A polypropylene-based conductive composite material and a preparation method thereof
The preparation of modified graphene and polypropylene pressurization method is solved, and the flame retardant performance and mechanical properties of polypropylene-based conductive composite materials are improved, thus achieving the improvement of conductivity, electromagnetic shielding performance and flame retardant performance, forming a Composite material with excellent comprehensive properties.
Patent Information
- Application Number
- CN202410474756.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-19
AI Technical Summary
The flame retardant properties of existing polypropylene-based conductive composite materials are insufficient, and the processing method leads to poor bonding force between the polymer matrix and the conductive filler, resulting in poor mechanical properties, especially toughness.
Modified graphene and polypropylene are fully mixed, and temperature and pressure are controlled by the pressurization method to prepare a conductive composite material with modified graphene. Modified graphene is treated with ultrasonic dispersion and chemical modification to increase the surface long-chain season. The ammonium salt molecular chain and bisphosphite groups enhance their interface binding force and flame retardant properties with the polypropylene matrix.
It significantly improves the flame retardant properties and mechanical properties of composite materials, forms a clear and uniform thickness isolation conductive network, improves the conductivity and electromagnetic shielding performance, and achieves excellent results at a boost temperature of 165-175℃ and a pressure of 200MPa. Comprehensive performance.
Smart Images

Figure CN118222040B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive materials, and in particular relates to a polypropylene-based conductive composite material and a preparation method thereof. Background Art
[0002] Conductive polymer composite materials are made by adding conductive fillers such as carbon and metal particles to a polymer matrix to give the polymer material conductive properties. Polypropylene, a polymer matrix, is a cost-effective general-purpose plastic with the advantages of being non-toxic, odorless, low density, good hygroscopicity resistance, good corrosion resistance, and good solubility resistance. It is widely used in automotive products, medical and health care, and food. In order to improve the conductive properties of polypropylene, conductive fillers such as metal powders and carbon (carbon fiber, carbon nanotubes, graphene) are mainly added. These conductive fillers can be distributed between the interfaces of the polymer matrix polypropylene particles and establish a penetrating conductive network between the polypropylene particles, thereby achieving high conductivity and electromagnetic shielding performance at low filler loading, forming a polypropylene-based conductive polymer composite material with an isolation structure.
[0003] The patent with application number 202211195034.1 discloses a conductive polypropylene composite material and a preparation method thereof, which uses copolymer polypropylene resin as a polymer matrix, and adds antistatic masterbatch, TPX masterbatch and granulated additives. The antistatic masterbatch contains at least one of carbon nanotubes and carbon fibers. The TPX masterbatch is made of graphene, white carbon black, and TPX. It is extruded by a twin-screw extruder to obtain a conductive polypropylene composite material with extremely low volume resistivity and excellent mechanical properties; the patent with application number 202311778866.0 discloses a conductive polypropylene composite material and a preparation method thereof, which uses polypropylene as a polymer matrix, and adds modified nanocellulose fibers to improve the conductive properties of the material, wherein the modified nanocellulose fibers are formed by surface modification of nanocellulose fibers by carbon nanotubes under the synergistic action of coupling agents and cross-linking agents, so that the carbon nanotubes are evenly distributed. On the surface of nanocellulose fibers, it has a better interfacial conductive effect, achieving excellent conductive function under the condition of a small amount of carbon nanotubes added. The patent also uses a twin-screw extruder to extrude and mold to produce a conductive polypropylene composite material with excellent mechanical properties; the polypropylene polymer matrix used in the above patent has poor flame retardancy, a low limiting oxygen index, and is easy to drip when burning, resulting in the flame retardancy of the polypropylene-based conductive composite material not meeting the application requirements, and when preparing the composite material, processing conditions such as temperature and pressure have a great influence on the structure and comprehensive performance of the conductive composite material, and the conductive composite material prepared by the conventional extrusion molding method has a poor bonding force between the polymer matrix and the conductive filler, resulting in poor mechanical properties, especially toughness. Therefore, it is necessary to study the processing method of the conductive composite material to obtain a conductive composite material with better comprehensive performance. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a polypropylene-based conductive composite material and a preparation method thereof to solve the problems in the prior art.
[0005] The technical solution adopted by the present invention to solve the above problems is:
[0006] A method for preparing a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating the mixture to 165-175° C., maintaining the temperature for 10 min to melt the mixture, pressurizing the mixture to 200 MPa, and then cooling the mixture at a rate of 15° C. / min to obtain a conductive composite material;
[0007] Furthermore, the content of the modified graphene is 2.0-2.5wt%; and the particle size of the polypropylene is ≤125μm.
[0008] The preparation method of the modified graphene is:
[0009] S1. Add graphene to deionized water, disperse it evenly by ultrasonication, add concentrated sulfuric acid dropwise, react at 50-60°C for 2-3h, filter after the reaction is completed, wash with deionized water until the filtrate is neutral, and dry the filter residue to obtain pretreated graphene;
[0010] S2, add the pretreated graphene to the organic solvent-deionized water system, ultrasonically disperse it uniformly, add modified-aminopropyltrimethoxysilane, react at 60-70° C. for 3-4 hours, filter after the reaction is completed, wash with deionized water, and dry the filter residue to obtain modified graphene; the chemical structural formula of the modified-aminopropyltrimethoxysilane is:
[0011]
[0012] Furthermore, in step S1, the mass ratio of graphene to concentrated sulfuric acid is 1:2-4.
[0013] Furthermore, the mass ratio of the pretreated graphene and modified-aminopropyltrimethoxysilane in step S2 is 1:0.3-0.5; the organic solvent in the organic solvent-deionized water system is one of methanol, ethanol, ethylene glycol or acetone; the mass ratio of the organic solvent and deionized water is 5-10:1.
[0014] Furthermore, the preparation method of the modified aminopropyltrimethoxysilane in step S2 is:
[0015] (1) adding ethanol, γ-aminobutyric acid, 4-chloro-1-butanol and triethylamine to a reaction vessel in sequence, and refluxing for 4-5 hours at 78-80° C. to obtain aminobutyric acid-alcohol; the molar ratio of the γ-aminobutyric acid, 4-chloro-1-butanol and triethylamine is 1:2.1-2.2:1.5-2.0;
[0016] (2) adding anhydrous tetrahydrofuran, aminobutyric acid-alcohol and triethylamine to a reaction vessel, and adding diethylphosphite chloride dropwise at 0-5° C., and reacting for 2-3 hours at this temperature to obtain aminobutyric acid-phosphite; the molar ratio of aminobutyric acid-alcohol, diethylphosphite chloride and triethylamine is 1:2.0-2.1:1.3-1.5;
[0017] (3) adding ethanol, aminobutyric acid-phosphite and 1-chlorododecane to a reaction vessel in sequence, and reflux reacting at 78-80° C. for 12-14 hours to obtain aminobutyric acid-quaternary ammonium salt; the molar ratio of the aminobutyric acid-phosphite to 1-chlorododecane is 1:1.0-1.1;
[0018] (4) adding anhydrous tetrahydrofuran, aminobutyric acid-quaternary ammonium salt and triphosgene into a reaction vessel in sequence, and adding pyridine dropwise at 0-5° C., reacting at room temperature for 6-8 hours to obtain acyl chloride-quaternary ammonium salt; the molar ratio of aminobutyric acid-quaternary ammonium salt, triphosgene and pyridine is 1:1.0-1.1:1.3-1.5;
[0019] (5) Anhydrous dichloromethane, 3-aminopropyltrimethoxysilane and acyl chloride-quaternary ammonium salt are added to the reaction container in sequence, and reacted at room temperature for 2-4 hours to obtain modified-aminopropyltrimethoxysilane; the molar ratio of the 3-aminopropyltrimethoxysilane to the acyl chloride-quaternary ammonium salt is 1:1.0-1.1.
[0020] The present invention also provides a polypropylene-based conductive composite material, which is prepared by the above-mentioned method for preparing the polypropylene-based conductive composite material.
[0021] The present invention has the following beneficial effects:
[0022] In order to enhance the flame retardant property of the composite material, the present invention adopts modified-aminopropyltrimethoxysilane to modify graphene, and obtains the modified graphene with long-chain quaternary ammonium salt molecular chains and bisphosphite groups on the surface. The interface bonding force between the modified graphene and an organic polypropylene matrix is better, and the bonding between the two is tighter, which is helpful to improve the comprehensive performance of the composite material; wherein the long-chain quaternary ammonium salt molecular chains give the modified graphene good dispersibility, can prevent the modified graphene from agglomerating in the polypropylene matrix, and is helpful to form a composite material with uniform structure; the bisphosphite groups give the modified graphene excellent flame retardant property, thereby greatly improving the flame retardant property of the composite material.
[0023] The present invention controls the boost temperature to be 165-175° C. and the boost pressure to be 200 MPa, which is beneficial to maintaining the integrity and uniformity of the conductive network structure and forming a composite material of a conductive network with a clear isolation structure and uniform thickness; compared with a conventional extrusion molding processing method, when the boost pressure is 200 MPa, structural defects such as voids and loose overlaps caused by random distribution of conductive fillers inside the polymer can be reduced, so that the interface bonding force between the modified graphene and the polypropylene matrix is tighter, which is beneficial to improving the connectivity of the conductive network, and enhancing the conductivity and electromagnetic shielding performance of the composite material. At the same time, the crystal structure of the polypropylene matrix is transformed into a pure γ crystal with better mechanical properties, thereby obtaining a composite material with better mechanical properties.
[0024] The present invention uses polypropylene and modified graphene as raw materials, adopts a supercharging method, and obtains a polypropylene / modified graphene conductive composite material by controlling the supercharging temperature and the supercharging pressure; the prepared composite material has good conductivity, electromagnetic shielding performance and mechanical properties, especially excellent flame retardant performance, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Polarized optical microscope (POM) images of composite materials prepared at different pressurization temperatures;
[0026] Figure 2 Polarized optical microscope (POM) images of the composite materials prepared under different boost pressures;
[0027] Figure 3 The electromagnetic shielding effect (EMI SE) and conductivity diagram of the composite materials prepared under different boost pressures in the K band (18-26.5GHz);
[0028] Figure 4 (a) Engineering stress-strain curve and (b) one-dimensional WAXD curve of the composite materials prepared under different boost pressures. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0030] In the technical scheme of the present invention, the raw materials and reagents used in the following embodiments and comparative examples are all common commercially available products, wherein the model of polypropylene is T30S, purchased from Xinjiang Dushanzi Petrochemical Co., Ltd., with a relative molecular mass of 399 kg / mol and a melt flow rate of 3.0 g / 10 min; the model of graphene is XT-C4-07, purchased from Shanghai Xiangtian Nanomaterial Co., Ltd.; the present invention adopts a universal grinder to fully grind the purchased polypropylene to obtain polypropylene raw materials with different particle sizes (125 μm, 100 μm, 90 μm).
[0031] In the technical solution of the present invention, the preparation method of the modified aminopropyltrimethoxysilane used is:
[0032] (1) 500 mL of ethanol, 10.3 g of γ-aminobutyric acid, 22.8 g of 4-chloro-1-butanol and 15.2 g of triethylamine were added to a reaction vessel in sequence, and refluxed at 78-80° C. for 5 h. After the reaction was completed, ethanol and unreacted 4-chloro-1-butanol were removed, and then extracted with 500 mL of water and 500 mL of dichloromethane. The organic phase was concentrated under reduced pressure to obtain 20.5 g of aminobutyric acid-alcohol; the molar ratio of γ-aminobutyric acid, 4-chloro-1-butanol and triethylamine was 1:2.1:1.5; the reaction process was:
[0033]
[0034] Aminobutyric acid-alcohol: ESI (m / z): 248.3 [M+H]+, 1H-NMR (600 MHz, DMSO-d6, δ ppm): 12.01 (s, 1H), 4.14 (s, 2H), 3.46-3.49 (m, 4H), 3.01-3.03 (m, 4H), 2.38-2.41 (m, 4H), 1.59-1.62 (m, 6H), 1.36-1.38 (m, 4H).
[0035] (2) Add 400 mL of anhydrous tetrahydrofuran, 20.0 g of aminobutyric acid-alcohol and 10.6 g of triethylamine to a reaction vessel, add 26.6 g of diethylphosphite chloride dropwise at 0° C., and keep warm for 3 h. After the reaction is completed, remove the tetrahydrofuran, extract with 400 mL of water and 400 mL of dichloromethane, and concentrate the organic phase under reduced pressure to obtain 34.6 g of aminobutyric acid-phosphite; the molar ratio of aminobutyric acid-alcohol, diethylphosphite chloride and triethylamine is 1:2.1:1.3; the reaction process is:
[0036]
[0037] GABA-phosphite: ESI (m / z): 488.5 [M+H] + , 1H-NMR (600MHz, DMSO-d6, δppm): 12.03 (s, 1H), 3.81-3.85 (m, 12H), 3.02-3.04 (m, 4H), 2.35 -2.40(m, 4H), 1.76-1.79(m, 2H), 1.52-1.54(m, 4H), 1.36-1.38(m, 4H), 1.25-1.28(m, 12H).
[0038] (3) 300 mL of ethanol, 30.0 g of aminobutyric acid-phosphite and 12.6 g of 1-chlorododecane were added to the reaction vessel in sequence, and the mixture was refluxed at 78-80° C. for 14 h. After the reaction was completed, the ethanol was removed, and 300 mL of water and 300 mL of dichloromethane were used for extraction. The aqueous phase was concentrated under reduced pressure to obtain 35.4 g of aminobutyric acid-quaternary ammonium salt; the molar ratio of aminobutyric acid-phosphite to 1-chlorododecane was 1:1.0; the reaction process was as follows:
[0039]
[0040] Aminobutyric acid-quaternary ammonium salt: ESI (m / z): 693.2 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 12.01 (s, 1H), 3.82-3.85 (m, 12H), 3.23-3.28 (m, 10H), 2.00 -2.03 (m, 2H), 1.71-1.74 (m, 6H), 1.51-1.54 (m, 4H), 1.25-1.30 (m, 30H), 0.88-0.90 (m, 3H).
[0041] (4) 200 mL of anhydrous tetrahydrofuran, 25.0 g of aminobutyric acid-quaternary ammonium salt and 10.7 g of triphosgene were added to the reaction vessel in sequence, and 4.3 g of pyridine was added dropwise at 0°C. After the addition was completed, the reaction was carried out at room temperature for 8 hours. After the reaction was completed, the filtrate was filtered and concentrated under reduced pressure to obtain 21.8 g of acyl chloride-quaternary ammonium salt; the molar ratio of aminobutyric acid-quaternary ammonium salt, triphosgene and pyridine was 1:1.0:1.5; the reaction process was:
[0042]
[0043] Acyl chloride-quaternary ammonium salt: ESI (m / z): 711.7 [M+H] + , 1H-NMR (600MHz, DMSO-d6, δppm): 3.80-3.85 (m, 12H), 3.22-3.26 (m, 8H), 2.82-2.84 (m, 2H), 2. 02-2.05(m, 2H), 1.71-1.74(m, 6H), 1.52-1.54(m, 4H), 1.25-1.30(m, 30H), 0.88-0.90(m, 3H).
[0044] (5) 150 mL of anhydrous dichloromethane, 5.0 g of 3-aminopropyltrimethoxysilane and 19.8 g of acyl chloride-quaternary ammonium salt were added to the reaction vessel in sequence, and the reaction was carried out at room temperature for 2-4 h. After the reaction was completed, the dichloromethane was removed to obtain 20.8 g of modified-aminopropyltrimethoxysilane; the molar ratio of 3-aminopropyltrimethoxysilane to acyl chloride-quaternary ammonium salt was 1:1.0; the reaction process was:
[0045]
[0046] Modified-aminopropyltrimethoxysilane: ESI (m / z): 854.5 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 7.70 (s, 1H), 3.81-3.85 (m, 12H), 3.43-3.50 (m, 11H), 3.22-3.26 (m, 8H), 2.34-2.36 (m, 2H), 2.01-2.03(m, 2H), 1.75-1.79(m, 6H), 1.48-1.51(m, 6H), 1.25-1.30(m, 30H), 0.88-0.90(m, 3H), 0.56-0.58(m, 2H).
[0047] Example 1
[0048] A method for preparing a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 175°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0049] The preparation method of modified graphene is:
[0050] S1. Add graphene to deionized water, disperse it evenly by ultrasonication, add concentrated sulfuric acid dropwise, react at 60°C for 3h, filter after the reaction is completed, and wash the filtrate with deionized water until the filtrate is neutral, and dry the filter residue to obtain pretreated graphene; the mass ratio of graphene to concentrated sulfuric acid is 1:4; the content of graphene in deionized water is 25wt%;
[0051] S2. Add pretreated graphene to a methanol-deionized water system, disperse it evenly by ultrasonication, add modified-aminopropyltrimethoxysilane, react for 3 hours at 70°C, filter after the reaction is completed, wash with deionized water, and dry the filter residue to obtain modified graphene; the mass ratio of pretreated graphene to modified-aminopropyltrimethoxysilane is 1:0.5; the mass ratio of methanol to deionized water is 10:1; the content of pretreated graphene in the methanol-deionized water system is 25wt%.
[0052] Example 2
[0053] A method for preparing a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 165°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0054] The preparation method of modified graphene is:
[0055] S1. Add graphene to deionized water, disperse it evenly by ultrasonication, add concentrated sulfuric acid dropwise, react at 50°C for 2.5h, filter after the reaction, wash with deionized water until the filtrate is neutral, and dry the residue to obtain pretreated graphene; the mass ratio of graphene to concentrated sulfuric acid is 1:3; the content of graphene in deionized water is 25wt%;
[0056] S2. Add pretreated graphene to the ethylene glycol-deionized water system, disperse it evenly by ultrasonication, add modified-aminopropyltrimethoxysilane, react at 65°C for 4 hours, filter after the reaction is completed, wash with deionized water, and dry the filter residue to obtain modified graphene; the mass ratio of pretreated graphene to modified-aminopropyltrimethoxysilane is 1:0.4; the mass ratio of ethylene glycol to deionized water is 5:1; the content of pretreated graphene in the ethylene glycol-deionized water system is 25wt%.
[0057] Example 3
[0058] A method for preparing a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 170°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.3wt%, and the particle size of the polypropylene is 100μm.
[0059] The preparation method of modified graphene is:
[0060] S1. Add graphene to deionized water, disperse it evenly by ultrasonication, add concentrated sulfuric acid dropwise, react at 55°C for 2h, filter after the reaction is completed, and wash the filtrate with deionized water until the filtrate is neutral, and dry the filter residue to obtain pretreated graphene; the mass ratio of graphene to concentrated sulfuric acid is 1:2; the content of graphene in deionized water is 25wt%;
[0061] S2. Add pretreated graphene to an acetone-deionized water system, disperse it evenly by ultrasonication, add modified-aminopropyltrimethoxysilane, react for 3.5 hours at 60°C, filter after the reaction is completed, wash with deionized water, and dry the filter residue to obtain modified graphene; the mass ratio of pretreated graphene to modified-aminopropyltrimethoxysilane is 1:0.3; the mass ratio of acetone to deionized water is 8:1; the content of pretreated graphene in the acetone-deionized water system is 25wt%.
[0062] Example 4
[0063] A preparation method of a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 165°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.0wt%, and the particle size of the polypropylene is 90μm.
[0064] The preparation method of modified graphene is:
[0065] S1. Add graphene to deionized water, disperse it evenly by ultrasonication, add concentrated sulfuric acid dropwise, react at 60°C for 2h, filter after the reaction is completed, and wash the filtrate with deionized water until the filtrate is neutral, and dry the filter residue to obtain pretreated graphene; the mass ratio of graphene to concentrated sulfuric acid is 1:3; the content of graphene in deionized water is 25wt%;
[0066] S2. Add pretreated graphene to an ethanol-deionized water system, disperse it evenly by ultrasonication, add modified-aminopropyltrimethoxysilane, react for 3.5 hours at 70°C, filter after the reaction is completed, wash with deionized water, and dry the filter residue to obtain modified graphene; the mass ratio of pretreated graphene to modified-aminopropyltrimethoxysilane is 1:0.4; the mass ratio of ethanol to deionized water is 10:1; the content of pretreated graphene in the ethanol-deionized water system is 25wt%.
[0067] Comparative Example 1
[0068] A method for preparing a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 175°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0069] The preparation method of modified graphene is:
[0070] S1, the same as step S1 in Example 1;
[0071] S2. Add pretreated graphene to a methanol-deionized water system, disperse it evenly by ultrasonication, add 3-aminopropyltrimethoxysilane, react at 70°C for 3 hours, filter after the reaction is completed, wash with deionized water, and dry the filter residue to obtain modified graphene; the mass ratio of pretreated graphene to 3-aminopropyltrimethoxysilane is 1:0.5; the mass ratio of methanol to deionized water is 10:1; the content of pretreated graphene in the methanol-deionized water system is 25wt%.
[0072] Comparative Example 2
[0073] A preparation method of a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 175°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of graphene is 2.5wt%, and the particle size of polypropylene is 125μm.
[0074] Comparative Example 3
[0075] A preparation method of a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 185°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0076] The preparation method of modified graphene is the same as that in Example 1.
[0077] Comparative Example 4
[0078] A preparation method of a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 195°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 200MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0079] The preparation method of modified graphene is the same as that in Example 1.
[0080] Comparative Example 5
[0081] A preparation method of a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 175°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 150MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0082] The preparation method of modified graphene is the same as that in Example 1.
[0083] Comparative Example 6
[0084] A method for preparing a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 175°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 100MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0085] The preparation method of modified graphene is the same as that in Example 1.
[0086] Comparative Example 7
[0087] A preparation method of a polypropylene-based conductive composite material comprises the following steps: fully and uniformly mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating it to 175°C, maintaining it for 10 minutes to melt the mixture, pressurizing it to 50MPa, and then cooling it at a rate of 15°C / min to obtain a conductive composite material; the content of the modified graphene is 2.5wt%, and the particle size of the polypropylene is 125μm.
[0088] The preparation method of modified graphene is the same as that in Example 1.
[0089] Related tests
[0090] The composite materials of Examples 1-2 and Comparative Examples 3-7 were analyzed by polarizing microscope (POM) with a sample thickness of 14 μm. The results are as follows: Figure 1 , Figure 2 As shown in the figure, the black area represents modified graphene, and the gray area is the polypropylene matrix; the electromagnetic shielding effect of the composite material was tested using the Malaysian N522B material dielectric performance test system, and the conductivity of the composite material was tested using the RTS-8 four-probe tester. The results are shown in Table 1. Figure 3 As shown; the mechanical properties of the composite material were tested using an AG-Xplus high and low temperature universal material testing machine, with a tensile speed of 100 μm / min. The results are shown in Table 1. Figure 4 (a) As shown; the crystal structure of the composite material was analyzed using a wide-angle X-ray diffractometer, the X-ray light source was a Cu target, the wavelength was 0.154nm, the working standard voltage was 50kA, the working current was 1000μA, and the results were as follows Figure 4 (b) as shown.
[0091] Table 1 Performance test results of composite materials
[0092]
[0093] As shown in Table 1, the composite materials of Examples 1-4 have higher EMI SE values, electrical conductivity, yield strength and elongation at break, indicating that the polypropylene / modified graphene composite material prepared by the present invention has good electrical conductivity, electromagnetic shielding performance and mechanical properties, especially excellent flame retardant performance when the supercharging temperature is 165-175°C and the supercharging pressure is 200MPa; compared with Comparative Examples 1-2, the surface of the modified graphene used in Example 1 contains long-chain quaternary ammonium salt molecular chains and bisphosphite groups, and has better interfacial bonding with the organic polypropylene matrix, and the combination between the two is more compact, which helps to improve the comprehensive performance of the composite material; wherein the long-chain quaternary ammonium salt molecular chains give the modified graphene good dispersibility, can prevent it from agglomerating in the polypropylene matrix, and help to form a composite material with uniform structure; the bisphosphite groups give the modified graphene excellent flame retardant properties, thereby greatly improving the flame retardant properties of the composite material.
[0094] Depend on Figure 1 The results show that when the supercharging temperature is 175°C (Example 1) and 165°C (Example 2), the prepared composite material has a clear conductive network of the isolation structure and uniform thickness, and the conductive path is relatively complete; when the supercharging temperature is 185°C (Comparative Example 3) and 195°C (Comparative Example 4), the formed conductive network of the isolation structure is thicker and uneven, because the viscosity of polypropylene decreases at a higher supercharging temperature, and the modified graphene is more easily diffused into the polypropylene matrix, resulting in obvious agglomeration. The present invention controls the supercharging temperature within the range of 165-175°C, which is beneficial to maintaining the integrity and uniformity of the conductive network structure.
[0095] Depend on Figure 2 The results show that the conductive network of the isolation structure formed when the boost pressure is 50 MPa (Comparative Example 7) is thicker and more uneven. At a lower boost pressure, the viscosity of polypropylene is smaller, and the modified graphene is more easily diffused in the polypropylene matrix, and obvious agglomeration occurs; with the increase of the boost pressure (100 MPa, Comparative Example 6; 150 MPa, Comparative Example 5), the agglomeration of the modified graphene weakens, and the network in the isolation structure becomes more uniform; when the boost pressure is 200 MPa (Example 1), the prepared conductive network of the isolation structure is clear and has uniform thickness. The present invention is beneficial to maintaining the integrity and uniformity of the conductive network structure by controlling the boost pressure to 200 MPa.
[0096] Depend on Figure 3The results show that the EMI SE value of the composite material increases slowly with the increase of the boost pressure. When the boost pressure is 50MPa (Comparative Example 7) and 100MPa (Comparative Example 6), the EMI SE value of the composite material is lower than 10.0dB; when the boost pressure is 150MPa (Comparative Example 5), the EMI SE value of the composite material is 10.0dB; when the boost pressure reaches 200MPa (Example 1), the EMI SE of the composite material increases to a maximum value of 20.5dB (reaching the commercial standard). At the same time, the conductivity of the composite material reaches the highest value (20.0S / m); this shows that high pressure can reduce structural defects such as agglomeration, voids and loose overlap caused by the random distribution of conductive fillers inside the polymer, which is beneficial to improving the connectivity of the conductive network; in order to clarify the shielding mechanism of the composite material, according to the calculation of the microwave absorption (SEA) and microwave reflection (SER) parts of the total EMI shielding effectiveness (SET) in the K band, it is obvious that the electromagnetic shielding effect of the composite material is mainly based on absorption.
[0097] Depend on Figure 4 (a) The results show that when the boost pressure is 50 MPa (Comparative Example 7) and 100 MPa (Comparative Example 6), the composite material undergoes brittle fracture during the stretching process, and the elongation at break is very low. After the boost pressure is increased to 150 MPa (Comparative Example 5), the composite material undergoes a brittle-toughness transition. When the boost pressure is increased to 200 MPa (Example 1), the toughness of the composite material is further improved, and the elongation at break reaches a maximum value (115%); at a pressure of 200 MPa, the interfacial bonding force between the polypropylene particles can be made tighter, the adhesion between the modified graphene and the polypropylene matrix is enhanced, a continuous phase isolation structure conductive network is formed, and the deformation resistance of the composite material is improved; Figure 4 (b) The results show that when the boost pressure is 50 MPa (Comparative Example 7), the polypropylene in the composite material crystallizes to form α crystals; when the pressure is increased to 100 MPa (Comparative Example 6), a small amount of γ crystals begin to appear; when the pressure is further increased to 150 MPa (Comparative Example 5), most of the polypropylene forms γ crystals, but a small amount of α crystals still exist; when the pressure is increased to 200 MPa (Example 1), the polypropylene forms pure γ crystals; It can be seen from literature reports that α-polypropylene has a cross-mother-daughter crystal structure, so the toughness is poor, while the molecular chains in the γ-polypropylene lamellae are cross-linked with each other, and the toughness is better. The mechanical properties of γ-polypropylene are better than those of α-polypropylene.
[0098] comprehensive Figure 3 , Figure 4 Compared with comparative examples 5-7, in Example 1, when the supercharging temperature is 175°C, the present invention controls the supercharging pressure to 200MPa, thereby preparing a composite material with good mechanical properties, electrical conductivity and electromagnetic shielding properties.
[0099] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements inherent to such process, method, article or device; although the embodiments of the present application have been shown and described, it can be understood by those of ordinary skill in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a polypropylene-based conductive composite material, characterized in that: The method comprises the following steps: fully mixing polypropylene and modified graphene to obtain a mixture; placing the mixture in an aluminum box, heating the mixture to 165-175°C, maintaining the temperature for 10 minutes to melt the mixture, pressurizing the mixture to 200 MPa, and then cooling the mixture at a rate of 15°C / min to obtain a conductive composite material; The preparation method of the modified graphene is: S1. Add graphene to deionized water, disperse it evenly by ultrasonication, add concentrated sulfuric acid dropwise, react at 50-60°C for 2-3h, filter after the reaction is completed, wash with deionized water until the filtrate is neutral, and dry the filter residue to obtain pretreated graphene; S2, adding the pretreated graphene to the organic solvent-deionized water system, ultrasonically dispersing it uniformly, adding modified-aminopropyltrimethoxysilane, reacting at 60-70° C. for 3-4 hours, filtering after the reaction is completed, washing with deionized water, and drying the filter residue to obtain modified graphene; The chemical structural formula of the modified aminopropyltrimethoxysilane is:
2. The method for preparing a polypropylene-based conductive composite material according to claim 1, characterized in that: The content of the modified graphene is 2.0-2.5wt%; and the particle size of the polypropylene is ≤125μm.
3. The method for preparing a polypropylene-based conductive composite material according to claim 1, characterized in that: The mass ratio of graphene to concentrated sulfuric acid in step S1 is 1:2-4.
4. The method for preparing a polypropylene-based conductive composite material according to claim 1, characterized in that: The mass ratio of the pretreated graphene and modified-aminopropyltrimethoxysilane in step S2 is 1:0.3-0.5; the organic solvent in the organic solvent-deionized water system is one of methanol, ethanol, ethylene glycol or acetone; the mass ratio of the organic solvent and deionized water is 5-10:
1.
5. The method for preparing a polypropylene-based conductive composite material according to claim 1, characterized in that: The preparation method of modified aminopropyltrimethoxysilane in step S2 is: (1) adding ethanol, γ-aminobutyric acid, 4-chloro-1-butanol and triethylamine to a reaction vessel in sequence, and reacting under reflux at 78-80° C. for 4-5 hours to obtain aminobutyric acid-alcohol; (2) adding anhydrous tetrahydrofuran, aminobutyric acid-alcohol and triethylamine to a reaction vessel, and adding diethylphosphite chloride dropwise at 0-5° C., and then keeping the temperature for reaction for 2-3 hours to obtain aminobutyric acid-phosphite; (3) adding ethanol, aminobutyric acid-phosphite and 1-chlorododecane to a reaction vessel in sequence, and reflux reacting at 78-80° C. for 12-14 hours to obtain aminobutyric acid-quaternary ammonium salt; (4) anhydrous tetrahydrofuran, aminobutyric acid-quaternary ammonium salt and triphosgene are added to the reaction vessel in sequence, and pyridine is added dropwise at 0-5° C. After the addition is completed, the reaction is carried out at room temperature for 6-8 hours to obtain an acyl chloride-quaternary ammonium salt; (5) Anhydrous dichloromethane, 3-aminopropyltrimethoxysilane and acyl chloride-quaternary ammonium salt are added to the reaction container in sequence, and reacted at room temperature for 2-4 hours to obtain modified-aminopropyltrimethoxysilane.
6. The method for preparing a polypropylene-based conductive composite material according to claim 5, characterized in that: The molar ratio of γ-aminobutyric acid, 4-chloro-1-butanol and triethylamine in step (1) is 1:2.1-2.2:1.5-2.0; the molar ratio of aminobutyric acid-alcohol, diethylphosphite chloride and triethylamine in step (2) is 1:2.0-2.1:1.3-1.
5.
7. The method for preparing a polypropylene-based conductive composite material according to claim 5, characterized in that: The molar ratio of aminobutyric acid-phosphite to 1-chlorododecane in step (3) is 1:1.0-1.1; the molar ratio of aminobutyric acid-quaternary ammonium salt, triphosgene and pyridine in step (4) is 1:1.0-1.1:1.3-1.
5.
8. The method for preparing a polypropylene-based conductive composite material according to claim 5, characterized in that: The molar ratio of 3-aminopropyltrimethoxysilane to acyl chloride-quaternary ammonium salt in step (5) is 1:1.0-1.
1.
9. A polypropylene-based conductive composite material, characterized in that: The polypropylene-based conductive composite material is prepared by the preparation method of any one of claims 1 to 8.