Color-changing asphalt waterproofing coiled material and preparation method thereof
By using a color-changing isolation film on asphalt waterproof roll, the color-changing agent generates gas at a specific temperature to make the isolation film melt quickly, solving the problem of difficult temperature control during fire-baking construction, and improving the bonding area and construction reliability , reducing the potential risk of water rushing.
Patent Information
- Application Number
- CN202410282036.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-12
AI Technical Summary
The existing asphalt waterproof coils are difficult to control the flame temperature and time during the fire-baking construction process, resulting in a decrease in bonding performance, and excessive PE isolation film residues lead to a potential water leakage.
Use a changeable isolation film, which contains a discolorant that discolors at 180℃~350℃ and produces gas. When heated, the gas expands to destroy the isolation film structure, causing it to melt and shrink quickly, fully expose the asphalt coating material, increase the bonding area and reduce the disconnection. Water hazard.
Control the fire roasting progress through the color change of the color change agent, ensure full bonding, improve construction quality and reliability, and reduce the risk of water trapping.
Smart Images

Figure CN118219638B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of waterproofing membrane technology, and in particular to a color-changing asphalt waterproofing membrane and a preparation method thereof. Background Art
[0002] Asphalt waterproofing membrane is one of the waterproofing materials with the highest production and the widest application in the field of waterproofing membrane. During the construction process of asphalt waterproofing membrane, hot air or fire baking is required to heat-melt the PE isolation film on its surface so that the asphalt coating inside the asphalt waterproofing membrane can be bonded and overlapped with the construction base.
[0003] The current baking process is relatively crude, and the flame temperature and baking time are difficult to control. If the baking is insufficient, the PE isolation film on the surface of the asphalt waterproofing membrane cannot be completely melted, which will lead to a decrease in bonding performance; and excessive baking will cause the polymer in the asphalt waterproofing membrane to decompose and the material performance to decrease. In addition, the PE isolation film often has a large area of residue after melting, which causes the coating layer on the membrane to not be completely exposed, and the membrane and the base layer cannot be fully bonded, which is prone to leaks and causes hidden dangers of water leakage. Summary of the invention
[0004] In view of the problems existing in the prior art, the embodiments of the present application provide a color-changing asphalt waterproofing membrane and a preparation method thereof, in order to improve the problems existing in the asphalt waterproofing membrane during the fire-baking construction process.
[0005] An embodiment of the first aspect of the present application provides a color-changing asphalt waterproofing membrane, comprising a waterproof core layer and a color-changing isolation membrane arranged on at least one side surface of the waterproof core layer; the color-changing isolation membrane comprises a color-changing agent, and the color-changing agent comprises a color-changing material that can change color and generate gas at a color-changing temperature, and the color-changing temperature is 180°C to 350°C.
[0006] The color-changing isolation membrane will produce gas when it decomposes and changes color when heated. These gases can expand rapidly and destroy the structure of the color-changing isolation membrane, causing the color-changing isolation membrane to melt and shrink rapidly. The asphalt coating on the surface of the waterproof core layer can be fully exposed, reducing the residual isolation membrane on the surface of the waterproof core layer, which can increase the bonding area of the waterproof membrane and allow the waterproof membrane to fully contact the base layer, thereby reducing the risk of water seepage and improving construction quality and reliability.
[0007] In some embodiments, the color-changing agent includes one or more of indigo·TiO2, Cu(OH)2, (NH4)2Cr2O7, and CdCO3.
[0008] In some embodiments, the waterproof core layer includes a tread base layer and an asphalt coating layer disposed on both sides of the tread base layer, and the asphalt coating layer includes the following raw material compositions in parts by weight: 40 parts of base asphalt; 1 to 10 parts of oil; 6 to 18 parts of rubber powder; and 20 to 40 parts of filler.
[0009] In some embodiments, the base asphalt includes one or more of 70# asphalt, 90# asphalt, and 200# asphalt.
[0010] In some embodiments, the filler includes one or more of talc, heavy calcium, montmorillonite, and kaolin.
[0011] In some embodiments, the rubber powder includes one or more of tire rubber powder, miscellaneous rubber powder, and shoe rubber powder.
[0012] In some embodiments, the raw materials of the asphalt coating layer also include 3 to 8 parts by weight of functional additives, and the functional additives include one or more of ferric orthophosphate, aluminum orthophosphate, ferric chloride, sodium silicate, sodium dichromate, sodium hexametaphosphate, and kaolin.
[0013] In some embodiments, the raw materials of the asphalt coating layer also include 2 to 8 parts by weight of a modifier, and the modifier includes one or more of butadiene-styrene-butadiene triblock copolymer, styrene-butadiene rubber, hydrogenated styrene-butadiene block copolymer, and butadiene-isoprene-butadiene triblock copolymer.
[0014] In some embodiments, the thickness of the color-changing isolation film is 10 μm to 30 μm.
[0015] In some embodiments, the waterproof core layer has a thickness of 2.8 mm to 4 mm.
[0016] The embodiment of the second aspect of the present application provides a method for preparing a color-changing asphalt waterproofing membrane, comprising the following steps:
[0017] Provide waterproof core layer and color-changing isolation film respectively;
[0018] The color-changeable isolation film is coated on at least one side of the waterproof core layer to obtain the asphalt waterproofing membrane.
[0019] In some embodiments, providing a color-variable isolation film comprises:
[0020] Polyvinyl alcohol and a color-changing agent are dispersed in a volatile organic solvent to obtain a mixture;
[0021] At least part of the volatile organic solvent in the mixture is removed, and the mixture is dried to form a film to obtain a color-changeable isolation film.
[0022] In some embodiments, the volatile organic solvent includes one or more of methanol, ethanol, formaldehyde, and acetone.
[0023] In some embodiments, the mass ratio of the polyvinyl alcohol to the color-changing agent is 1:(0.5-3).
[0024] In some embodiments, providing a waterproof core layer comprises:
[0025] Mixing base asphalt, oil, rubber powder, filler, functional additive and modifier to obtain asphalt coating material;
[0026] The asphalt coating material is discharged and molded on the tire base layer to form an asphalt coating material layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solution of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0028] Figure 1 This is the surface state of the asphalt waterproofing membrane obtained in Example 1 of the present application after being fired.
[0029] Figure 2 This is the surface state of the asphalt waterproofing membrane obtained in Comparative Example 1 of the present application after being fired. DETAILED DESCRIPTION
[0030] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating examples of the present application. In the accompanying drawings and the following description, at least some of the known structures and technologies are not shown to avoid unnecessary ambiguity in the present application; and, for clarity, the size of some structures may be exaggerated. In addition, the features, structures or characteristics described below may be combined in one or more embodiments in any suitable manner.
[0031] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish an entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In the description of the present application, it should be noted that, unless otherwise specified, the meaning of "multiple" is more than two. Moreover, the term "include", "comprise" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only include those elements, but also include other elements not clearly listed, or also include elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements limited by the sentence "include..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.
[0032] Color-changing asphalt waterproof membrane
[0033] An embodiment of the first aspect of the present application provides a color-changing asphalt waterproofing membrane, comprising a waterproof core layer and a color-changing isolation membrane arranged on at least one side surface of the waterproof core layer; the color-changing isolation membrane comprises a color-changing agent, the color-changing agent comprises a color-changing material that can change color and generate gas at a color-changing temperature, and the color-changing temperature is 180°C to 350°C.
[0034] The waterproof core layer is the main layer of the color-changing asphalt waterproofing membrane, and the color-changing isolation membrane is covered on at least one side of the waterproof core layer. When the asphalt waterproofing membrane is subjected to fire baking construction, the color-changing agent in the isolation membrane reacts with heat, and the color of the color-changing agent changes during the reaction process. Therefore, the progress of the fire baking construction can be controlled according to the color change of the isolation membrane, and the fire baking temperature and time can be grasped in time, reducing the problem of poor construction quality caused by insufficient or excessive fire baking, and improving the convenience and reliability of construction.
[0035] The color-changing isolation membrane will produce gas when it decomposes and changes color due to heat. These gases can expand rapidly and destroy the structure of the color-changing isolation membrane, causing the color-changing isolation membrane to melt and shrink rapidly. The asphalt coating on the surface of the waterproof core layer can be fully exposed, reducing the residual isolation membrane on the surface of the waterproof core layer, which can increase the bonding area of the waterproof membrane and allow the waterproof membrane to be fully bonded to the base layer, thereby reducing the risk of water seepage and improving construction quality and reliability.
[0036] Reference Figure 1 and Figure 2 , Figure 1 The surface state of the asphalt waterproofing membrane with a color-changing agent added to the isolation membrane after being baked is shown. Figure 2The surface state of the asphalt waterproofing membrane without a color-changing agent in the isolation membrane after being baked is shown. It can be seen that the isolation membrane with a color-changing agent is broken and melted and shrunk after being baked, and the waterproof core layer is exposed in a large area. However, the isolation membrane of the asphalt waterproofing membrane without a color-changing agent shrinks after being baked, but the exposed area of the waterproof core layer is small.
[0037] The color-changeable isolation film can be coated on one side surface or both sides surface of the waterproof core layer, preferably on both sides surface.
[0038] The color changing temperature of the color changing agent is 180℃~350℃, and can be selected as 180℃~310℃. The color changing temperature refers to the temperature range in which the color changing agent will undergo physical or chemical changes such as decomposition, vaporization, and secondary reaction. When these physical or chemical changes occur, the color of the color changing agent itself will also change compared to the color at room temperature.
[0039] In some embodiments, the color-changing isolation film may include a color-changing polyvinyl alcohol film. The polyvinyl alcohol has good dispersibility with the color-changing agent and a low melting temperature, and can quickly melt and shrink during heating, thereby further increasing the exposed area of the asphalt coating during the fire-baking construction process and improving the construction reliability of the coiled material.
[0040] In some embodiments, the color-changing agent includes one or more of indigo·TiO2, Cu(OH)2, (NH4)2Cr2O7, and CdCO3.
[0041] Indigo TiO2 is blue at room temperature and will decompose to produce indigo gas and white TiO2 at around 210°C. When it is used as a color-changing agent in a color-changing isolation film, when the color of the isolation film changes from blue to white during the fire-baking construction process, it indicates that the color-changing agent in the isolation film has been completely decomposed, thereby judging the progress of the fire-baking construction during the construction process.
[0042] Indigo TiO2 is often a composite material of indigo and TiO2, which can be prepared by the following methods:
[0043] S10, commercially purchased indigo, indigo and concentrated sulfuric acid (concentration of 98%) are mixed for sulfonation reaction for 30 minutes, the mass ratio of indigo to concentrated sulfuric acid is 1:(0.1-0.5), the sulfonated mixed solution is mixed and diluted with deionized water, and the pH is adjusted to 7-8 with a pH regulator;
[0044] S20, adding nano titanium dioxide to the mixed solution diluted in step S10, soaking and adsorbing for 10 hours to 15 hours, performing ultrasonic dispersion for 10 minutes to 15 minutes every hour, and then filtering, washing and drying to obtain indigo TiO2.
[0045] The pH regulator may be one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, and ammonia water.
[0046] In some embodiments, the mass ratio of indigo to titanium dioxide may be 1:(5-15).
[0047] Cu(OH)2 is blue at room temperature and decomposes into water vapor and black CuO at around 180°C; (NH4)2Cr2O7 is orange-red at room temperature and decomposes into water vapor, nitrogen and green Cr2O3 at around 225°C; CdCO3 is white at room temperature and decomposes into carbon dioxide gas and yellow-brown CdO at around 310°C.
[0048] In some embodiments, the waterproof core layer includes a tread base layer and an asphalt coating layer disposed on the surfaces of both sides of the tread base layer. The asphalt coating layer includes the following raw material compositions in parts by weight: 40 parts of base asphalt, 1 to 10 parts of oil, 6 to 18 parts of rubber powder, and 20 to 40 parts of filler.
[0049] In some embodiments, the base asphalt may include one or more of 70# asphalt, 90# asphalt, and 200# asphalt. The base asphalt is the main component of the asphalt waterproofing membrane, providing the membrane with main waterproof properties.
[0050] In some embodiments, the oil may include one or more of aromatic oil, base oil, naphthenic oil, and reduced oil. The oil may improve the low temperature performance and formability of asphalt, making it easier to form the waterproofing membrane during processing and having better performance in a low temperature environment.
[0051] In some embodiments, the filler may include one or more of talc, heavy calcium, montmorillonite, and kaolin. The filler may provide a better main support effect for the asphalt waterproofing membrane, so that the asphalt waterproofing membrane has good mechanical properties.
[0052] In some embodiments, the rubber powder may include one or more of tire rubber powder, miscellaneous rubber powder, and shoe rubber powder.
[0053] Optionally, the particle size of the rubber powder can be 40 mesh to 80 mesh. The rubber powder can improve the high and low temperature performance of the roll material, so that the asphalt waterproof roll material has good performance in both high and low temperature environments.
[0054] In some embodiments, the raw materials of the asphalt coating layer also include 3 to 8 parts by weight of functional additives, which may include one or more of ferric orthophosphate, aluminum orthophosphate, ferric chloride, sodium silicate, sodium dichromate, sodium hexametaphosphate, and kaolin.
[0055] Functional additives can improve the bonding properties of the asphalt coating layer. During the construction process, after the functional additives in the asphalt coating layer come into contact with the base layer, these functional additives can flocculate, penetrate and crystallize with the cement in the base layer, participate in the hydration reaction of the cement, and then react to form a stable crystalline network, thereby improving the bonding strength between the waterproof membrane and the base layer.
[0056] In some embodiments, the raw materials of the asphalt coating layer also include 2 to 8 parts by weight of a modifier, and the modifier may include one or more of butadiene-styrene-butadiene triblock copolymer (SBS), styrene-butadiene rubber (SBR), hydrogenated styrene-butadiene block copolymer (SEBS), and butadiene-isoprene-butadiene triblock copolymer (SIS).
[0057] Modifiers can improve the cohesive strength and high and low temperature performance of the coating layer, so that the waterproof membrane has better mechanical properties and high and low temperature performance.
[0058] In some embodiments, the coating layer includes the following raw material compositions in parts by weight: 40 parts of base asphalt, 3 to 8 parts of oil, 8 to 15 parts of rubber powder, 26 to 35 parts of filler, 4 to 6 parts of functional additives, and 3 to 6 parts of modifiers.
[0059] In some embodiments, the tire base comprises a polyester tire base pre-impregnated with asphalt, and the weight of the polyester tire base is 180 g / m 2 ~310g / m 2 , optional 200g / m 2 ~260g / m 2 .
[0060] The base layer has good mechanical properties and tensile strength, and can also improve the waterproof effect of the waterproof membrane.
[0061] In some embodiments, the thickness of the color-variable isolation film is 10 μm to 30 μm.
[0062] In some embodiments, the waterproof core layer has a thickness of 2.8 mm to 4 mm.
[0063] Preparation method of asphalt waterproofing membrane
[0064] The second aspect of the present application provides a method for preparing an asphalt waterproofing membrane, comprising the following steps:
[0065] S10, providing a waterproof core layer and a color-changing isolation film;
[0066] S20, a color-changeable isolation film is coated on at least one side of the waterproof core layer to obtain an asphalt waterproof membrane.
[0067] In some embodiments, providing a waterproof core layer in step S10 includes:
[0068] Mixing base asphalt, oil, rubber powder, filler, functional additive and modifier to obtain asphalt coating material;
[0069] The asphalt coating material is discharged and molded on the tire base layer to form an asphalt coating material layer.
[0070] In some embodiments, the asphalt coating layer includes a main asphalt coating layer and a fusible asphalt coating layer. The fusible asphalt coating layer is arranged on the side of the main asphalt coating layer away from the tread base layer. The raw material composition of the fusible asphalt coating layer can be the same as or different from that of the main asphalt coating layer.
[0071] Exemplarily, the preparation method of the main asphalt coating layer and the fusible asphalt coating layer is as follows:
[0072] Forming the main asphalt coating layer:
[0073] (1) Add base asphalt and oil according to the ratio into a reaction vessel, stir for 20 minutes and then add the modifier;
[0074] (2) After the polymer is completely dispersed, add the rubber powder and stir at room temperature for 2 hours;
[0075] (3) Add fillers and functional additives, stir for 1 hour to make them evenly dispersed, and obtain asphalt coating material;
[0076] (4) The asphalt coating is formed on the tire base layer to form a main asphalt coating layer. The thickness of the main asphalt coating layer accounts for 85% to 95% of the total thickness of the asphalt coating layer.
[0077] Forming a fusible coating layer:
[0078] (1) Add the base asphalt according to the ratio into the reaction vessel, stir for 20 minutes, then add the modifier; keep warm and stir for 2 hours;
[0079] (2) adding fillers and functional additives, stirring for 1 hour to make them evenly dispersed, and obtaining an asphalt coating material;
[0080] (3) The asphalt coating material is discharged and molded on the main asphalt coating material layer to form a fusible asphalt coating material layer, and then a waterproof core layer is obtained after cooling.
[0081] The asphalt coating layer includes a main asphalt coating layer and a fusible asphalt coating layer which are stacked. The fusible asphalt coating layer does not contain oil and rubber powder, and is easier to bond to the base layer during the fire-baking construction process, thereby improving the bonding strength of the waterproof membrane.
[0082] In some embodiments, providing a color-variable isolation film includes:
[0083] Polyvinyl alcohol and a color-changing agent are dispersed in a volatile organic solvent to obtain a mixture;
[0084] At least part of the volatile organic solvent in the mixture is removed, and the mixture is dried to form a film to obtain a color-changing isolation film. Thus, the polyvinyl alcohol and the color-changing agent are dispersed in the volatile organic solvent so that the two are evenly dispersed, and the volatile organic solvent is removed by drying, so that the polyvinyl alcohol molecules can be cross-linked to form a film, and the color-changing agent is wrapped in the polyvinyl alcohol film to form a color-changing isolation film.
[0085] The color-changing isolation film is a polyvinyl alcohol film, which is a water-soluble film. During fire-baking construction, it can quickly melt and shrink to expose the asphalt coating layer, which can increase the bonding area between the waterproof membrane and the base layer and improve the waterproof performance.
[0086] In some embodiments, the volatile organic solvent includes one or more of methanol, ethanol, formaldehyde, and acetone.
[0087] In some embodiments, the mass ratio of polyvinyl alcohol to the color-changing agent is 1:(0.5-3), and can be optionally 1:(0.8-2).
[0088] By regulating the mass ratio of polyvinyl alcohol and the color-changing agent within the above range, the obtained color-changing isolation film has good color performance and can obviously reflect the color change during fire baking construction to judge the degree of fire baking. At the same time, the isolation film can maintain high mechanical properties and provide a good isolation coating effect for the asphalt coating layer.
[0089] Example
[0090] The present invention is described below with reference to specific examples. It should be noted that the examples described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this area or the product specifications are used. Unless otherwise specified, the ratios used in the following examples are all mass ratios. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0091] Example 1
[0092] A color-changing asphalt waterproofing coiled material comprises a waterproof core layer and a color-changing isolation membrane covering one side of the waterproof core layer, wherein the waterproof core layer comprises a base layer and an asphalt coating layer located on both sides of the base layer, and the color-changing isolation membrane is covered on the surface of the asphalt coating layer on one side, and is prepared by the following method:
[0093] Preparation of waterproof core layer
[0094] S10, adding 40 parts by weight of 70# asphalt and 12 parts by weight of naphthenic oil into a reactor preheated to 160° C., stirring for 20 minutes to mix evenly;
[0095] S20, add 3 parts by weight of SBS, keep warm and stir until the polymer is fully dispersed and swollen, then add 10 parts by weight of 40-60 mesh tire rubber powder, and keep warm and stir for 2 hours;
[0096] S30, adding 30 parts by weight of filler heavy calcium and 5 parts by weight of functional additive ferric orthophosphate, and stirring for 1 hour to make the dispersion uniform, to obtain the main asphalt coating material;
[0097] S40, the weight of the main asphalt coating material after asphalt pre-impregnation is 240g / m 2 The material is discharged and formed on the polyester base to form the main asphalt coating layer, and the overall thickness is controlled to be 2.8mm;
[0098] S50, continue to take 30 parts by weight of 70# asphalt and 30 parts by weight of 200# asphalt into the reactor preheated to 160°C, stir for 20 minutes, add 3 parts by weight of SBS, keep warm and stir to make the high molecular polymer completely dispersed and swollen; add 30 parts by weight of filler heavy calcium and 5 parts by weight of functional additive ferric orthophosphate, keep warm and stir for 1 hour to make it evenly dispersed, and obtain a fusible asphalt coating material;
[0099] S60, taking the fusible asphalt coating material and discharging and molding it on the surface of the main asphalt coating material layer to form a fusible asphalt coating material layer, controlling the overall thickness to be 3 mm, and obtaining a waterproof core layer after cooling.
[0100] Preparation of color-changing agent indigo·TiO2
[0101] S10, commercially purchased indigo, indigo and concentrated sulfuric acid (concentration 98%) were mixed for sulfonation reaction for 30 min, the mass ratio of indigo to concentrated sulfuric acid was 1:0.2, the sulfonated mixed solution was mixed and diluted with deionized water at a mass ratio of 1:3, and the pH was adjusted to 7-8;
[0102] S20, adding nano titanium dioxide to the mixed solution diluted in step S10, soaking and adsorbing for 12 hours, performing ultrasonic dispersion for 10 minutes every hour, and then filtering, washing, and drying to obtain indigo·TiO2. The mass ratio of indigo to titanium dioxide is 1:8.
[0103] Preparation of color-changing isolation film
[0104] Polyvinyl alcohol (17-88 type), color-changing agent indigo·TiO2 and ethanol are mixed evenly in a mass ratio of 1:1:5, and the mixture is dried to form a film to obtain a color-changing isolation film. The thickness of the color-changing isolation film is 50 μm;
[0105] Preparation of color-changing asphalt waterproofing membrane:
[0106] The prepared color-changeable isolation film is covered on one side surface of the waterproof core layer to obtain a color-changeable asphalt waterproof roll material.
[0107] Embodiments 2 to 11
[0108] The preparation method of the color-changing asphalt waterproofing membrane is consistent with that of Example 1, except that the raw material ratio of the color-changing isolation membrane is different, as shown in Table 1:
[0109] The raw material ratio of the fusible asphalt coating layer is consistent with that in Example 1 and is not listed separately in Table 1.
[0110] Example 12
[0111] The preparation method of the color-changing asphalt waterproofing membrane is the same as that of Example 1, except that the waterproof core layer is not provided with a fusible asphalt coating layer.
[0112] Comparative Examples 1-2
[0113] The preparation method of the color-changing asphalt waterproofing membrane is consistent with that in the embodiment, except that no color-changing agent is added to the isolation membrane. The other raw materials are detailed in Table 1.
[0114] Comparative Example 3
[0115] The preparation method of the color-changing asphalt waterproofing membrane is consistent with that in the embodiment, except that a PE film with a thickness of 30 μm is used as the isolation membrane, and the other raw materials are detailed in Table 1.
[0116]
[0117] Test Section
[0118] 1) Color change test
[0119] The prepared waterproof membrane was subjected to a fire test using a gas spray gun, and the color change of the isolation membrane before and after fire heating was observed.
[0120] 2) Peel strength with cement
[0121] On a cement block with a size of 50cm (length) × 30cm (width) × 5cm (thickness), apply a layer of cement slurry (the weight ratio of cement to water is 1:0.42), lay the asphalt waterproof membrane on the cement slurry, and compact it with a 2kg roller. Referring to GB / T 35467-2017 "Wet-laid waterproof membrane", the peeling strength between the membrane and concrete is maintained and tested, and the average peeling strength is taken.
[0122] 3) Seam peel strength
[0123] The asphalt waterproofing membrane is overlapped by means of fire baking, and the flame gun is used for the fire baking. The fire baking time is determined according to the discoloration of the isolation membrane. The overlap is performed after the isolation membrane is completely discolored and shrunk (Comparative Examples 1 to 3 are overlapped after the isolation membrane is shrunk). The seam peeling strength of the asphalt waterproofing membrane is tested with reference to the standard GB 18242-2008 "Elastomer SBS modified asphalt waterproofing membrane".
[0124] The performance test results are detailed in Table 2.
[0125] Table 2:
[0126]
[0127]
[0128] Combined with the data in Table 2, the color-changing isolation film provided in the embodiment of the present application has obvious color changes before and after baking, so that the temperature and time of the baking construction can be timely grasped, thereby improving the convenience and reliability of the construction.
[0129] From the data of the peel strength of the asphalt waterproofing membrane in Table 2, it can be seen that the asphalt waterproofing membrane in the embodiment of the present application has a higher bonding strength with the base layer, which indicates that the shrinkage of the color-changing isolation membrane after the fire baking construction is better, and the main coating layer of the waterproofing membrane is more tightly bonded to the base layer. In addition, the asphalt waterproofing membrane in the embodiment of the present application has a higher seam peel strength than the asphalt waterproofing membrane in the comparative example, which indicates that the asphalt waterproofing membrane in the embodiment of the present application has a better bonding effect at the seam, which can further reduce the hidden danger of water leakage after construction and improve construction reliability.
[0130] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A color-changing asphalt waterproofing membrane, characterized in that: It comprises a waterproof core layer and a color-changing isolation film located on at least one surface of the waterproof core layer; The color-changing isolation film includes a color-changing agent, and the color-changing agent includes a color-changing material that can change color and generate gas at a color-changing temperature, and the color-changing temperature is 180° C. to 350° C.; The color-changing isolation film is a color-changing polyvinyl alcohol film, and the mass ratio of polyvinyl alcohol to the color-changing agent is 1: (0.5-3).
2. The color-changing asphalt waterproofing membrane according to claim 1 is characterized in that: The color-changing agent includes one or more of indigo·TiO2, Cu(OH)2, (NH4)2Cr2O7, and CdCO3.
3. The color-changing asphalt waterproofing membrane according to claim 1 or 2, characterized in that: The waterproof core layer includes a tread base layer and an asphalt coating layer provided on both sides of the tread base layer. The asphalt coating layer includes the following raw material compositions in parts by weight: 40 parts of base asphalt; 1-10 parts oil; 6-18 parts of rubber powder; 20 to 40 parts of filler.
4. The color-changing asphalt waterproofing membrane according to claim 3 is characterized in that: The matrix asphalt includes one or more of 70# asphalt, 90# asphalt, and 200# asphalt; and / or The oil comprises one or more of aromatic oil, base oil, naphthenic oil and reduced line oil; and / or The filler comprises one or more of talc, heavy calcium, montmorillonite and kaolin; and / or The rubber powder includes one or more of tire rubber powder, miscellaneous rubber powder and shoe rubber powder.
5. The color-changing asphalt waterproofing membrane according to claim 3 is characterized in that: The raw materials of the asphalt coating layer also include 3 to 8 parts by weight of functional additives, and the functional additives include one or more of ferric orthophosphate, aluminum orthophosphate, ferric chloride, sodium silicate, sodium dichromate, sodium hexametaphosphate, and kaolin.
6. The color-changing asphalt waterproofing membrane according to claim 3 is characterized in that: The raw materials of the asphalt coating layer also include 2 to 8 parts by weight of a modifier, and the modifier includes one or more of butadiene-styrene-butadiene triblock copolymer, styrene-butadiene rubber, hydrogenated styrene-butadiene block copolymer, and butadiene-isoprene-butadiene triblock copolymer.
7. The color-changing asphalt waterproofing membrane according to claim 1, characterized in that: The thickness of the color-changing isolation film is 10 μm to 30 μm; and / or The thickness of the waterproof core layer is 2.8 mm to 4 mm.
8. The method for preparing the color-changing asphalt waterproofing membrane according to any one of claims 1 to 7, characterized in that: The steps include: Provide waterproof core layer and color-changing isolation film respectively; The color-changeable isolation film is coated on at least one side of the waterproof core layer to obtain the asphalt waterproofing membrane.
9. The method for preparing the color-changing asphalt waterproofing membrane according to claim 8, characterized in that: The provision of a color-variable isolation film comprises: Polyvinyl alcohol and a color-changing agent are dispersed in a volatile organic solvent to obtain a mixture; At least part of the volatile organic solvent in the mixture is removed, and the mixture is dried to form a film to obtain a color-changeable isolation film; wherein, The volatile organic solvent includes one or more of methanol, ethanol, formaldehyde and acetone; and / or The mass ratio of the polyvinyl alcohol to the color-changing agent is 1:(0.5-3).
10. The method for preparing the color-changing asphalt waterproofing membrane according to claim 8, characterized in that: The provision of a waterproof core layer comprises: Mixing base asphalt, oil, rubber powder, filler, functional additive and modifier to obtain asphalt coating material; The asphalt coating material is discharged and molded on the tire base layer to form an asphalt coating material layer.