to provide a method for recovering valuable metals from waste batteries.

[0006] This application adopts the following technical solutions:

[0007] One aspect of the present application discloses a method for recovering valuable metals from waste batteries, comprising: adding piezoelectric material to black powder of waste batteries and mixing them evenly to obtain a mixture; adding water and a promoter to the mixture to obtain a prepreg system, and applying mechanical stress treatment to the prepreg system; adding water to the prepreg system after the mechanical stress treatment to obtain a water immersion system, and applying ultrasound to the water immersion system; solid-liquid separation to obtain a leachate and a leach residue, wherein the leachate is a lithium-containing solution.

[0008] It should be noted that the method for recovering valuable metals from waste batteries of the present application combines mechanical activation with piezoelectric effect in physics and applies it to the process of chemical reaction, using piezoelectric materials to generate higher piezoelectric potential under mechanical stress to form piezoelectric effect, through the mutual conversion of energy between mechanical energy, electrical energy and chemical energy and charge separation, generating active oxygen (ROS) and free radicals with extremely strong redox properties in the reaction system to reduce and replace various reducing agents and acids used in chemical reactions, thereby achieving leaching of valuable metals. On the other hand, the process of applying mechanical stress can also activate the materials in the system, improving the leaching effect for the subsequent leaching stage. In the present application, piezoelectric activation pretreatment is performed through the pre-leaching process, which can also activate the materials (refine the particle size of the materials, destroy the crystal structure, increase the activity of the materials, reduce the reaction activation energy, reduce the temperature required for the reaction, improve the uniformity of the particle distribution of the materials and promote the diffusion of solid ions), and enhance the leaching efficiency.

[0009] It should also be noted that in the present application, by fully mixing the battery black powder and the piezoelectric material in advance, the piezoelectric material can contact and react with the nearest material more quickly when the charge is separated by mechanical stress. If the battery black powder and the piezoelectric material are not fully mixed in advance, it may cause a local reaction at the beginning, while some materials cannot react because they do not contact the piezoelectric material. When the piezoelectric material moves in the system and starts to contact, the particle size of the piezoelectric material will change after the mechanical force acts. The particle size affects the charge separation and reaction, thereby reducing the reaction efficiency and requiring a longer reaction time.

[0010] It should also be noted that in this application, applying ultrasonic treatment during the water immersion stage can generate mechanical stress and then form a piezoelectric effect, promote the leaching of metal ions, and also generate a cavitation effect, making the materials in the water immersion system more dispersed, avoiding the influence of physical agglomeration / agglomeration on the leaching efficiency, thereby significantly improving the leaching effect. The piezoelectric multi-field synergistic treatment of the mechanical stress field and the ultrasonic field can help further improve the leaching efficiency.

[0011] It should also be noted that in this application, a selective priority lithium extraction method is adopted, with piezoelectric materials as the medium. The lithium extraction process realizes the priority leaching of lithium through the conversion between mechanical energy-electrical energy-chemical energy and the redox reaction of lithium. Compared with the existing sulfation roasting and reduction roasting priority lithium extraction processes, the shortcomings of high energy consumption and loss of metallic lithium in the pyrometallurgical process are avoided; compared with the conventional wet priority lithium extraction process, the use of reducing agents and acid-base reagents is reduced, which is conducive to alleviating the pressure of wastewater treatment at the back end. In addition, compared with the one-step leaching and rear-end separation and extraction of lithium, the selective priority lithium extraction can reduce the loss of metallic lithium during the rear-end separation and improve the recovery rate of lithium.

[0012] In one implementation of the present application, the battery black powder is obtained by disassembling, crushing and sorting the waste battery after it is fully discharged. It should be noted that the battery black powder mainly comes from the positive and negative electrode materials inside the battery, and the positive and negative electrodes are coated with active materials, such as lithium cobalt oxide (LiCoO2), lithium iron phosphate (LiFePO4), ternary materials (nickel cobalt manganese oxide NCM or nickel cobalt aluminum oxide NCA, etc.). The battery black powder contains metal elements with high recycling value, such as lithium, cobalt, nickel, manganese, etc. When recycling the battery, the process of obtaining the battery black powder mainly includes the following steps: fully discharge the waste battery to improve safety; disassemble and crush, remove the outer shell and other non-electrode parts, and then put the part containing the positive and negative electrode materials into a crusher for crushing to separate the internal electrode sheet; sort, the crushed material is separated by a vibrating screen or airflow sorting method to preliminarily separate the metal shell, aluminum foil, copper foil and battery black powder containing active substances.

[0013] In one implementation of the present application, the battery black powder contains LiFePO4, LiCoO2, LiNiO2, LiMn2O4, LiNi x Co y Mn 1-x-y O2、LiNi x Co y Al 1-x-y At least one component of O2.

[0014] In one implementation of the present application, the piezoelectric material is selected from at least one of inorganic piezoelectric crystals, inorganic piezoelectric ceramics and organic piezoelectric materials. It should be noted that the larger the piezoelectric coefficient of the selected piezoelectric material, the better the effect of leaching metal ions.

[0015] In one implementation of the present application, the inorganic piezoelectric crystal includes but is not limited to quartz crystal, tourmaline, barium titanate and its derivative structure crystals, and ferroelectric crystals.

[0016] In one implementation of the present application, the inorganic piezoelectric ceramics include but are not limited to lead zirconate titanate ceramics, barium titanate ceramics, aluminum nitride ceramics, and zinc oxide ceramics.

[0017] In one implementation of the present application, the organic piezoelectric material includes but is not limited to polyvinylidene fluoride and its copolymers, and nylon.

[0018] In one implementation of the present application, the piezoelectric material is quartz crystal or tourmaline. It should be noted that in this case, a piezoelectric material that is easy to obtain, inexpensive, and has a large piezoelectric coefficient can be used. Quartz is cheap and easy to obtain, such as ordinary quartz sand or glass; tourmaline has a better effect, a high piezoelectric coefficient, is easier to generate piezoelectric potential, has a higher leaching efficiency, and can be used in a smaller amount.

[0019] In one implementation of the present application, in the prepreg system, the content of the piezoelectric material is 0.2-10 g / L. It should be noted that, in this case, the leaching efficiency of metal ions can be improved.

[0020] In one implementation of the present application, in the prepreg system, the content of the piezoelectric material is 0.2 to 5 g / L.

[0021] In one implementation of the present application, the promoter is selected from any one or more of hydrogen peroxide, ethanol, sodium sulfite, sodium bisulfite, glucose and ascorbic acid, etc. It should be noted that, in this case, the promoter can provide a starter or seed for the reaction (similar to the seed crystal added during the crystallization process), which can promote the leaching of metal ions. In addition, hydrogen peroxide can oxidize certain organic or inorganic substances that may be combined with lithium, converting them into easily soluble forms, thereby promoting the release of lithium ions from black powder; sulfite compounds such as sodium sulfite and sodium bisulfite can act as reducing agents under certain conditions, participate in chemical reactions, and reduce the oxidation state of certain metal oxides or other compounds, making lithium easier to leach; glucose and other polyhydroxy compounds can form soluble complexes with lithium ions through coordination, thereby helping lithium ions to transfer from solid black powder to solution; ascorbic acid also has strong reducing and complexing abilities, can form stable chelates with metal ions, and due to its antioxidant properties, can protect lithium from oxidation to a certain extent, which is beneficial to the leaching process; ethanol, as a polar solvent, can change the properties of the solid-liquid interface, allowing the solvent to better contact and dissolve lithium-containing materials.

[0022] In one implementation of the present application, the mass ratio of the battery black powder to the accelerator is 1:0.02 to 1:0.5. It should be noted that in this case, the leaching efficiency of metal ions can be improved.

[0023] In one implementation of the present application, the method of generating the mechanical stress is selected from any one or more of ball milling, vibration, ultrasound, pressurization, stirring, friction, aeration, etc.

[0024] In one implementation of the present application, the mechanical stress is generated by ball milling, and the rotation speed of the ball milling is 350-500 rpm. It should be noted that in this case, a larger mechanical stress can be provided to promote the leaching of metal ions.

[0025] In one implementation of the present application, the solid-liquid ratio in the prepreg system is 500-2000 g / L. It should be noted that in this case, it is beneficial to make the mechanical force field contact the material better and form mechanical stress, and it can also make the piezoelectric material and the battery black powder contact better. If the ball milling is used, the solid-liquid ratio is small, the water volume is large, and the ball milling effect will be worse. If the solid-liquid ratio is too high and the water volume is small, it is also not conducive to the activation of the material and the efficiency becomes low.

[0026] In one implementation of the present application, the mechanical stress treatment time is 10 to 60 minutes.

[0027] In one implementation of the present application, the solid-liquid ratio in the water leaching system is 100-500 g / L. It should be noted that in this case, it is beneficial to make the metal ions leached better, while if the solid-liquid ratio is too high, the concentration of metal ions in the solution is high, which is not conducive to leaching.

[0028] In one implementation of the present application, the water immersion temperature is 25-95°C.

[0029] In one implementation of the present application, the water immersion temperature is 50-70°C.

[0030] In one implementation of the present application, the immersion time is 20 to 120 minutes.

[0031] In one implementation of the present application, in the water immersion system, the frequency of ultrasound is 20 to 180 kHz.

[0032] In one implementation of the present application, the leaching residue is also added to the leaching agent, and ultrasonic treatment is applied to obtain a cobalt-containing solution. It should be noted that in the cobalt extraction stage, the metal ions are leached through the piezoelectric catalytic effect, which can reduce the use of acid reagents. It should also be noted that the ultrasonic treatment applied in the cobalt extraction stage can, firstly, generate mechanical stress and then form a piezoelectric effect to promote the leaching of metal ions, and secondly, it can also produce a cavitation effect, so that the materials in the water leaching system are more dispersed, avoiding the influence of physical agglomeration / agglomeration on the ion leaching efficiency, thereby significantly improving the leaching effect. The piezoelectric multi-field synergistic treatment of the mechanical stress field and the ultrasonic field can help to further improve the leaching efficiency.

[0033] It should also be noted that for lithium cobalt oxide battery black powder, ternary lithium battery black powder, etc., after lithium extraction, the leaching residue can be used to leach and recover cobalt, nickel, manganese and other ions. When recovering valuable elements from single lithium iron phosphate black powder, there is no need to perform secondary leaching on the leaching residue to recover other metal ions. Lithium can be selectively leached after water leaching to achieve separation of lithium and iron phosphate and other impurities.

[0034] In one implementation of the present application, the leaching agent is selected from any one or more aqueous solutions of sodium citrate, citric acid, disodium ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid, tartaric acid, glycine and acetic acid. It should be noted that in this case, compared with inorganic strong acids such as sulfuric acid and hydrochloric acid, the selectivity is better, and a stable coordination compound or complex can be formed with the target metal ion, thereby improving the extraction efficiency of the target metal ion in a complex system and reducing the interference of other elements; in addition, it is more environmentally friendly, safer, and the reaction conditions are milder. When sodium citrate and / or disodium ethylenediaminetetraacetic acid solution are selected as leaching agents, the entire recovery process can be performed without the use of any acid reagent.

[0035] In one implementation of the present application, the concentration of the leaching agent may be 0.1 to 3 mol / L.

[0036] In one implementation of the present application, the solid-liquid ratio of the leaching residue to the leaching agent is 50 to 500 g / L. It should be noted that, in this case, the leaching of the target metal ions can be promoted.

[0037] In one implementation of the present application, the frequency of ultrasound is 20 to 180 kHz.

[0038] The beneficial effects of this application are:

[0039] The invention can provide a clean, efficient, high comprehensive recycling value and low energy consumption recycling method for waste battery electrodes. The method has a simple operation process and is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the recycling process of waste lithium batteries involved in this application. DETAILED DESCRIPTION

[0041] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. In the following embodiments, many detailed descriptions are intended to enable the present application to be better understood. However, those skilled in the art can easily recognize that some of the features can be omitted in different situations, or can be replaced by other materials and methods. In some cases, some operations related to the present application are not shown or described in the specification, in order to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and the related operations can be fully understood according to the description in the specification and the general technical knowledge in the art.

[0042] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations. At the same time, the steps or actions in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence, unless otherwise specified that a certain sequence must be followed.

[0043] The existing methods for recovering metal elements in waste lithium batteries are mainly pyrometallurgical processes and hydrometallurgical processes. However, the recovery process of the hydrometallurgical process consumes a lot of energy, produces a lot of CO2 or other harmful gases, and has high pressure on the treatment of incineration tail gas, which is easy to cause air pollution and is subject to policy restrictions; some metal lithium and the like are difficult to recover in the slag, and the metal recovery rate is low. The product alloy needs to be further processed with processes such as hydrometallurgy to achieve the purification of different metals; in the hydrometallurgical process, there are many metal ion components in the solution, the operation procedure is complicated, and the process flow is long; the process uses a large amount of acid and alkali, and the wastewater treatment is difficult, which is easy to cause water and soil pollution, and improper treatment is easy to cause secondary pollution; it is suitable for waste batteries with relatively single composition, and the process needs to be adjusted when the composition changes significantly.

[0044] In view of this, the present application creatively adopts piezoelectric activation to recycle valuable metals from waste batteries, which has the following advantages: cleaner, more efficient, high comprehensive recovery value and low energy consumption. The method has a simple operation process, mild production conditions, low equipment requirements, safe and reliable process, clean and environmentally friendly, avoiding the high energy consumption and loss of metallic lithium caused by the use of pyrometallurgical process, and also reducing the use of a large amount of reducing agents and acids and alkalis relative to the traditional wet process, effectively reducing the pressure of wastewater disposal at the back end of the environment, and expanding the technical support for the application scope of technology in the field of battery recycling.

[0045] Hereinafter, the method for recycling valuable metals from waste batteries of the present application will be described in detail with reference to the accompanying drawings and specific implementation methods.

[0046] Figure 1: is a schematic diagram of the recycling process of waste lithium batteries involved in this application. Figure 1 As shown, the method for recovering valuable metals from waste batteries of the present application can first provide waste lithium batteries, and then discharge, disassemble and sort them to obtain battery black powder. Subsequently, piezoelectric materials and promoters are added to the battery black powder, and mechanical stress is applied for piezoelectric activation. Subsequently, water leaching is performed to preferentially leach lithium ions. For the leached residue, an aqueous solution of an organic solvent (such as an aqueous solution of an organic acid or an organic acid salt) is added for two-stage leaching to obtain a solution containing nickel, cobalt and manganese, and then subsequent separation and purification are performed.

[0047] The present application is further described in detail below by specific examples. The following examples are only further described for the present application and should not be construed as limiting the present application. In the following examples, unless otherwise specified, the reagents and instruments used are all commercially available, and the experimental operations are all carried out in accordance with the product instructions and conventional experimental specifications.

[0048] Experiment 1: After fully discharging, disassembling, crushing and sorting the waste lithium iron phosphate battery, the waste lithium iron phosphate battery black powder was obtained. Add 2g of quartz sand to 1000g of lithium iron phosphate battery black powder and mix thoroughly and transfer to a ball mill. Add 1L of water to the ball mill, add hydrogen peroxide at a mass ratio of 1:0.2 between lithium iron phosphate battery black powder and hydrogen peroxide, and perform ball milling at a speed of 450rpm for 30min. The milled slurry was transferred to a water immersion reactor, and water was added to a solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 50℃, the water immersion time was 60min, and ultrasonic enhanced leaching was simultaneously turned on at a frequency of 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained.

[0049] Experiment 2: After fully discharging, disassembling, crushing and sorting the waste lithium iron phosphate battery, the waste lithium iron phosphate battery black powder was obtained. 1200g of lithium iron phosphate battery black powder was placed in a ball mill and 1L of water was added to the ball mill. Hydrogen peroxide was added at a mass ratio of 1:0.5 between lithium iron phosphate battery black powder and hydrogen peroxide, and ball milling was performed at a speed of 450rpm for 60min. The ball-milled slurry was put into a water immersion reactor, and water was added to a solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 70℃, the water immersion time was 90min, and ultrasonic enhanced leaching was started simultaneously, with an ultrasonic frequency of 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained.

[0050] Experiment 3: After fully discharging, disassembling, crushing and sorting the waste cobalt-acid lithium battery, the waste cobalt-acid lithium battery black powder was obtained. 0.5g of tourmaline was added to 1000g of cobalt-acid lithium battery black powder and mixed thoroughly and then transferred to a ball mill. 1L of water was added to the ball mill, and sodium sulfite was added according to the mass ratio of cobalt-acid lithium battery black powder and sodium sulfite of 1:0.08, and ball milling was performed at a speed of 450rpm for 40min. The slurry after ball milling was put into a water immersion reactor, and water was added to a solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 70℃, the water immersion time was 60min, and ultrasonic enhanced leaching was started simultaneously, with an ultrasonic frequency of 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained. The water leaching residue was added to 3.5L of 0.2mol / L citric acid aqueous solution at 50℃, ultrasonically leached for 120min, and the cobalt-containing solution and leaching residue were obtained after filtration.

[0051] Experiment 4: After fully discharging, disassembling, crushing and sorting the waste lithium cobalt oxide battery, the waste lithium cobalt oxide battery black powder was obtained. 2g of tourmaline particle powder was added to 800g of lithium cobalt oxide battery black powder and fully mixed and then transferred to the tank of the reciprocating vibration device. 1L of water was added to the tank, and ethanol was added according to the mass ratio of lithium cobalt oxide battery black powder and ethanol of 1:0.1, and reciprocating vibration was treated for 90min. The slurry after reciprocating vibration was put into the water immersion reactor, and water was added to the solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 70℃, the water immersion time was 60min, and ultrasonic enhanced leaching was started simultaneously, and the ultrasonic frequency was 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained. The water leaching residue was added to 3.5L of 0.2mol / L citric acid aqueous solution at 70℃, ultrasonic leached for 120min, and the ultrasonic frequency was 150kHz. After filtration, a cobalt-containing solution and leaching residue were obtained.

[0052] Experiment 5: After fully discharging, disassembling, crushing and sorting the waste ternary lithium battery, the waste ternary lithium battery black powder was obtained. 4g of quartz sand was added to 1000g of ternary lithium battery black powder and fully mixed and then transferred to a ball mill. 1L of water was added to the tank, and hydrogen peroxide was added according to the mass ratio of ternary lithium battery black powder and hydrogen peroxide of 1:0.2, and ball milling was performed at a speed of 450rpm and a processing time of 30min. The slurry after ball milling was put into a water immersion reactor, and water was added to a solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 70℃, the water immersion time was 60min, and ultrasonic enhanced leaching was started simultaneously, and the ultrasonic frequency was 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained. The water leaching residue was added to 3.5L of 0.2mol / L citric acid aqueous solution at 70℃, ultrasonic leaching was performed for 90min, and the ultrasonic frequency was 150kHz. After filtration, a cobalt-nickel-manganese-containing solution and leaching residue were obtained.

[0053] Experiment 6: After fully discharging, disassembling, crushing and sorting the waste ternary lithium battery, the waste ternary lithium battery black powder was obtained. 4g of tourmaline particle powder was added to 1000g of ternary lithium battery black powder and fully mixed and then transferred to the reactor. 1L of water was added to the reactor, and hydrogen peroxide was added according to the mass ratio of ternary lithium battery black powder and hydrogen peroxide of 1:0.2, and air was introduced for aeration for 60min. Water was added to the post-reaction slurry to a solid-liquid ratio of 250g / L, the immersion temperature was 70℃, the immersion time was 60min, and ultrasonic enhanced leaching was started simultaneously, with an ultrasonic frequency of 150kHz. After solid-liquid separation, a lithium-containing solution and water-leached residue were obtained. The water-leached residue was added to 3.5L of 0.2mol / L citric acid aqueous solution at 70℃, ultrasonically leached for 90min, and the ultrasonic frequency was 150kHz. After filtration, a cobalt-nickel-manganese-containing solution and leached residue were obtained.

[0054] Experiment 7: After fully discharging, disassembling, crushing and sorting the waste ternary lithium battery, the waste ternary lithium battery black powder was obtained. 4g of quartz sand was added to 1000g of ternary lithium battery black powder and fully mixed and then transferred to a ball mill. 1L of water was added to the tank, and hydrogen peroxide was added according to the mass ratio of ternary lithium battery black powder and hydrogen peroxide of 1:0.2, and ball milling was performed at a speed of 450rpm and a processing time of 30min. The slurry after ball milling was put into a water immersion reactor, and water was added to a solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 70℃, the water immersion time was 60min, and ultrasonic enhanced leaching was started simultaneously, and the ultrasonic frequency was 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained. The water leaching residue was added to 3.5L of 0.2mol / L sodium citrate aqueous solution at 70℃, ultrasonic leaching for 120min, and the ultrasonic frequency was 150kHz. After filtration, a cobalt-nickel-manganese-containing solution and leaching residue were obtained.

[0055] Experiment 8: After fully discharging, disassembling, crushing and sorting the waste ternary lithium battery, the waste ternary lithium battery black powder was obtained. 1000g of ternary lithium battery black powder was placed in a ball mill and 1L of water was added to the ball mill. Hydrogen peroxide was added according to the mass ratio of ternary lithium battery black powder to hydrogen peroxide of 1:0.2, and ball milling was performed at a speed of 450rpm for 90min. The ball milled slurry was put into a water immersion reactor, and water was added to a solid-liquid ratio of 250g / L for water immersion. The water immersion temperature was 70℃, the water immersion time was 60min, and ultrasonic enhanced leaching was started simultaneously, and the ultrasonic frequency was 150kHz. After filtration, a lithium-containing solution and water leaching residue were obtained. The water leaching residue was added to 3.5L of 0.2mol / L sodium citrate aqueous solution at 70℃, ultrasonic leaching for 120min, and the ultrasonic frequency was 150kHz. After filtration, a cobalt-nickel-manganese-containing solution and leaching residue were obtained.

[0056] The metal element content in the supernatant of each test sample after reaction was tested by inductively coupled plasma optical emission spectrometry (ICP-OES), and the leaching rate of each metal was calculated to obtain the statistical data shown in the following table:

[0057]

[0058]

[0059] From the results in the above table, we can see that this experiment uses different types of battery black powder materials, and by comparing the addition of different piezoelectric catalysts, the generation of mechanical stress and other control measures, the valuable metals in the waste lithium batteries are synergistically leached. The leaching effect of each metal is obvious, and the leaching rates of lithium, cobalt, nickel and manganese are 97.98%, 98.88%, 98.28% and 98.11% respectively.

[0060] Among them, according to Experiment 1 and Experiment 2, since Experiment 2 did not use quartz sand, although the amount of battery black powder and accelerator used in Experiment 2 was higher, the ball milling time, water immersion temperature, and water immersion time were also higher, the lithium leaching rate of Experiment 2 was greatly reduced. This shows that the use of piezoelectric materials can greatly increase the metal leaching rate of waste batteries.

[0061] According to Experiment 3 and Experiment 4, the method of generating mechanical stress in Experiment 3 is ball milling, and the method of generating mechanical stress in Experiment 4 is reciprocating vibration. The instantaneous mechanical stress generated by ball impact is greater than that of reciprocating motion, and the piezoelectric potential formed by greater mechanical stress on the piezoelectric material is greater, which is more conducive to the leaching of metal ions; although the amount of piezoelectric material, battery black powder, and accelerator used in Experiment 4 is greater, and the pre-leaching treatment time is also longer, the leaching effect is lower than that of Experiment 3. This shows that the magnitude of mechanical stress has a greater impact on the metal leaching rate of waste batteries, and the greater the mechanical stress, the more conducive to the leaching of metals.

[0062] According to Experiment 5 and Experiment 6, the piezoelectric material used in Experiment 5 is quartz sand, and the method of generating mechanical stress is ball milling. The piezoelectric material used in Experiment 6 is tourmaline, and the method of generating mechanical stress is aeration. The instantaneous mechanical stress generated by the impact of the ball during ball milling is greater, which is more than ten or even hundreds of times greater than the mechanical stress generated by aeration. The greater mechanical stress acts on the piezoelectric material to form a greater piezoelectric potential, which is more conducive to the catalytic leaching of metal ions. Different piezoelectric materials will also have a certain impact. The piezoelectric coefficient of tourmaline is much greater than that of quartz sand, but due to the smaller mechanical stress, the leaching effect of Experiment 6 is still worse than that of Experiment 5. It shows that the mechanical stress size and the piezoelectric coefficient of the piezoelectric material have a greater impact on the leaching effect of metal ions. Different piezoelectric materials will also have a certain impact. The piezoelectric coefficient of tourmaline is much greater than that of quartz sand, but due to the smaller mechanical stress, the leaching effect is still worse than that of Example 3, which shows that the mechanical stress size and the piezoelectric coefficient of the piezoelectric material have a greater impact on the leaching effect of metal ions.

[0063] According to Experiment 7 and Experiment 8, since quartz sand was not used in Experiment 8, although the ball milling treatment time in Experiment 8 was longer, the leaching rate of various ions (lithium, cobalt, nickel, and manganese) in Experiment 8 was greatly reduced. This shows that the use of piezoelectric materials can greatly increase the leaching rate of various ions in waste batteries.

[0064] According to Experiment 5 and Experiment 7, the organic solvent used in Experiment 5 is citric acid, and the organic solvent used in Experiment 7 is sodium citrate. By making the leaching time of Experiment 7 longer, the leaching rates of cobalt, nickel and manganese in Experiment 7 can be comparable to those in Experiment 5, indicating that citrate can be used as an organic solvent, that is, acidic reagents can be omitted.

[0065] In summary, the recovery method of the present invention has simple process, mild production conditions, low equipment requirements, safe and reliable process, clean and environmentally friendly, avoiding the high energy consumption and loss of metallic lithium caused by the use of pyrometallurgical process, and also reducing the use of large amounts of reducing agents and acids and alkalis relative to traditional wet process, effectively reducing the pressure of wastewater disposal at the back end of the environment, and expanding the technical support for the application scope of technology in the field of battery recycling.

[0066] The above contents are further detailed descriptions of the present application in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present application is limited to these descriptions. For ordinary technicians in the technical field to which the present application belongs, several simple deductions or substitutions can be made without departing from the concept of the present application.

Claims

1. A method for recovering valuable metals from waste batteries, characterized in that: include: Adding piezoelectric material to waste battery black powder and mixing evenly to obtain a mixed material; adding water and an accelerator to the mixture to obtain a prepreg system, and applying mechanical stress treatment to the prepreg system; adding water to the pre-impregnated system after mechanical stress treatment to obtain a water-immersed system, and applying ultrasound to the water-immersed system; Solid-liquid separation to obtain a leachate and a leached residue, wherein the leachate is a lithium-containing solution; in: The piezoelectric material is selected from at least one of inorganic piezoelectric crystals, inorganic piezoelectric ceramics and organic piezoelectric materials. The inorganic piezoelectric crystals include at least one of quartz crystals, tourmaline, barium titanate and its derivative structure crystals and ferroelectric crystals. The inorganic piezoelectric ceramics include at least one of lead zirconate titanate ceramics, barium titanate ceramics, aluminum nitride ceramics and zinc oxide ceramics. The organic piezoelectric material includes at least one of polyvinylidene fluoride and its copolymers and nylon. In the prepreg system, the content of the piezoelectric material is 0.2-10 g / L; The accelerator is selected from any one or more of hydrogen peroxide, ethanol, sodium sulfite, sodium bisulfite, glucose and ascorbic acid; The mass ratio of the battery black powder to the accelerator is 1:0.02 to 1:0.

5.

2. The recycling method according to claim 1, characterized in that: The battery black powder is obtained by disassembling, crushing and sorting the waste batteries after they are fully discharged; the battery black powder contains LiFePO4, LiCoO2, LiNiO2, LiMn2O4, LiNi x Co y Mn 1-x-y O2、LiNi x Co y Al 1-x-y At least one component of O2.

3. The recycling method according to claim 1, characterized in that: The piezoelectric material is quartz crystal or tourmaline.

4. The recycling method according to any one of claims 1 to 3, characterized in that: In the prepreg system, the content of the piezoelectric material is 0.2-5 g / L.

5. The recycling method according to claim 1, characterized in that: The method of generating the mechanical stress is selected from any one or more of ball milling, vibration, ultrasound, pressurization, stirring, friction, and aeration; and the time of the mechanical stress treatment is 10 to 60 minutes.

6. The recycling method according to claim 5, characterized in that: The mechanical stress is generated by ball milling, and the rotation speed of the ball mill is 350-500 rpm.

7. The recycling method according to claim 1 or 5, characterized in that: In the prepreg system, the solid-liquid ratio is 500-2000 g / L.

8. The recycling method according to claim 1, characterized in that: In the water immersion system, the frequency of ultrasound is 20-180 kHz.

9. The recycling method according to claim 1, characterized in that: In the water immersion system, the solid-liquid ratio is 100-500 g / L; the water immersion temperature is 25-95° C.; and the water immersion time is 20-120 min.

10. The recycling method according to claim 9, characterized in that: The water immersion temperature is 50~70℃.

11. The recycling method according to claim 1, characterized in that: The method further comprises adding the leaching residue into a leaching agent and applying ultrasonic treatment to obtain a cobalt-containing solution; Wherein, the leaching agent is selected from any one or more aqueous solutions of sodium citrate, citric acid, disodium ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid, tartaric acid, glycine and acetic acid.

12. The recycling method according to claim 11, characterized in that: The concentration of the leaching agent is 0.1-3 mol / L.

13. The recycling method according to claim 12, characterized in that: The solid-to-liquid ratio of the leaching residue to the leaching agent is 50-500 g / L.

14. The recycling method according to claim 11, characterized in that: The frequency of the ultrasound in the ultrasonic treatment is 20-180 kHz.