A stable rubber asphalt base sample, composite modified asphalt and preparation method and application thereof

By optimizing the preparation process of rubber asphalt base sample and composite modified asphalt, the problem of insufficient performance of rubber modified asphalt in the existing technology has been solved, high viscosity, high elasticity and improved stability have been achieved, which meets the requirements of ultra-thin overlays in multiple scenarios. high performance requirements.

CN118222108BActive Publication Date: 2024-10-18浙江顺畅高等级公路养护有限公司 +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410347250.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-10-18
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

Existing rubber-modified asphalt cannot fully meet the needs of green, durable, high-performance ultra-thin overlays in terms of high-temperature performance, low-temperature crack resistance and viscosity, and the preparation process is complex and costly, which affects its application in highway maintenance. .

Method used

By optimizing the dosage and process parameters of rubber powder, a stable rubber asphalt base sample was prepared, combined with SBS modifier, natural asphalt, solvent and reinforcing agent, and multiple mixing and shearing development processes were used to form a high-viscosity and high-elasticity Compound modified asphalt to improve its viscosity, elastic recovery rate and stability.

Benefits of technology

It achieves high-temperature stability, low-temperature crack resistance and good storage stability, significantly improves the overall road performance of ultra-thin overlay asphalt mixture, and meets high performance and durability requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118222108B_ABST
    Figure CN118222108B_ABST
Patent Text Reader

Abstract

The present invention provides a stable rubber asphalt base sample, a composite modified asphalt, and a preparation method and application thereof. The stable rubber asphalt base sample comprises, by weight: 70 to 85 parts of heavy cross-linked matrix asphalt and 15 to 30 parts of rubber powder. The raw materials for preparing the composite modified asphalt comprise, by weight percentage, the following components: 40 to 70% of the above-mentioned stable rubber asphalt base sample, 1 to 10% of SBS modifier, 1 to 3% of natural asphalt, 5 to 10% of a dissolution promoter, 3 to 6% of a reinforcing agent, 0.1 to 0.5% of a stabilizer, and the balance is heavy cross-linked matrix asphalt. The present invention solves the storage stability problem of traditional rubber modified asphalt, and balances the relationship between high viscosity and high elasticity indicators by using an optimal material ratio and preparation method. The composite modified asphalt provided by the present invention significantly improves the rutting resistance, water stability, low-temperature crack resistance, etc. of ultra-thin overlay asphalt mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road construction materials, and in particular to a stable rubber asphalt base sample, a composite modified asphalt, and a preparation method and application thereof. Background Art

[0002] Ultra-thin overlay is a preventive pavement maintenance technology with a wide range of applications and good effects. Asphalt is the key to the road performance and service life of ultra-thin overlays. High-viscosity modified asphalt, rubber-modified asphalt, etc. are high-performance asphalts commonly used in ultra-thin overlays. However, the key indicators of the commonly used modified asphalts such as high-temperature performance, low-temperature crack resistance, and viscosity still cannot fully meet the performance requirements of green, durable, and high-performance ultra-thin overlays. At present, high-viscosity and high-elastic asphalt is a special type of modified asphalt that is often used to meet the requirements of ultra-thin overlays to serve well under specific loads and environmental conditions. It is difficult to balance the relationship between its high viscosity and high elasticity properties and ensure its good construction and workability. This has always been the difficulty in the preparation of high-performance, high-viscosity, and high-elastic asphalt.

[0003] Rubber modification technology is one of the important technical directions for achieving high-viscosity and high-elastic modification. However, in the conventional preparation process of rubber asphalt, the rubber powder is difficult to fully degrade. Most of them only swell in the asphalt, and the solid-liquid two-phase characteristics are obvious. There are defects such as easy segregation and poor storage stability, which limits the application of high-viscosity and high-elastic asphalt in this technical route. In order to solve the problem of poor stability of rubber asphalt, the pre-desulfurization technology can be used to treat the rubber powder or the Terminal Blend (TB) process can be used to prepare rubber asphalt to improve the stability of asphalt. However, both methods have limitations. On the one hand, the process of treating rubber powder with pre-desulfurization technology is complicated and the cost is high. On the other hand, the excessive de-crosslinking of the TB process reduces the elastic properties of the asphalt. At the same time, the temperature during preparation is high, and the asphalt is easy to age and the performance is affected. On the other hand, based on the shortcomings of traditional rubber modified asphalt such as poor construction and workability and difficulty in compaction, composite modified rubber asphalt has become an important development direction for ultra-thin overlay binders. The rubber powder / SBS composite modification method can be used to deal with the performance attenuation problem caused by rubber powder degradation.

[0004] CN117003512A discloses a high-toughness and high-elasticity composite modified asphalt and its preparation method, wherein the high-toughness and high-elasticity composite modified asphalt comprises the following components by weight: 85-89 parts of heavy-duty asphalt, 2-4 parts of aromatic oil retardant, 3-4 parts of high-viscosity toughening modifier, 6-7 parts of thermoplastic styrene-butadiene rubber modifier, and 0.1-0.3 parts of sulfide stabilizer. This invention can only improve the toughness and elasticity of heavy-duty asphalt to a certain extent by adding high-viscosity toughening modifier, and the degree of improvement is limited; and there are still problems such as low viscosity of the overlay binder, and the high temperature performance and low temperature crack resistance cannot meet the requirements of ultra-thin overlay maintenance.

[0005] CN116790127A discloses a composite rock asphalt binder for environmentally friendly noise reduction ultra-thin overlay and its preparation method, wherein the binder comprises, by mass percentage: 60-80% SBS modified asphalt, 8-12% rock asphalt, 4-6% rubber powder, 8-12% catalytic cracking oil slurry, 3-5% high molecular polymer, 0.3-0.5% compatibilizer, 0.2-0.4% stabilizer. The invention uses SBS modified asphalt as the main material, and utilizes the characteristics of rock asphalt with large molecular weight, high softening point and strong antioxidant capacity to compound rubber powder and high molecular polymer to achieve the purpose of improving the low temperature performance of rock asphalt modified asphalt, but the modified formula has insufficient performance of overlay anti-skid and high temperature anti-rutting under the long-term action of light and rain.

[0006] Therefore, it is urgent to develop a rubber asphalt that can balance the performance of rubber asphalt, optimize the preparation process, reduce highway maintenance costs, and be suitable for ultra-thin overlays in multiple scenarios. This is of great significance to promoting the application and promotion of ultra-thin overlay preventive maintenance technology in highway maintenance.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] One of the purposes of the present invention is to provide a stable rubber asphalt base sample, which comprises, by weight, 70 to 85 parts of heavy crosslinking matrix asphalt and 15 to 30 parts of rubber powder. The present invention first optimizes the amount of rubber powder to obtain a rubber asphalt base sample for preparing subsequent composite modified asphalt, and meets the requirements of balancing high viscosity and high elasticity.

[0009] The second purpose of the present invention is to provide a method for preparing a stable rubber asphalt base sample, the preparation method comprising the following steps: mixing the heavy cross-linked matrix asphalt and rubber powder according to a ratio, shearing and developing, and preparing the stable rubber asphalt base sample.

[0010] The third object of the present invention is to provide a composite modified asphalt, wherein the raw materials for preparing the composite modified asphalt include the following components by mass percentage: 40-70% of the stabilized rubber asphalt base sample, 1-10% of SBS modifier, 1-3% of natural asphalt, 5-10% of a dissolution promoter, 3-6% of a reinforcing agent, 0.1-0.5% of a stabilizer, and the balance is a heavy cross-linking matrix asphalt. Based on the stabilized rubber asphalt base sample, the present invention adopts a two-stage modification to prepare a composite modified high-viscosity and high-elastic asphalt for ultra-thin overlay.

[0011] The fourth object of the present invention is to provide a method for preparing a composite modified asphalt, which comprises the following steps: mixing a stabilized rubber asphalt base sample, a heavy cross-linking matrix asphalt and a solvent for the first time to obtain a mixture one; mixing the mixture one, an SBS modifier and a reinforcing agent for the second time to obtain a mixture two; mixing the mixture two and a stabilizer for the third time to obtain a mixture three; and mixing the mixture three and natural asphalt for the fourth time to obtain a composite modified asphalt.

[0012] The fifth object of the present invention is to provide an application of the stable rubber asphalt base sample or the composite modified asphalt in the preparation of ultra-thin overlays. The rubber asphalt base sample or the composite modified asphalt can be used to prepare high-performance and durable ultra-thin overlay asphalt mixtures, significantly improving the overall road performance of the ultra-thin overlays.

[0013] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0014] In a first aspect, the present invention provides a stabilized rubber asphalt base sample, wherein the stabilized rubber asphalt base sample comprises, by weight: 70 to 85 parts of heavy cross-linked matrix asphalt and 15 to 30 parts of rubber powder.

[0015] In the present invention, the rubber asphalt base sample is prepared by selecting a heavy cross-linked matrix asphalt and optimizing the amount of rubber powder, thereby obtaining a stable rubber asphalt base sample that is not easy to segregate (segregation index <2.5°C).

[0016] In the stabilized rubber asphalt base sample, the content of heavy cross-linking matrix asphalt is 70 to 85 parts, for example, it can be 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, etc.

[0017] In the stabilized rubber asphalt base sample, the content of rubber powder is 15 to 30 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.

[0018] Preferably, the heavy cross-linked base asphalt is selected from 70# heavy cross-linked base asphalt.

[0019] Preferably, the Brookfield rotation viscosity of the 70# heavy crosslinking base asphalt at 60°C is ≥250Pa·s, for example, it can be 250Pa·s, 252Pa·s, 254Pa·s, 255Pa·s, 260Pa·s, 265Pa·s, 270Pa·s, 280Pa·s, 300Pa·s, etc.

[0020] In the present invention, 70# heavy cross-linking matrix asphalt with a 60°C Brookfield rotation viscosity ≥ 250 Pa·s is preferred to ensure the high temperature stability of the material and improve the pavement service performance.

[0021] Preferably, the rubber powder is selected from original rubber powder with a particle size of 80 to 100 mesh, for example, it can be 80 mesh, 82 mesh, 84 mesh, 85 mesh, 86 mesh, 88 mesh, 90 mesh, 92 mesh, 94 mesh, 95 mesh, 96 mesh, 98 mesh, 100 mesh, etc.

[0022] In the present invention, it is preferred to add 80-100 mesh virgin rubber powder. After swelling and shearing treatment in the matrix asphalt, the rubber powder will absorb the light components in the matrix asphalt and form a gel film with a high asphalt content on the surface of the rubber powder particles, which reduces the temperature sensitivity of the rubber asphalt base sample and improves the adhesion, high temperature performance and low temperature ductility of the rubber asphalt base sample.

[0023] In a second aspect, the present invention provides a method for preparing a stabilized rubber asphalt base sample as described in the first aspect (using an internal mixing method), the preparation method comprising the following steps:

[0024] The heavy cross-linking matrix asphalt and rubber powder are mixed according to a proportion, and then sheared and developed to prepare the stabilized rubber asphalt base sample.

[0025] In the present invention, a rubber asphalt base sample that is not easy to segregate and is stable (segregation index < 2.5°C) is prepared by optimizing the rubber powder dosage and specific process parameters such as mixing, shearing, and development.

[0026] Preferably, the heavy-crosslinked base asphalt and the rubber powder are mixed in the following manner: the heavy-crosslinked base asphalt is heated, and then the rubber powder is added in batches for mixing.

[0027] Preferably, the heating temperature is 160-170°C, for example, it can be 160°C, 162°C, 164°C, 166°C, 168°C, 170°C, etc.

[0028] Preferably, the heavy cross-linking matrix asphalt and the rubber powder are mixed in the following manner: the heavy cross-linking matrix asphalt is heated to 160-170° C., and then the rubber powder is added and mixed.

[0029] In the present invention, the mixing method is limited in order to make the rubber powder fully swell and degrade, thereby obtaining a modification effect with better viscoelasticity.

[0030] Preferably, the shearing is by colloid mill shearing.

[0031] Preferably, the shearing temperature is 180-200°C, for example, it may be 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, 192°C, 194°C, 196°C, 198°C, 200°C, etc.

[0032] Preferably, the shear rate is 5000-7000 r / min, for example, it can be 5000 r / min, 5200 r / min, 5400 r / min, 5600 r / min, 5800 r / min, 6000 r / min, 6200 r / min, 6400 r / min, 6600 r / min, 6800 r / min, 7000 r / min, etc.

[0033] Preferably, the shearing time is 30 to 60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0034] Preferably, the development temperature is 180-200°C, for example, it can be 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, 192°C, 194°C, 196°C, 198°C, 200°C, etc.

[0035] Preferably, the developing is carried out under agitation.

[0036] Preferably, the stirring speed is 1800-2500 r / min, for example, it can be 1800 r / min, 1900 r / min, 2000 r / min, 2100 r / min, 2200 r / min, 2300 r / min, 2400 r / min, 2500 r / min, etc., and more preferably 2000-2200 r / min.

[0037] Preferably, the stirring time is 12 to 16 hours, for example, it can be 12 hours, 12.5 hours, 13 hours, 13.5 hours, 14 hours, 14.5 hours, 15 hours, 15.5 hours, 16 hours, etc.

[0038] In the present invention, the preferred development temperature is 180-200°C and the stirring time is 12-16h, which are significantly improved compared with conventional rubber asphalt preparation. This is to maximize the desulfurization and depolymerization reactions of the rubber powder particles through long-term stirring under higher temperature conditions, maximize dissolution in asphalt, and reduce the high-temperature viscosity of the rubber asphalt, thereby ensuring the storage stability and construction workability of the subsequent preparation of the composite modified asphalt.

[0039] In a third aspect, the present invention provides a composite modified asphalt, wherein the raw materials for preparing the composite modified asphalt include the following components by weight percentage:

[0040] As described in the first aspect, the stabilized rubber asphalt base sample is 40-70%, the SBS modifier is 1-10%, the natural asphalt is 1-3%, the solvent promoter is 5-10%, the reinforcing agent is 3-6%, the stabilizer is 0.1-0.5%, and the balance is the heavy cross-linking matrix asphalt.

[0041] In the present invention, the stabilized rubber asphalt base sample described in the first aspect is diluted with the newly added heavy cross-linked matrix asphalt (preferably the same grade heavy cross-linked asphalt is used to dilute the base sample), and the newly added heavy cross-linked asphalt does not participate in the high-temperature development process of the rubber asphalt base sample, which can effectively reduce the aging degree and production energy consumption of the rubber asphalt with the target rubber powder content. At the same time, the present invention also uses the above-mentioned optimal material blending ratio to balance the proportions of various materials such as the solubilizer, SBS modifier, reinforcing agent, stabilizer, and natural asphalt, so as to achieve the comprehensive improvement of waste rubber utilization and road performance, and can greatly improve the 60°C viscosity and elastic recovery rate of the modified asphalt, and the high and low temperature stability.

[0042] Taking the total mass of the raw materials for preparing the composite modified asphalt as 100%, the content of the stabilized rubber asphalt base sample is 40-70%, for example, it can be 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, etc.

[0043] Taking the total mass of raw materials for preparing the composite modified asphalt as 100%, the content of the SBS modifier is 1-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.

[0044] Taking the total mass of raw materials for preparing the composite modified asphalt as 100%, the content of natural asphalt is 1-3%, for example, it can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, etc.

[0045] Taking the total mass of raw materials for preparing the composite modified asphalt as 100%, the content of the dissolution agent is 5-10%, for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, etc.

[0046] Taking the total mass of the raw materials for preparing the composite modified asphalt as 100%, the content of the reinforcing agent is 3-6%, for example, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc.

[0047] Taking the total mass of raw materials for preparing the composite modified asphalt as 100%, the content of the stabilizer is 0.1-0.5%, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, etc.

[0048] Preferably, the SBS modifier is a styrene-butadiene-styrene block copolymer.

[0049] The styrene-butadiene-styrene block copolymer is a thermoplastic elastomer, which forms a network structure in the asphalt through swelling and shearing processes in the present invention, thereby improving the thermal stability, high and low temperature performance, and elastic recovery performance of the asphalt.

[0050] Preferably, the SBS modifier is selected from linear SBS modifiers and / or star-shaped SBS modifiers.

[0051] Preferably, the SBS modifier is selected from linear styrene-butadiene-styrene block copolymers and / or star styrene-butadiene-styrene block copolymers.

[0052] Preferably, the relative molecular weight of the linear styrene-butadiene-styrene block copolymer is 80,000-120,000, for example, 80,000, 85,000, 90,000, 95,000, 100,000, 105,000, 110,000, 115,000, 120,000, etc.

[0053] Preferably, the relative molecular weight of the star-shaped styrene-butadiene-styrene block copolymer is 140,000 to 160,000, for example, 140,000, 142,000, 144,000, 146,000, 148,000, 150,000, 152,000, 154,000, 156,000, 158,000, 160,000, etc.

[0054] Preferably, the block ratio of the styrene-butadiene-styrene block copolymer is 30 / 70 (wherein 30 is styrene and 70 is butadiene).

[0055] Preferably, the styrene-butadiene-styrene block copolymer is non-oil-extended.

[0056] Preferably, the SBS modifier is a combination of a linear SBS modifier and a star-shaped SBS modifier, and the mass ratio of the linear SBS modifier to the star-shaped SBS modifier is (4-6):(1-2);

[0057] Among them, "4-6" can be, for example, 4, 4.5, 5, 5.5, 6, etc.;

[0058] Here, “1-2” can be, for example, 1, 1.2, 1.4, 1.6, 1.8, 2, etc.

[0059] In the present invention, it is preferred to add a linear SBS modifier and a star-shaped SBS modifier in combination. This is because the linear SBS has better compatibility with the base asphalt than the star-shaped SBS, and the star-shaped SBS has better viscosity-increasing and elasticity-enhancing effects than the linear SBS. Taking into account the performance characteristics of both, by adjusting the ratio of the two, the two can play a synergistic role, thereby effectively reducing the total usage of SBS and further improving the performance of the composite modified asphalt.

[0060] Preferably, the linear SBS modifier is LG501S and / or 1301.

[0061] Preferably, the star-shaped SBS modifier is 4302.

[0062] Preferably, the natural asphalt is selected from rock asphalt, and more preferably Iranian rock asphalt.

[0063] In the present invention, the above-mentioned Iranian rock asphalt has a high asphaltene content and has good compatibility with the base asphalt, which can further improve the aging resistance and high-temperature stability of the composite modified asphalt.

[0064] Preferably, the solubilizing agent is selected from aromatic oil and / or furfural oil.

[0065] In the present invention, the above-mentioned dissolving agent softens the asphalt, improves its ductility, and effectively promotes the compatibility of rubber powder, star-shaped SBS, linear SBS and asphalt, and can further improve the low-temperature performance of the composite modified asphalt.

[0066] Preferably, the aromatic oil is WKD.

[0067] Preferably, the reinforcing agent is selected from any one of C9 petroleum resin, C5 petroleum resin or phenolic resin, or a combination of at least two thereof.

[0068] In the present invention, the reinforcing agent can be evenly dispersed in the asphalt, and has a beneficial effect on the high temperature stability and strength of the composite modified asphalt.

[0069] Preferably, the stabilizer is selected from sulfur and / or trans-polyoctene.

[0070] In the present invention, the stabilizer can form an interfacial absorption layer between the polymer and the asphalt, thereby improving the stability of the composite modified asphalt. It should be noted that a chemical reaction will occur after the stabilizer is added, so that the asphalt forms a stable structure. The stabilizer is preferably added after the modifier is evenly dispersed in the asphalt, which is more conducive to improving the stability of the composite modified asphalt.

[0071] Preferably, the heavy cross-linked base asphalt is selected from 70# heavy cross-linked base asphalt.

[0072] Furthermore, the heavy crosslinking matrix asphalt is more preferably a 70# heavy crosslinking matrix asphalt having a Brookfield rotational viscosity at 60°C of ≥250 Pa·s.

[0073] In a fourth aspect, the present invention provides a method for preparing the composite modified asphalt as described in the third aspect, wherein the method for preparing the composite modified asphalt comprises the following steps:

[0074] The stabilized rubber asphalt base sample, the heavy crosslinking base asphalt and the solvent are mixed for the first time to obtain a mixture 1;

[0075] Mixing the mixture 1, the SBS modifier and the reinforcing agent for a second time to obtain a mixture 2;

[0076] Mixing the mixture 2 and the stabilizer for a third time to obtain a mixture 3;

[0077] The mixture three and the natural asphalt are mixed for the fourth time to obtain a composite modified asphalt.

[0078] In the present invention, while utilizing the optimal material blending ratio, the above-mentioned specific mixing, shearing, development and other process methods are adopted to prepare a composite modified high-viscosity and high-elastic asphalt with better road performance, thereby better balancing the ratios of various materials such as the solubilizer, SBS modifier, reinforcing agent, stabilizer, and natural asphalt.

[0079] Preferably, the specific steps of the first mixing are:

[0080] The stabilized rubber asphalt base sample and the heavily cross-linked matrix asphalt are heated separately, and then the heavily cross-linked matrix asphalt and the solvent are added to the heated stabilized rubber asphalt base sample to obtain a mixture.

[0081] Preferably, during the preparation of mixture one, the stabilized rubber asphalt base sample is heated to 170-190°C, for example, it can be 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, etc.

[0082] Preferably, during the preparation of mixture one, the heavy crosslinking matrix asphalt is heated to 140-160°C, for example, 140°C, 142°C, 144°C, 146°C, 148°C, 150°C, 152°C, 154°C, 156°C, 158°C, 160°C, etc.

[0083] Preferably, the specific steps of the first mixing are:

[0084] The stabilized rubber asphalt base sample is heated to 170-190° C., the heavily cross-linked matrix asphalt is heated to 140-160° C., and then the heavily cross-linked matrix asphalt and the solvent are added to the heated stabilized rubber asphalt base sample to obtain a mixture.

[0085] Preferably, the specific steps of the second mixing are:

[0086] The mixture 1 is heated, and then the SBS modifier and the reinforcing agent are added to the heated mixture 1, and the mixture is stirred and sheared to obtain the mixture 2.

[0087] Preferably, during the preparation of mixture 2, mixture 1 is heated to 170-190°C, for example, 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, etc.

[0088] Preferably, during the preparation of mixture 2, the stirring speed is 2000-2500 r / min, for example, it can be 2000 r / min, 2100 r / min, 2200 r / min, 2300 r / min, 2400 r / min, 2500 r / min, etc., and the stirring time is 30-60 min, for example, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0089] Preferably, during the preparation of the mixture 2, the shearing is performed by a colloid mill.

[0090] Preferably, during the preparation of mixture 2, the shear rate is 7000-9000 r / min, for example, it can be 7000 r / min, 7200 r / min, 7400 r / min, 7600 r / min, 7800 r / min, 8000 r / min, 8200 r / min, 8400 r / min, 8600 r / min, 8800 r / min, 9000 r / min, etc.

[0091] Preferably, during the preparation of mixture 2, the shearing time is 30 to 60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0092] Preferably, the specific steps of the second mixing are:

[0093] The mixture 1 is heated to 170-190° C., and then the SBS modifier and the reinforcing agent are added to the heated mixture 1, and stirred at a speed of 2000-2500 r / min for 30-60 min, and then sheared by a colloid mill, the shear rate is 7000-9000 r / min, and the shear time is 30-60 min, to obtain a mixture 2.

[0094] Preferably, the specific steps of the third mixing are:

[0095] A stabilizer was added to the mixture two, and the mixture was stirred to obtain a mixture three.

[0096] Preferably, during the preparation of mixture three, the temperature needs to be controlled at 170-190°C, for example, it can be 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, etc.

[0097] Preferably, in the preparation process of mixture three, the stirring speed is 2000-2500r / min, for example, it can be 2000r / min, 2100r / min, 2200r / min, 2300r / min, 2400r / min, 2500r / min, etc., and the stirring time is 120-180min, for example, it can be 120min, 125min, 130min, 135min, 140min, 145min, 150min, 155min, 160min, 165min, 170min, 175min, 180min, etc.

[0098] Preferably, the specific steps of the third mixing are:

[0099] The temperature is controlled at 170-190° C., a stabilizer is added to the mixture two, and the mixture is stirred at a speed of 2000-2500 r / min for 120-180 min to obtain a mixture three.

[0100] Preferably, the stabilizer needs to be added to the mixture two in batches, and the amount of the stabilizer added each time is 0.03-0.1% of the total mass of the mixture two, for example, it can be 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, etc.

[0101] In the present invention, the stabilizer needs to be added to the mixture two in batches. This is because a chemical reaction will occur after the stabilizer is added to form a stable structure in the composite modified asphalt. However, adding a large amount of stabilizer at one time will affect the chemical reaction effect and is not conducive to the formation of a stable structure. Therefore, the stabilizer is added in batches to ensure that the stabilizer and the asphalt fully react and the properties are more stable.

[0102] Preferably, the specific steps of the fourth mixing are:

[0103] Add natural asphalt to mixture three and stir to obtain composite modified asphalt.

[0104] Preferably, during the preparation of the composite modified asphalt, the temperature needs to be controlled at 170-190°C, for example, it can be 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, etc.

[0105] Preferably, in the preparation process of composite modified asphalt, the stirring speed is 2000-2500r / min, for example, it can be 2000r / min, 2100r / min, 2200r / min, 2300r / min, 2400r / min, 2500r / min, etc., and the stirring time is 30-60min, for example, it can be 30min, 35min, 40min, 45min, 50min, 55min, 60min, etc.

[0106] Preferably, the specific steps of the fourth mixing are:

[0107] The temperature is controlled at 170-190° C., natural asphalt is added to the mixture three, and stirred at a rotation speed of 2000-2500 r / min for 30-60 min to obtain a composite modified asphalt.

[0108] In a fifth aspect, the present invention provides a use of the stabilized rubber asphalt base sample as described in the first aspect, or the composite modified asphalt as described in the third aspect, in the preparation of an ultra-thin overlay.

[0109] Compared with the prior art, the present invention has the following beneficial effects:

[0110] (1) The composite modified asphalt of the present invention can realize the comprehensive improvement of waste rubber utilization and road performance at the same time. The rubber powder swells in the modified asphalt system and forms a network structure, which can greatly improve the viscosity and elastic recovery rate of the modified asphalt. The high temperature stability (dynamic viscosity at 60°C is 500,000 to 700,000 Pa·s, high temperature PG grade ≥100), deformation characteristics (elastic recovery rate at 25°C>96%, elongation at 5°C>30cm), and adhesion to aggregate are all good.

[0111] (2) The composite modified asphalt of the present invention has good storage stability. It utilizes high-speed shearing and stirring of various additives, and utilizes the preferred development temperature and time to ensure that the various additives are fully mixed and reacted to form a stable composite system. The system can be stored normally and can achieve no or low precipitation and segregation during use, thereby improving the storage stability of the composite modified asphalt. The segregation index is <1.2°C, which is convenient for engineering applications.

[0112] (3) The composite modified asphalt of the present invention can be used to prepare high-performance ultra-thin overlay asphalt mixture, which has good high-temperature stability (60°C dynamic stability>13000 times / mm, 70°C dynamic stability>8000 times / mm), water stability (freeze-thaw splitting strength ratio>87%, residual stability>94%), low-temperature crack resistance (-10°C low-temperature failure strain>10000με), adhesion performance (scattering loss<1.0%), and durability (three freeze-thaw cycle splitting strength ratio>85%), providing good driving comfort, crack resistance, rutting resistance, etc. for the ultra-thin overlay of asphalt pavement. BRIEF DESCRIPTION OF THE DRAWINGS

[0113] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0114] Figure 1 The present invention is a flow chart for preparing the stabilized rubber asphalt base sample and the composite modified asphalt.

[0115] Figure 2 This is a graph showing the change in viscosity index of the base sample provided in Example 1 during the development process at different temperatures. DETAILED DESCRIPTION

[0116] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0117] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0118] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the product of the invention is usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0119] Figure 1 The following is a flow chart of the preparation of the stabilized rubber asphalt base sample and the composite modified asphalt of the present invention. Figure 1 As shown, the preparation method of the stabilized rubber asphalt base sample comprises the following steps: after mixing the heavy cross-linked matrix asphalt and the rubber powder according to the proportion, shearing and developing are performed to prepare the stabilized rubber asphalt base sample. The preparation method of the composite modified asphalt comprises the following steps: the stabilized rubber asphalt base sample, the heavy cross-linked matrix asphalt and the solvent are mixed for the first time to obtain mixture one; the mixture one, the SBS modifier and the reinforcing agent are mixed for the second time to obtain mixture two; the mixture two and the stabilizer are mixed for the third time to obtain mixture three; the mixture three and the natural asphalt are mixed for the fourth time to obtain the composite modified asphalt. The present invention has no special requirements for the specific implementation method of the stirring, and the method well known to those skilled in the art can be adopted. The present invention limits the mixing method to obtain a modification effect with better viscoelasticity.

[0120] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0121] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0122] Example 1

[0123] This embodiment provides a stable rubber asphalt base sample and a composite modified asphalt containing the same.

[0124] The stabilized rubber asphalt base sample comprises, by weight percentage, 30% of 80-mesh virgin rubber powder and 70% of 70# heavy cross-linking matrix asphalt.

[0125] Among them, the Brookfield rotation viscosity of 70# heavy crosslinking base asphalt at 60℃ is 291.367Pa·s.

[0126] The stabilized rubber asphalt base sample is specifically prepared by the following steps:

[0127] (a) Weigh the raw materials according to their mass percentage: 30% of 80-mesh virgin rubber powder and 70% of 70# heavy cross-linking base asphalt;

[0128] (b) heating 70# heavy cross-linking base asphalt to 160° C., and then adding rubber powder in 5 portions, with the amount of rubber powder added each time being 8.57% of the total mass of the heavy cross-linking base asphalt, to obtain a mixture of heavy cross-linking base asphalt and virgin rubber powder;

[0129] (c) controlling the temperature of the mixture of heavy-duty base asphalt and virgin rubber powder to 180° C. and shearing the mixture by a colloid mill at a shear rate of 5500 r / min for 40 min;

[0130] (d) developing the sheared mixture, the development temperature is controlled at 180° C., and the development is carried out under stirring, the stirring speed is 2000 r / min, and the stirring time is 14 h, to obtain the stabilized rubber asphalt base sample.

[0131] The raw materials for preparing the composite modified asphalt include the following components by mass percentage:

[0132] The above-mentioned stabilized rubber asphalt base sample is 41.3%, star-shaped SBS modifier 4302 (styrene-butadiene-styrene block copolymer) is 1%, linear SBS modifier 1301 (styrene-butadiene-styrene block copolymer) is 5%, C9 petroleum resin is 3%, Iranian rock asphalt is 2%, aromatic oil is 6%, sulfur is 0.2%, and the balance is 70# base asphalt.

[0133] The composite modified asphalt is specifically prepared by the following steps:

[0134] (1) Weigh the raw materials according to their mass percentage: 41.3% of the above-mentioned stabilized rubber asphalt base sample, 1% of star-shaped SBS modifier (styrene-butadiene-styrene block copolymer), 5% of linear SBS modifier (styrene-butadiene-styrene block copolymer), 3% of C9 petroleum resin, 2% of Iranian rock asphalt, 6% of aromatic oil, 0.2% of sulfur, and the balance of 70# base asphalt;

[0135] (2) heating the 70# base asphalt to 150° C., controlling the temperature of the stabilized rubber asphalt base sample to 170° C., and then adding the 70# base asphalt and aromatic oil to the stabilized rubber asphalt base sample to obtain a mixture 1;

[0136] (3) The mixture 1 is temperature controlled to 170° C., and then C9 petroleum resin, star-shaped SBS modifier, and linear SBS modifier are added to the base sample, and stirred at a speed of 2200 r / min for 50 min; the mixture is sheared by a colloid mill, and the shear rate is controlled at 8000 r / min for 40 min to obtain a mixture 2, wherein C9 petroleum resin is added once at 3%; the star-shaped SBS modifier is added once at 1%; and the linear SBS modifier is added twice, each time at 2.5%;

[0137] (4) Controlling the temperature of the mixture 2 to 170° C., adding sulfur, and continuing to stir at a speed of 2200 r / min for 180 min to obtain a mixture 3; wherein the sulfur is added in 4 portions, each time adding 0.05%, and once every 5 min;

[0138] (5) The mixture is temperature-controlled to 170° C., natural asphalt is added, and stirring is continued at a speed of 2200 r / min for 40 min. After stopping stirring, a high-viscosity and high-elastic composite modified asphalt with stable properties is obtained.

[0139] According to the test method specified in the "Highway Engineering Asphalt and Asphalt Mixture Test Procedure" (JTG E20-2011), the technical index test of the product of Example 1 is performed, and the results are shown in Table 3. In order to verify the road performance of the mixture, the gradation is based on Table 4, the optimal asphalt-stone ratio is 7.1%, the compaction temperature is 165°C, and the relevant test pieces of the mixture are formed according to the specification. The technical index test results are shown in Table 5.

[0140] Example 2

[0141] This embodiment provides a stable rubber asphalt base sample and a composite modified asphalt containing the same.

[0142] The stabilized rubber asphalt base sample comprises, by weight percentage, 30% of 80-mesh virgin rubber powder and 70% of 70# heavy cross-linking matrix asphalt.

[0143] Among them, the Brookfield rotation viscosity of 70# heavy crosslinking base asphalt at 60℃ is 291.367Pa·s.

[0144] The stabilized rubber asphalt base sample is specifically prepared by the following steps:

[0145] (a) Weigh the raw materials according to their mass percentage: 30% of 80-mesh virgin rubber powder and 70% of 70# heavy cross-linking base asphalt;

[0146] (b) heating 70# heavy cross-linking base asphalt to 160° C., and then adding rubber powder in 5 portions, with the amount of rubber powder added each time being 8.57% of the total mass of the heavy cross-linking base asphalt, to obtain a mixture of heavy cross-linking base asphalt and virgin rubber powder;

[0147] (c) controlling the temperature of the mixture of heavy-duty base asphalt and virgin rubber powder to 180° C. and shearing the mixture by a colloid mill at a shear rate of 5500 r / min for 40 min;

[0148] (d) developing the sheared mixture, the development temperature is controlled at 180° C., and the development is carried out under stirring, the stirring speed is 2000 r / min, and the stirring time is 14 h, to obtain the stabilized rubber asphalt base sample.

[0149] The raw materials for preparing the composite modified asphalt include the following components by mass percentage:

[0150] The above-mentioned stabilized rubber asphalt base sample is 55.1%, star-shaped SBS modifier 4302 (styrene-butadiene-styrene block copolymer) is 1%, linear SBS modifier 1301 (styrene-butadiene-styrene block copolymer) is 5%, C9 petroleum resin is 3%, Iranian rock asphalt is 2%, aromatic oil is 6%, sulfur is 0.2%, and the balance is 70# base asphalt.

[0151] The composite modified asphalt is specifically prepared by the following steps:

[0152] (1) Weigh the raw materials according to their mass percentage: 55.1% of the above-mentioned stabilized rubber asphalt base sample, 1% of star-shaped SBS modifier (styrene-butadiene-styrene block copolymer), 5% of linear SBS modifier (styrene-butadiene-styrene block copolymer), 3% of C9 petroleum resin, 2% of Iranian rock asphalt, 6% of aromatic oil, 0.2% of sulfur, and the remainder of 70# base asphalt.

[0153] (2) heating the 70# base asphalt to 150° C., controlling the temperature of the stabilized rubber asphalt base sample to 175° C., and then adding the 70# base asphalt and aromatic oil to the base sample to obtain a mixture 1;

[0154] (3) The mixture 1 is temperature controlled to 175° C., and then C9 petroleum resin, star-shaped SBS modifier, and linear SBS modifier are added to the base sample, and stirred at a speed of 2200 r / min for 50 min; the mixture is sheared by a colloid mill, and the shear rate is controlled at 8000 r / min for 40 min to obtain a mixture 2; wherein C9 petroleum resin is added once at 3%; the star-shaped SBS modifier is added once at 1%; and the linear SBS modifier is added twice, each time at 2.5%;

[0155] (4) Controlling the temperature of the mixture 2 to 175° C., adding sulfur, and continuing to stir at a speed of 2200 r / min for 180 min to obtain a mixture 3; wherein the sulfur is added in 4 portions, each time at 0.05%, and once every 5 min;

[0156] (5) The mixture is temperature-controlled to 170° C., natural asphalt is added, and stirring is continued at a speed of 2200 r / min for 40 min. After stopping stirring, a high-viscosity and high-elastic composite modified asphalt with stable properties is obtained.

[0157] According to the test method specified in the "Highway Engineering Asphalt and Asphalt Mixture Test Procedure" (JTG E20-2011), the technical index test of the product of Example 2 is performed, and the results are shown in Table 3. In order to verify the road performance of the mixture, the gradation is based on Table 4, the optimal asphalt-stone ratio is 7.5%, the compaction temperature is 165°C, and the relevant test pieces of the mixture are formed according to the specification. The technical index test results are shown in Table 5.

[0158] Example 3

[0159] This embodiment provides a stable rubber asphalt base sample and a composite modified asphalt containing the same.

[0160] The stabilized rubber asphalt base sample comprises, by weight percentage, 30% of 80-mesh virgin rubber powder and 70% of 70# heavy cross-linking matrix asphalt.

[0161] Among them, the Brookfield rotation viscosity of 70# heavy crosslinking base asphalt at 60℃ is 291.367Pa·s.

[0162] The stabilized rubber asphalt base sample is specifically prepared by the following steps:

[0163] (a) Weigh the raw materials according to their mass percentage: 30% of 80-mesh virgin rubber powder and 70% of 70# heavy cross-linking base asphalt;

[0164] (b) heating 70# heavy cross-linking base asphalt to 160° C., and then adding rubber powder in 5 portions, with the amount of rubber powder added each time being 8.57% of the total mass of the heavy cross-linking base asphalt, to obtain a mixture of heavy cross-linking base asphalt and virgin rubber powder;

[0165] (c) controlling the temperature of the mixture of heavy-duty base asphalt and virgin rubber powder to 180° C. and shearing the mixture by a colloid mill at a shear rate of 5500 r / min for 40 min;

[0166] (d) developing the sheared mixture, the development temperature is controlled at 180° C., and the development is carried out under stirring, the stirring speed is 2000 r / min, and the stirring time is 14 h, to obtain the stabilized rubber asphalt base sample.

[0167] The raw materials for preparing the composite modified asphalt include the following components by mass percentage:

[0168] The above-mentioned stabilized rubber asphalt base sample is 68.9%, star-shaped SBS modifier 4302 (styrene-butadiene-styrene block copolymer) is 1%, linear SBS modifier 1301 (styrene-butadiene-styrene block copolymer) is 5%, C9 petroleum resin is 3%, Iranian rock asphalt is 2%, aromatic oil is 6%, sulfur is 0.2%, and the balance is 70# base asphalt.

[0169] The composite modified asphalt is specifically prepared by the following steps:

[0170] (1) Weigh the raw materials according to their mass percentage: 68.9% of the above-mentioned stabilized rubber asphalt base sample, 1% of star-shaped SBS modifier (styrene-butadiene-styrene block copolymer), 5% of linear SBS modifier (styrene-butadiene-styrene block copolymer), 3% of C9 petroleum resin, 2% of Iranian rock asphalt, 6% of aromatic oil, 0.2% of sulfur, and the balance of 70# base asphalt;

[0171] (2) heating the 70# base asphalt to 150° C., controlling the temperature of the stabilized rubber asphalt base sample to 180° C., and then adding the 70# base asphalt and aromatic oil to the stabilized rubber asphalt base sample to obtain a mixture 1;

[0172] (3) The mixture 1 is temperature controlled to 180° C., and then C9 petroleum resin, star-shaped SBS modifier, and linear SBS modifier are added to the base sample, and stirred at a speed of 2200 r / min for 50 min; the mixture is sheared by a colloid mill, and the shear rate is controlled at 8000 r / min for 40 min to obtain a mixture 2, wherein C9 petroleum resin is added once at 3%; the star-shaped SBS modifier is added once at 1%; and the linear SBS modifier is added twice, each time at 2.5%;

[0173] (4) Controlling the temperature of the mixture 2 to 180° C., adding sulfur, and continuing to stir at a speed of 2200 r / min for 180 min to obtain a mixture 3; wherein the sulfur is added in 4 portions, each time at 0.05%, and once every 5 min;

[0174] (5) The mixture is temperature-controlled to 170° C., natural asphalt is added, and stirring is continued at a speed of 2200 r / min for 40 min. After stopping stirring, a high-viscosity and high-elastic composite modified asphalt with stable properties is obtained.

[0175] According to the test method specified in the "Highway Engineering Asphalt and Asphalt Mixture Test Procedure" (JTG E20-2011), the technical index test of the product of Example 1 is performed, and the results are shown in Table 3. In order to verify the road performance of the mixture, the gradation is based on Table 4, the optimal asphalt-stone ratio is 8.1%, the compaction temperature is 165°C, and the relevant test pieces of the mixture are molded according to the specifications. The technical index test results are shown in Table 5.

[0176] Comparative Example 1

[0177] This comparative example provides a composite modified asphalt, and the raw materials for preparing the composite modified asphalt include the following components by mass percentage:

[0178] Star-shaped SBS modifier (styrene-butadiene-styrene block copolymer) 1%, linear SBS modifier (styrene-butadiene-styrene block copolymer) 5%, C9 petroleum resin 3%, Iranian rock asphalt 2%, aromatic oil 6%, sulfur 0.2%, and the balance is 70# base asphalt.

[0179] The composite modified asphalt is specifically prepared by the following steps:

[0180] (1) Weigh the raw materials according to their mass percentage: 1% of star-shaped SBS modifier 4302 (styrene-butadiene-styrene block copolymer), 5% of linear SBS modifier 1301 (styrene-butadiene-styrene block copolymer), 3% of C9 petroleum resin, 2% of Iranian rock asphalt, 6% of aromatic oil, 0.2% of sulfur, and the balance of 70# base asphalt;

[0181] (2) heating the 70# base asphalt to 150° C., and then adding aromatic oil to the 70# base asphalt to obtain a mixture 1;

[0182] (3) The temperature of the first mixture is controlled to 170° C., C9 petroleum resin, star-shaped SBS modifier, and linear SBS modifier are added to the base sample in small amounts and multiple times, and stirred at a speed of 2200 r / min for 50 min; the mixture is sheared by a colloid mill, and the shear rate is controlled at 8000 r / min for 40 min to obtain a second mixture; wherein C9 petroleum resin is added once, and 3% is added each time; the star-shaped SBS modifier is added once, and 1% is added each time; the linear SBS modifier is added twice, and 2.5% is added each time;

[0183] (4) Controlling the temperature of the mixture 2 to 170° C., adding sulfur, and continuing to stir at a speed of 2200 r / min for 180 min to obtain a mixture 3; wherein the sulfur is added in 4 portions, each time adding 0.05%, and once every 5 min;

[0184] (5) The mixture is temperature-controlled to 170° C., natural asphalt is added, and stirring is continued at a speed of 2200 r / min for 40 min. After stopping stirring, a high-viscosity and high-elastic composite modified asphalt with stable properties is obtained.

[0185] Comparative Example 2

[0186] This comparative example provides a composite modified asphalt, and the raw materials for preparing the composite modified asphalt include the following components by mass percentage:

[0187] 80 mesh virgin rubber powder 15%, star-shaped SBS modifier 4302 (styrene-butadiene-styrene block copolymer) 1%, linear SBS modifier 1301 (styrene-butadiene-styrene block copolymer) 5%, C9 petroleum resin 3%, Iranian rock asphalt 2%, aromatic oil 6%, sulfur 0.2%, and the balance is 70# base asphalt.

[0188] The composite modified asphalt is specifically prepared by the following steps:

[0189] (1) Weigh the raw materials according to their mass percentage: 80 mesh virgin rubber powder 15%, star-shaped SBS modifier (styrene-butadiene-styrene block copolymer) 1%, linear SBS modifier (styrene-butadiene-styrene block copolymer) 5%, C9 petroleum resin 3%, Iranian rock asphalt 2%, aromatic oil 6%, sulfur 0.2%, and the balance 70# base asphalt;

[0190] (2) heating the 70# base asphalt to 150° C., and then adding rubber powder and aromatic oil to the 70# base asphalt to obtain a mixture 1;

[0191] (3) The temperature of the first mixture is controlled to 170° C., C9 petroleum resin, star-shaped SBS modifier, and linear SBS modifier are added to the base sample in small amounts and multiple times, and stirred at a speed of 2200 r / min for 50 min; the mixture is sheared by a colloid mill, and the shear rate is controlled at 8000 r / min for 40 min to obtain a second mixture; wherein C9 petroleum resin is added once at 3%; the star-shaped SBS modifier is added once at 1%; and the linear SBS modifier is added twice, each time at 2.5%;

[0192] (4) Controlling the temperature of the mixture 2 to 170° C., adding sulfur, and continuing to stir at a speed of 2200 r / min for 180 min to obtain a mixture 3; wherein the sulfur is added in 4 portions, each time adding 0.05%, and once every 5 min;

[0193] (5) The mixture is temperature-controlled to 170° C., natural asphalt is added, and stirring is continued at a speed of 2200 r / min for 40 min. After stopping stirring, a high-viscosity and high-elastic composite modified asphalt with stable properties is obtained.

[0194] Test Example 1

[0195] Test sample: the stabilized rubber asphalt base sample provided in Example 1;

[0196] Test standard: According to the test method specified in the "Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011), the viscosity index of the base sample during the development process was tested, as shown in Table 1 and Figure 2 shown.

[0197] Table 1

[0198] Stirring time (h) 135℃ viscosity (Pa·s) 180℃ viscosity (Pa·s) 4 116.362 27.263 6 108.803 13.691 8 20.252 2.851 12 14.175 2.348 14 12.981 2.133

[0199] As shown in Table 1 above and Figure 2 It can be seen from the test data that with the increase of stirring time, the 135℃ and 180℃ Brookfield viscosities of the stabilized rubber asphalt base sample both decrease. After 12 hours of stirring, the changes in the 135℃ and 180℃ Brookfield viscosities are small, indicating that the swelling and degradation of the rubber powder have basically ended. Therefore, for Example 1, the recommended stirring time is at least 12 hours.

[0200] Test Example 2

[0201] Test sample: composite modified asphalt provided in Examples 1 to 3 and Comparative Examples 1 to 2;

[0202] Test standard: According to the test method specified in the "Test Specification for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011), as shown in Table 2 below:

[0203] Table 2

[0204]

[0205]

[0206] The test results are shown in Table 3 below:

[0207] Table 3

[0208]

[0209]

[0210] As shown in the test data of Table 3 above, the high-viscosity and high-elastic asphalt provided by the present invention has excellent thermal stability, elastic recovery performance, high temperature stability, bonding performance, and elongation performance. From the technical indicators, the asphalt provided by the present invention can simultaneously meet the following requirements: 25°C elastic recovery ≥ 96%, G*sin&≥2.2kPa critical temperature ≥ 100°C, 5°C elongation > 30cm, and 180°C viscosity < 4Pa·s, ensuring construction and workability. In addition, the viscosity and elastic recovery rate of Comparative Example 1 are both low, indicating that the rubber powder can improve the viscosity and elastic recovery rate in the modified asphalt system; in Comparative Example 2, the rubber powder has not undergone sufficient swelling and degradation, resulting in a high viscosity and a low elastic recovery rate.

[0211] Test Example 3

[0212] Test sample: composite modified asphalt provided in Examples 1 to 3;

[0213] Test standard: According to the test method specified in the "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011), in order to verify the road performance of the mixture, the gradation is based on Table 4 and the relevant test specimens of the mixture are formed according to the specifications;

[0214] The percentage of ore synthetic grading sieve holes passing through is shown in Table 4:

[0215] Table 4

[0216]

[0217] The test results are shown in Table 5 below:

[0218] Table 5

[0219]

[0220]

[0221] As shown in the test data of Table 5 above, the composite modified high-viscosity and high-elastic asphalt mixture of the present invention has excellent anti-rutting performance, with a dynamic stability of more than 13,000 times / mm at 60°C and more than 8,000 times / mm at 70°C. The composite modified high-viscosity and high-elastic asphalt mixture has outstanding low-temperature performance, with a failure strain of more than 10,000 με at -10°C, indicating that the mixture has excellent crack resistance at low temperatures. The residual stability of the mixture is >94%, and the freeze-thaw splitting test strength ratio is >87%, which shows good water stability. The splitting strength ratio of three freeze-thaw cycles is >85%, which shows good durability.

[0222] In summary, the present invention solves the storage stability problem of traditional rubber modified asphalt, balances the relationship between high viscosity and high elasticity indicators by utilizing the preferred material ratio and preparation method, and significantly improves the anti-rutting performance, water stability, and low-temperature crack resistance of the ultra-thin overlay asphalt mixture.

[0223] Furthermore, the asphalt mixture of the present invention has been subjected to two colloid mill high-speed shearing and grinding processes; wherein, the purpose of the first colloid mill shearing is to promote the swelling and dispersion of rubber powder in the asphalt; the purpose of the second colloid mill shearing is to accelerate the dispersion of the modifier in the asphalt and improve the stability of the asphalt. The high-viscosity and high-elasticity asphalt of the present invention has excellent storage stability and can be heated multiple times and stored for a long time. The polymer modifier of the present invention forms a stable network structure in the asphalt through swelling, shearing and other processes, thereby improving the high and low temperature performance and thermal stability of the asphalt. The PG grade is ≥100, which is significantly improved compared to SBS modified asphalt. The ultra-thin overlay asphalt mixture prepared with the high-viscosity and high-elasticity asphalt of the present invention has a performance level far exceeding the requirements of industry specifications and has good long-term durability.

[0224] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite modified asphalt, characterized in that: The raw materials for preparing the composite modified asphalt include the following components by mass percentage: 40-70% of stabilized rubber asphalt base sample, 1-10% of SBS modifier, 1-3% of natural asphalt, 5-10% of solvent promoter, 3-6% of reinforcing agent, 0.1-0.5% of stabilizer, and the balance is heavy cross-linking matrix asphalt; The stabilized rubber asphalt base sample comprises, by weight: 70-85 parts of heavy cross-linked matrix asphalt and 15-30 parts of rubber powder; the preparation method of the stabilized rubber asphalt base sample comprises the following steps: mixing the heavy cross-linked matrix asphalt and the rubber powder according to a proportion, shearing and developing, and preparing the stabilized rubber asphalt base sample; The SBS modifier is a combination of a linear SBS modifier and a star-shaped SBS modifier, wherein the mass ratio of the linear SBS modifier to the star-shaped SBS modifier is (4-6):(1-2); the SBS modifier is a styrene-butadiene-styrene block copolymer; The natural asphalt is Iranian rock asphalt; The reinforcing agent is selected from any one of C9 petroleum resin, C5 petroleum resin or phenolic resin, or a combination of at least two of them.

2. The composite modified asphalt according to claim 1, characterized in that: The heavy cross-linked matrix asphalt in the raw material for preparing the stabilized rubber asphalt base sample is selected from 70# heavy cross-linked matrix asphalt.

3. The composite modified asphalt according to claim 1, characterized in that: The rubber powder is selected from original rubber powder with a particle size of 80 to 100 meshes.

4. The composite modified asphalt according to claim 1, characterized in that: The method of mixing the heavy-duty matrix asphalt and the rubber powder is specifically as follows: the heavy-duty matrix asphalt is heated to 160-170° C., and then the rubber powder is added and mixed.

5. The composite modified asphalt according to claim 1, characterized in that: The shearing is performed by colloid mill shearing, the shearing temperature is 180-200° C., the shearing rate is 5000-7000 r / min, and the shearing time is 30-60 min.

6. The composite modified asphalt according to claim 1, characterized in that: The growth temperature is 180-200°C.

7. The composite modified asphalt according to claim 1, characterized in that: The growth is carried out under stirring, the stirring speed is 1800-2500 r / min, and the stirring time is 12-16 hours.

8. The composite modified asphalt according to claim 1, characterized in that: The linear SBS modifier is LG501S and / or 1301.

9. The composite modified asphalt according to claim 1, characterized in that: The star-shaped SBS modifier is 4302.

10. The composite modified asphalt according to claim 1, characterized in that: The solubilizing agent is selected from aromatic oil and / or furfural oil.

11. The composite modified asphalt according to claim 10, characterized in that: The aromatic oil is WKD.

12. The composite modified asphalt according to claim 1, characterized in that: The stabilizer is selected from sulfur and / or trans-polyoctene.

13. The composite modified asphalt according to claim 1, characterized in that: The heavy cross-linked base asphalt in the raw material for preparing the composite modified asphalt is selected from 70# heavy cross-linked base asphalt.

14. The composite modified asphalt according to claim 13, characterized in that: The heavy crosslinking matrix asphalt is a 70# heavy crosslinking matrix asphalt with a Brookfield rotation viscosity of ≥250 Pa·s at 60°C.

15. A method for preparing a composite modified asphalt according to any one of claims 1 to 14, characterized in that: The preparation method of the composite modified asphalt comprises the following steps: The stabilized rubber asphalt base sample, the heavy crosslinking base asphalt and the solvent are mixed for the first time to obtain a mixture 1; Mixing the mixture 1, the SBS modifier and the reinforcing agent for a second time to obtain a mixture 2; Mixing the mixture 2 and the stabilizer for a third time to obtain a mixture 3; The mixture three and the natural asphalt are mixed for the fourth time to obtain a composite modified asphalt.

16. The method for preparing composite modified asphalt according to claim 15, characterized in that: The specific steps of the first mixing are: The stabilized rubber asphalt base sample is heated to 170-190° C., the heavily cross-linked matrix asphalt is heated to 140-160° C., and then the heavily cross-linked matrix asphalt and the solvent are added to the heated stabilized rubber asphalt base sample to obtain a mixture.

17. The method for preparing composite modified asphalt according to claim 15, characterized in that: The specific steps of the second mixing are: The mixture 1 is heated to 170-190° C., and then the SBS modifier and the reinforcing agent are added to the heated mixture 1, and stirred at a speed of 2000-2500 r / min for 30-60 min, and then sheared by a colloid mill, the shear rate is 7000-9000 r / min, and the shear time is 30-60 min, to obtain a mixture 2.

18. The method for preparing composite modified asphalt according to claim 15, characterized in that: The specific steps of the third mixing are: The temperature is controlled at 170-190° C., a stabilizer is added to the mixture two, and the mixture is stirred at a speed of 2000-2500 r / min for 120-180 min to obtain a mixture three.

19. The method for preparing composite modified asphalt according to claim 18, characterized in that: The stabilizer needs to be added to the mixture two in batches, and the amount of the stabilizer added each time is 0.03-0.1% of the total mass of the mixture two.

20. The method for preparing composite modified asphalt according to claim 15, characterized in that: The specific steps of the fourth mixing are: The temperature is controlled at 170-190° C., natural asphalt is added to the mixture three, and stirred at a rotation speed of 2000-2500 r / min for 30-60 min to obtain a composite modified asphalt.

21. Use of the composite modified asphalt according to any one of claims 1 to 14 in preparing an ultra-thin overlay.

Citation Information

Patent Citations

  • Super-tough asphalt concrete for paving ultrathin overlay and preparation method of super-tough asphalt concrete

    CN117003512A

  • High-mixing-amount rubber powder-SBS composite modified asphalt and preparation method thereof