A preparation method and application of modified resin catalyst

By using the evaporated ammonia deposition method to load metal elements on the resin, a highly active and stable modified resin catalyst is prepared, which solves the problems of high production cost and poor catalyst stability during the synthesis of triacetoneamine, and achieves efficient catalysis and long-term stability. use.

CN118218022BActive Publication Date: 2024-10-18宿迁联盛科技股份有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410658605.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-18
Estimated Expiration
2044-05-27

Smart Images

  • Figure CN118218022B_ABST
    Figure CN118218022B_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a modified resin catalyst. The method comprises the following steps: a sulfonic acid resin is swollen and washed and then carbonized; the carbonized catalyst is aminated and then loaded with metal substances by an ammonia evaporation deposition method; and the desired catalyst is obtained by calcination and hydrogen ion replacement. The catalyst prepared by the method has rich pore structure, large specific surface area, and firmly anchored metal elements. The synergistic catalytic effect of inorganic-organic and L-acid-B-acid can make the catalyst have high catalytic activity, selectivity and stability. The prepared catalyst is applied in a fixed bed synthesis process of triacetoneamine, has high acetone conversion rate and high triacetoneamine selectivity, and has extremely high industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to the preparation and application of a catalyst for modified resin. Background Art

[0002] Polymer materials are widely used in industry and agriculture, but they are prone to aging under the influence of light, oxygen, heat, etc. For example, rubber products become sticky and hardened, plastics and fiber products become discolored and brittle, etc. In industry, light stabilizers are often added to polymer materials to extend the service life of the materials. Hindered amine light stabilizers have the advantages of excellent light stabilization effect, low cost, easy availability, and good compatibility, and they occupy a pivotal position in the field of light stabilizers. 2,2,6,6-Tetramethyl-4-piperidone (triacetoneamine) is the structural unit of many light stabilizers and is also the derivative parent of many fine chemical intermediates.

[0003] The synthesis of triacetoneamine reported so far mainly includes indirect method and direct method. The indirect method is to use acetone as raw material, first synthesize fluorone, diacetone alcohol, and acetone nitrile under the action of a catalyst, and then synthesize triacetoneamine through catalytic reaction. CN111285794A discloses an improved method for preparing triacetoneamine, wherein the crude product triacetoneamine, acetone, isopropyl acetate and a constituent raw material of diacetone alcohol, diacetoneamine, acetone nitrile, phorone, and diphorone are subjected to catalytic reaction to obtain triacetoneamine. US 3943139 discloses a method for obtaining triacetoneamine through catalytic reaction of phorone and ammonia. The yield of synthesizing triacetoneamine by the indirect method is acceptable, but phorone, diacetone alcohol, and acetone nitrile have similar boiling points, and the synthesis and separation process are difficult. Therefore, the indirect method for producing triacetoneamine will increase production costs and is difficult to achieve industrial production.

[0004] The direct method uses acetone and ammonia as raw materials to synthesize triacetoneamine under the action of a catalyst. CN 110947412B discloses a magnesium aluminum hydrotalcite composite microsphere and a preparation method thereof, and a preparation method of triacetoneamine. In this method, magnesium aluminum hydrotalcite is loaded on multi-walled carbon nanotubes, and triacetoneamine is synthesized by catalysis. The catalyst synthesized by this method has poor stability and a complicated catalytic process. CN 114797896A discloses a preparation method and a use method of a catalyst for fixed bed synthesis of 2,2,6,6-tetramethyl-4-piperidone, wherein metal ions are impregnated on D072, D061, and NKC-9 resins by an impregnation method, and triacetoneamine is synthesized by using this as a catalyst. In this method, the metal ions are loaded on the resin only by adsorption, and the metal active center is easy to fall off, so the stability of the catalyst is poor.

[0005] The purpose of the present invention is to propose a preparation and application of a modified resin catalyst. The sulfonic acid resin is swollen and washed and then carbonized. The carbonized catalyst is aminated and loaded with metal substances using an ammonia evaporation deposition method, and then calcined and hydrogen ion replaced to obtain the desired catalyst. Summary of the invention

[0006] In order to solve the above problems, the present invention discloses the preparation and application of a modified resin catalyst, wherein a metal element is loaded on a resin treated with carbonization and ammoniation by an ammonia evaporation deposition method, thereby obtaining a novel catalyst with inorganic-organic and L-acid-B-acid synergistic effects. The catalyst has high catalytic activity, selectivity and stability. The catalyst can efficiently catalyze the synthesis of triacetoneamine, achieve high-yield conversion of triacetoneamine, and can be used for a long time and stably in a fixed bed reaction process.

[0007] To achieve the above object, the technical solution of the present invention is as follows:

[0008] A method for preparing a modified resin catalyst, characterized in that it comprises the following steps:

[0009] (1) Soak the resin in deionized water to fully swell it, wash the swollen resin with deionized water until the washing liquid is clear, dry the washed resin in an oven, and continue to dry it in a vacuum drying oven;

[0010] (2) The dried resin is placed in a tubular furnace and calcined at 200-400°C for 3-6 hours in a N2 atmosphere;

[0011] (3) Soaking the calcined resin in 25 wt.% ammonia water to obtain a mixture A;

[0012] (4) Dissolve the metal nitrate in deionized water, add 25 wt.% ammonia water, and stir for 30 min to obtain solution B;

[0013] (5) Pour solution B into mixture A and stir for aging for 4 to 8 hours;

[0014] (6) heating the mixture obtained by aging in step (5) to evaporate ammonia in the solution until the pH of the solution is 5-7, filtering to obtain a solid, washing with deionized water, drying the washed solid in an oven, and further drying in a vacuum drying oven to obtain a solid C;

[0015] (7) placing solid C in a tubular furnace and calcining it under a N2 atmosphere to obtain solid D;

[0016] (8) Place solid D in a quartz tube and pass 0.5~1 mol / L hydrochloric acid solution into the quartz tube at a speed of 5 m / h from the bottom to replace the NH4 +Then, deionized water is passed into the quartz tube from the lower end at a speed of 10 m / h to remove the residual hydrochloric acid in the resin; the replaced solid is placed in an oven for drying, and then placed in a vacuum drying oven for drying to obtain a metal-modified resin catalyst.

[0017] Furthermore, in step (1), the resin is one of K 2621, K 2629, HD 587, Amberlyst 36, Amberlyst 15, and NKC-9, and during immersion, the volume ratio of the resin to deionized water is 1:10-20.

[0018] Furthermore, in step (3), the mass volume ratio of the calcined resin to the ammonia water is 1:4-8, and the soaking time is 8-24 hours.

[0019] Furthermore, in step (4), the metal nitrate is dissolved in deionized water to obtain a metal nitrate solution with a concentration of 0.1-2 mol / L, and the volume ratio of the metal salt solution to 25 wt.% ammonia water is 1:0.2-0.6.

[0020] Furthermore, the nitrate is one or more of Al(NO3)3·9H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Ce(NO3)2·6H2O, La(NO3)3·6H2O, Ba(NO3)2, Zn(NO3)2·6H2O, and Mg(NO3)2·6H2O.

[0021] Furthermore, in step (6), the mixture obtained by aging in step (5) is heated to 40-80° C. to evaporate ammonia in the solution.

[0022] Furthermore, in step (7), the calcination temperature is 400-600° C., and the calcination time is 4-7 hours.

[0023] Furthermore, in step (8), the volume ratio of the hydrochloric acid solution to the solid D is 1-4:1, and the volume ratio of the deionized water to the hydrochloric acid solution is 5-20:1.

[0024] The present invention also provides a modified resin catalyst prepared by the above preparation method.

[0025] The present invention also provides the use of the modified resin catalyst in the synthesis of triacetoneamine.

[0026] The application comprises the following steps:

[0027] (1) The modified resin catalyst is loaded into a fixed bed reactor, and the fixed bed is heated and kept warm using an electric heating furnace.

[0028] (2) N2 gas was continuously introduced into the fixed bed reactor for 12 h to discharge the impurity gases inside the fixed bed system.

[0029] (3) Turn on the heating furnace and maintain the internal temperature of the fixed bed at 40-80°C. After the acetone and ammonia are mixed in the gas-liquid mixer, they pass through the fixed bed reactor from top to bottom. The feed molar ratio of acetone to ammonia is 1:2-15, and the volumetric space velocity of ammonia is 3.5-12.5h -1 .

[0030] (4) The reaction product flows into the product storage tank. After cooling, the product obtains triacetoneamine reaction liquid. Samples are taken every 8 hours and the acetone and triacetoneamine contents are detected by gas chromatography.

[0031] The synthetic route of the reaction of the present invention is:

[0032]

[0033] The beneficial effects of the present invention are:

[0034] (1) The present invention uses sulfonic acid resin as raw material, and can effectively remove small molecules and oligomeric organic matter and inorganic matter in the raw material through swelling treatment, thereby increasing the specific surface area of ​​the resin, thereby increasing the utilization rate of the resin pores and the activity of the catalyst.

[0035] (2) The resin catalyst is treated with N2 atmosphere. The carbonization treatment can remove excess H in the resin and small molecules in the pores to form more carbon skeletons, providing more loading sites for metal element precipitation and exposing more sulfonic acid active substances to the catalytic environment.

[0036] (3) The addition of metal elements and the hydrochloric acid treatment process provide the catalyst with more L-acid and B-acid sites, thereby increasing the acidity of the catalyst. The synergistic effect of L-acid and B-acid can effectively enhance the activity of the catalyst.

[0037] (4) The synergistic effect of multiple metal salts increases the active sites of the catalyst, and organic catalysis and inorganic catalysis proceed in a coordinated manner, effectively improving the activity and stability of the catalyst.

[0038] (5) The metal elements are loaded onto the carbonized resin by the ammonia vapor deposition method. The metal elements are more evenly distributed, the metal particles are smaller, the metal crystals are higher, the anchoring is more firm, and the metal active components are not easy to lose. Therefore, the catalyst loaded with metal has higher catalytic activity and catalytic stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the N2 isotherm adsorption-desorption curve of the catalyst prepared in Example 1 of the present invention, and the inset is the pore size distribution diagram. DETAILED DESCRIPTION

[0040] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0041] The manufacturers and models of the compounds used in the following examples are as follows; other chemical reagents used, unless otherwise specified, were obtained through conventional commercial channels:

[0042]

[0043] Example 1

[0044] The preparation steps of the modified resin catalyst are as follows:

[0045] (1) Take 50 ml of K2621 resin and put it into a beaker. Soak it in 500 ml of deionized water for 24 hours until the resin is fully swollen. Wash the swollen resin with deionized water until the washing liquid is clear. Dry the washed resin in an oven at 100°C for 12 hours, and then continue to dry it in a vacuum drying oven at 60°C for 12 hours.

[0046] (2) The dried resin was placed in a tubular furnace and calcined at 300 °C for 5 h in a N2 atmosphere.

[0047] (3) The calcined resin was placed in 300 ml of 25 wt.% ammonia water and soaked for 12 h to obtain a mixture A.

[0048] (4) Weigh 37.5 g of aluminum nitrate nonahydrate and dissolve it in 100 ml of deionized water. Add 30 ml of 25 wt.% ammonia water and stir for 30 min to obtain solution B.

[0049] (5) Pour solution B into mixture A and stir for 4 h.

[0050] (6) The above mixture was placed in a water bath and heated at 80°C to evaporate the ammonia in the solution until the pH of the solution was 6. The solid was filtered out and washed eight times with 500 ml of deionized water. The washed solid was placed in an oven and dried at 100°C for 12 h. The solid was then placed in a vacuum drying oven and dried at 60°C for 12 h to obtain solid C.

[0051] (7) Solid C was placed in a tubular furnace and calcined at 450 °C for 5 h under a N2 atmosphere to obtain solid D.

[0052] (8) Place solid D in a quartz tube and pass 100 ml of 1 mol / L hydrochloric acid solution into the tube from the bottom at a rate of 5 m / h to displace the NH4 +; Continue to use 1000 ml of deionized water to pass into the quartz tube from the lower end at a speed of 10 m / h to remove the residual hydrochloric acid in the resin. The replaced solid is placed in an oven at 100°C for 12 hours, and then placed in a vacuum drying oven at 60°C for 12 hours to obtain a metal-modified resin catalyst, which is recorded as CAT-1.

[0053] The N2 isothermal adsorption-desorption curve of the catalyst prepared in Example 1 of the present invention is as follows: Figure 1 As shown, Figure 1 The inset is the pore size distribution diagram; the specific surface area of ​​the catalyst is 85m 2 / g, the pore size is mainly distributed in the range of 26~59nm, the catalyst has a certain specific surface area, and the pore size distribution is relatively concentrated, which makes the catalyst have a higher reaction activity.

[0054] Example 2

[0055] The preparation steps of modified resin catalyst are as follows:

[0056] The other conditions were the same as those in Example 1, except that the resin type in step (1) was changed to HD 587, and the obtained catalyst was denoted as CAT-2.

[0057] Example 3

[0058] The preparation steps of modified resin catalyst are as follows:

[0059] The other conditions were the same as those in Example 1, except that the resin type in step (1) was changed to Amberlyst 36, and the obtained catalyst was denoted as CAT-3.

[0060] Example 4

[0061] The preparation steps of modified resin catalyst are as follows:

[0062] The other conditions were the same as those in Example 1, except that the volume of deionized water used for soaking in step (1) was changed to 1000 ml. The obtained catalyst was designated as CAT-4.

[0063] Example 5

[0064] The preparation steps of modified resin catalyst are as follows:

[0065] The other conditions were the same as those in Example 1, except that the calcination temperature in N2 atmosphere in step (2) was changed to 200°C. The obtained catalyst was designated as CAT-5.

[0066] Example 6

[0067] The preparation steps of modified resin catalyst are as follows:

[0068] The other conditions were the same as those in Example 1, except that the calcination time in N2 atmosphere in step (2) was changed to 3 h. The obtained catalyst was designated as CAT-6.

[0069] Example 7

[0070] The preparation steps of modified resin catalyst are as follows:

[0071] The other conditions were the same as those in Example 1, except that the amount of ammonia water added in step (3) was changed to 200 ml. The obtained catalyst was denoted as CAT7.

[0072] Example 8

[0073] The preparation steps of modified resin catalyst are as follows:

[0074] The other conditions were the same as those in Example 1, except that the soaking time in step (3) was changed to 8 h. The obtained catalyst was designated as CAT-8.

[0075] Example 9

[0076] The preparation steps of modified resin catalyst are as follows:

[0077] The other conditions were the same as those in Example 1, except that the type and amount of metal nitrate added in step (4) were changed: 43.4 g of cerium nitrate hexahydrate was weighed and dissolved in 100 ml of deionized water. The resulting catalyst was recorded as CAT-9.

[0078] Example 10

[0079] The preparation steps of modified resin catalyst are as follows:

[0080] The other conditions were the same as those in Example 1, except that the amount of aqueous ammonia added in step (4) was changed to 60 ml. The obtained catalyst was denoted as CAT-10.

[0081] Embodiment 11

[0082] The preparation steps of modified resin catalyst are as follows:

[0083] The other conditions were the same as those in Example 1, except that the aging time in step (5) was changed to 6 h. The obtained catalyst was designated as CAT-11.

[0084] Example 12

[0085] The preparation steps of modified resin catalyst are as follows:

[0086] The other conditions were the same as those in Example 1, except that the water bath temperature in step (6) was changed to 40°C. The obtained catalyst was designated as CAT-12.

[0087] Example 13

[0088] The preparation steps of modified resin catalyst are as follows:

[0089] The other conditions were the same as those in Example 1, except that the pH of the titration endpoint solution in step (6) was changed to a solution pH of 5. The obtained catalyst was recorded as CAT-13.

[0090] Embodiment 14

[0091] The preparation steps of modified resin catalyst are as follows:

[0092] The other conditions were the same as those in Example 1, except that the calcination temperature in N2 atmosphere in step (7) was changed to 600°C. The obtained catalyst was designated as CAT-14.

[0093] Embodiment 15

[0094] The preparation steps of modified resin catalyst are as follows:

[0095] The other conditions were the same as those in Example 1, except that the calcination time in N2 atmosphere in step (7) was changed to 4 h. The obtained catalyst was denoted as CAT-15.

[0096] Example 16

[0097] The preparation steps of modified resin catalyst are as follows:

[0098] The other conditions were the same as those in Example 1, except that the concentration of hydrochloric acid in step (8) was changed to 0.5 mol / L. The obtained catalyst was denoted as CAT-16.

[0099] Embodiment 17

[0100] The preparation steps of modified resin catalyst are as follows:

[0101] The other conditions were the same as those in Example 1, except that the amount of hydrochloric acid used in step (7) was changed to 200 ml. The obtained catalyst was designated as CAT-17.

[0102] Comparative Example 1

[0103] The purpose is to compare with Example 1 to illustrate the effect of the swelling step on the catalytic activity.

[0104] The preparation steps of modified resin catalyst are as follows:

[0105] (1) Take 50 ml of K 2621 resin and put it into a beaker. Wash it with deionized water until the washing liquid is clear. Dry the washed resin in an oven at 100°C for 12 hours and then dry it in a vacuum drying oven at 60°C for 12 hours.

[0106] (2) The dried resin was placed in a tubular furnace and calcined at 300 °C for 5 h in a N2 atmosphere.

[0107] (3) The calcined resin was placed in 300 ml of 25 wt.% ammonia water and soaked for 12 h to obtain a mixture A.

[0108] (4) Weigh 37.5 g of aluminum nitrate nonahydrate and dissolve it in 100 ml of deionized water. Add 30 ml of 25 wt.% ammonia water and stir for 30 min to obtain solution B.

[0109] (5) Pour solution B into mixture A and stir for 4 h.

[0110] (6) The above mixture was placed in a water bath and heated at 80°C to evaporate the ammonia in the solution until the pH of the solution was 6. The solid was filtered out and washed eight times with 500 ml of deionized water. The washed solid was placed in an oven and dried at 100°C for 12 h. The solid was then placed in a vacuum drying oven and dried at 60°C for 12 h to obtain solid C.

[0111] (7) Solid C was placed in a tubular furnace and calcined at 450 °C for 5 h under a N2 atmosphere to obtain solid D.

[0112] (8) Place solid D in a quartz tube and pass 100 ml of 1 mol / L hydrochloric acid solution into the tube from the bottom at a rate of 5 m / h to displace the NH4 + ; Continue to use 1000 ml of deionized water to pass into the quartz tube from the lower end at a speed of 10 m / h to remove the residual hydrochloric acid in the resin. The replaced solid is placed in an oven at 100°C for 12 hours, and then placed in a vacuum drying oven at 60°C for 12 hours to obtain a metal-modified resin catalyst, which is recorded as CAT-18.

[0113] Comparative Example 2

[0114] The purpose is to compare with Example 1 to illustrate the effect of the carbonization step on the catalytic activity.

[0115] The preparation steps of modified resin catalyst are as follows:

[0116] (1) Take 50 ml of K 2621 resin and put it into a beaker. Soak it in 500 ml of deionized water for 24 hours until the resin is fully swollen. Wash the swollen resin with deionized water until the washing liquid is clear. Dry the washed resin in an oven at 100°C for 12 hours, and then continue to dry it in a vacuum drying oven at 60°C for 12 hours.

[0117] (2) The dried resin was placed in 300 ml of 25 wt.% ammonia water and soaked for 12 h to obtain a mixture A.

[0118] (3) Weigh 37.5 g of aluminum nitrate nonahydrate and dissolve it in 100 ml of deionized water. Add 30 ml of 25 wt.% ammonia water and stir for 30 min to obtain solution B.

[0119] (4) Pour solution B into mixture A and stir for 4 h.

[0120] (5) The above mixture was placed in a water bath and heated at 80°C to evaporate the ammonia in the solution until the pH of the solution was 6. The solid was filtered out and washed 8 times with 500 ml of deionized water. The washed solid was placed in an oven and dried at 100°C for 12 h. It was then placed in a vacuum drying oven and dried at 60°C for 12 h to obtain solid C.

[0121] (6) Solid C was placed in a tubular furnace and calcined at 450 °C for 5 h under a N2 atmosphere to obtain solid D.

[0122] (7) Place solid D in a quartz tube and pass 100 ml of 1 mol / L hydrochloric acid solution into the tube from the bottom at a rate of 5 m / h to displace the NH4 + ; Continue to use 1000 ml of deionized water to pass into the quartz tube from the lower end at a speed of 10 m / h to remove the residual hydrochloric acid in the resin. The replaced solid is placed in an oven at 100°C for 12 hours, and then placed in a vacuum drying oven at 60°C for 12 hours to obtain a metal-modified resin catalyst, which is recorded as CAT-19.

[0123] Comparative Example 3

[0124] The purpose is to compare with Example 1 to illustrate the effect of the ammonia soaking step on the catalytic activity.

[0125] The preparation steps of modified resin catalyst are as follows:

[0126] (1) Take 50 ml of K2621 resin and put it into a beaker. Soak it in 500 ml of deionized water for 24 hours until the resin is fully swollen. Wash the swollen resin with deionized water until the washing liquid is clear. Dry the washed resin in an oven at 100°C for 12 hours, and then continue to dry it in a vacuum drying oven at 60°C for 12 hours.

[0127] (2) The dried resin was placed in a tubular furnace and calcined at 300°C for 5 h under a N2 atmosphere to obtain solid A.

[0128] (3) Weigh 37.5 g of aluminum nitrate nonahydrate and dissolve it in 100 ml of deionized water. Add 30 ml of 25 wt.% ammonia water and stir for 30 min to obtain solution B.

[0129] (4) Place solid A into solution B and stir for 4 h.

[0130] (5) The above mixture was placed in a water bath and heated at 80°C to evaporate the ammonia in the solution until the pH of the solution was 6. The solid was filtered out and washed 8 times with 500 ml of deionized water. The washed solid was placed in an oven and dried at 100°C for 12 h. It was then placed in a vacuum drying oven and dried at 60°C for 12 h to obtain solid C.

[0131] (6) Solid C was placed in a tubular furnace and calcined at 450 °C for 5 h under a N2 atmosphere to obtain solid D.

[0132] (7) Place solid D in a quartz tube and pass 100 ml of 1 mol / L hydrochloric acid solution into the tube from the bottom at a rate of 5 m / h to displace the NH4 + ; Continue to use 1000 ml of deionized water to pass into the quartz tube from the lower end at a speed of 10 m / h to remove the hydrochloric acid remaining in the resin. The replaced solid is placed in an oven at 100°C for 12 hours, and then placed in a vacuum drying oven at 60°C for 12 hours to obtain a metal-modified resin catalyst, which is recorded as CAT-20.

[0133] Comparative Example 4

[0134] The purpose is to compare with Example 1 to illustrate the effect of the metal salt loading step on the catalytic activity.

[0135] The preparation steps of modified resin catalyst are as follows:

[0136] (1) Take 50 ml of K2621 resin and put it into a beaker. Soak it in 500 ml of deionized water for 24 hours until the resin is fully swollen. Wash the swollen resin with deionized water until the washing liquid is clear. Dry the washed resin in an oven at 100°C for 12 hours, and then continue to dry it in a vacuum drying oven at 60°C for 12 hours.

[0137] (2) The dried resin was placed in a tubular furnace and calcined at 300 °C for 5 h in a N2 atmosphere.

[0138] (3) Place solid D in a quartz tube and pass 100 ml of 1 mol / L hydrochloric acid solution into the tube from the bottom at a speed of 5 m / h to replace the NH4 + ; Continue to use 1000 ml of deionized water to pass into the quartz tube from the lower end at a speed of 10 m / h to remove the hydrochloric acid remaining in the resin. The replaced solid is placed in an oven at 100°C for 12 hours, and then placed in a vacuum drying oven at 60°C for 12 hours to obtain a metal-modified resin catalyst, which is recorded as CAT-21.

[0139] Comparative Example 5

[0140] The purpose is to compare with Example 1 to illustrate the effect of the support calcination step on the catalytic activity.

[0141] The preparation steps of modified resin catalyst are as follows:

[0142] (1) Take 50 ml of K2621 resin and put it into a beaker. Soak it in 500 ml of deionized water for 24 hours until the resin is fully swollen. Wash the swollen resin with deionized water until the washing liquid is clear. Dry the washed resin in an oven at 100°C for 12 hours, and then continue to dry it in a vacuum drying oven at 60°C for 12 hours.

[0143] (2) The dried resin was placed in a tubular furnace and calcined at 300 °C for 5 h in a N2 atmosphere.

[0144] (3) The calcined resin was placed in 300 ml of 25 wt.% ammonia water and soaked for 12 h to obtain a mixture A.

[0145] (4) Weigh 37.5 g of aluminum nitrate nonahydrate and dissolve it in 100 ml of deionized water. Add 30 ml of 25 wt.% ammonia water and stir for 30 min to obtain solution B.

[0146] (5) Pour solution B into mixture A and stir for 4 h.

[0147] (6) The above mixture was placed in a water bath and heated at 80°C to evaporate the ammonia in the solution until the pH of the solution was 6. The solid was filtered out and washed eight times with 500 ml of deionized water. The washed solid was placed in an oven and dried at 100°C for 12 h. The solid was then placed in a vacuum drying oven and dried at 60°C for 12 h to obtain solid C.

[0148] (7) Place solid C in a quartz tube and pass 100 ml of 1 mol / L hydrochloric acid solution into the tube at a rate of 5 m / h from the bottom to displace the NH4 + ; Continue to use 1000 ml of deionized water to pass into the quartz tube from the lower end at a speed of 10 m / h to remove the hydrochloric acid remaining in the resin. The replaced solid is placed in an oven at 100°C for 12 hours, and then placed in a vacuum drying oven at 60°C for 12 hours to obtain a metal-modified resin catalyst, which is recorded as CAT-22.

[0149] The evaluation process and conditions of the catalyst are:

[0150] (1) 200 ml of catalyst was loaded into a fixed bed reactor with an inner diameter of 30 mm and a length of 800 mm, and the fixed bed was heated and kept warm using an electric heating furnace.

[0151] (2) N2 gas was continuously introduced into the fixed bed reactor for 12 h to discharge the impurity gases inside the fixed bed system.

[0152] (3) Connect circulating water to maintain the internal temperature of the fixed bed at 63°C. Acetone and ammonia are mixed in the gas-liquid mixer and then pass through the fixed bed reactor from top to bottom. The feed molar ratio of acetone to ammonia is 1:6.5, and the volumetric space velocity of ammonia is 10h -1 .

[0153] (4) The reaction product flows into the product storage tank. After cooling, the product obtains triacetoneamine reaction liquid. Samples are taken every 8 hours and the acetone and triacetoneamine contents are detected by gas chromatography.

[0154] The reaction was carried out using CAT-1 to CAT-22 as catalysts. Each catalyst was evaluated for 240 hours. The average acetone conversion rate and the average selectivity of triacetoneamine were shown in Table 1 below:

[0155] Table 1

[0156]

[0157] The present invention changes the conditions to prepare a series of modified resin catalysts, among which the catalyst using Amberlyst 36 resin to deposit aluminum has the highest reaction activity, and the average acetone conversion rate reaches 63.9% after continuous operation for 120 minutes, and the average triacetone amine selectivity reaches 67.6%. The activity and selectivity of the prepared catalysts are different under different reaction conditions, among which the activity and selectivity of the catalyst without ammoniation deposited aluminum are the worst, and the average acetone conversion rate is 10.6% and the average triacetone amine selectivity is 15.3% after continuous operation for 240 hours. The reason is that since no ammoniation is performed before aluminum deposition, the sulfonic acid group in the active center is converted into aluminum sulfonate, and aluminum sulfonate is relatively stable during the reaction process, which reduces the reaction activity and selectivity of the resin catalyst.

[0158] It should be noted that the above content only illustrates the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a modified resin catalyst, It is characterized in that The following steps are involved: (1) Soak the resin in deionized water to fully swell it, wash the swollen resin with deionized water until the washing liquid is clear, dry the washed resin in an oven, and continue to dry it in a vacuum drying oven; (2) The dried resin is placed in a tube furnace at N 2 Calcinate at 200-400℃ for 3-6h under atmosphere; (3) Soaking the calcined resin in 25 wt% ammonia water to obtain a mixture A; (4) Dissolve the metal nitrate in deionized water, add 25 wt% ammonia water, and stir for 30 min to obtain solution B; (5) Pour solution B into mixture A and stir for aging for 4 to 8 hours; (6) heating the mixture obtained by aging in step (5) to evaporate ammonia in the solution until the pH of the solution is 5-7, filtering to obtain a solid, washing with deionized water, drying the washed solid in an oven, and further drying in a vacuum drying oven to obtain a solid C; (7) Place solid C in a tube furnace and heat it under N 2 Calcination under atmosphere to obtain solid D; (8) Put solid D into a quartz tube, use 0.5~1 mol / L hydrochloric acid solution to pass into the quartz tube from the lower end at a speed of 5m / h, and then use deionized water to pass into the quartz tube from the lower end at a speed of 10m / h; put the replaced solid into an oven for drying, and then put it into a vacuum drying oven for drying, so as to obtain a metal-modified resin catalyst; The resin is a sulfonic acid type resin.

2. A method for preparing a modified resin catalyst according to claim 1, It is characterized in that In step (1), the resin is one of K 2621, K 2629, HND 587, Amberlyst 36, Amberlyst 15, and NKC-9.

3. A method for preparing a modified resin catalyst according to claim 1, It is characterized in that In step (3), the mass volume ratio of the calcined resin to 25wt% ammonia water is 1:4-8, and the soaking time is 8-24h.

4. A method for preparing a modified resin catalyst according to claim 1, It is characterized in that In step (4), metal nitrate is dissolved in deionized water to obtain a metal nitrate solution with a concentration of 0.1-2 mol / L, and the volume ratio of the metal salt solution to 25 wt% ammonia water is 1:0.2-0.

6.

5. A method for preparing a modified resin catalyst according to claim 4, It is characterized in that The nitrate is Al(NO 3 ) 3 9H 2 O.Ni(NO 3 ) 2 6H 2 O, Cu(NO 3 ) 2 ·3H 2 O、Ce(NO 3 ) 2 6H 2 O、La(NO 3 ) 3 6H 2 O、Ba(NO 3 ) 2、 Zn(NO 3 ) 2 6H 2 O、Mg(NO 3 ) 2 6H 2 One or more of O.

6. A method for preparing a modified resin catalyst according to claim 1, It is characterized in that In step (6), the mixture obtained by aging in step (5) is heated to 40-80° C. to evaporate ammonia in the solution.

7. The method for preparing a modified resin catalyst according to claim 1, It is characterized in that In step (7), the calcination temperature is 400-600° C. and the calcination time is 4-7 hours.

8. The method for preparing a modified resin catalyst according to claim 1, It is characterized in that In step (8), the volume ratio of the hydrochloric acid solution to the solid D is 1-4:1, and the volume ratio of the deionized water to the hydrochloric acid solution is 5-20:

1.

9. A modified resin catalyst prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the modified resin catalyst as claimed in claim 9 in the synthesis of triacetoneamine.

Citation Information

Patent Citations

  • Magnesium-aluminum hydrotalcite composite microspheres and their preparation methods, and the preparation method of triacetone amine.

    CN110947412B

  • Method for preparing triacetone amine

    CN111285794A

  • Preparation and use method of catalyst for fixed bed synthesis of 2, 2, 6, 6-tetramethyl-4-piperidone

    CN114797896A

  • Process for the manufacture of triacetone-amine

    US3943139A

  • Modified cation exchange resin catalyst and its preparation method and application

    CN103769215A