A method for recovering copper and nickel from waste materials

Through microbial pools and electrolytic extraction technology, the problem of low recovery rate caused by high chromium in copper-nickel sludge has been solved, efficient and low-impurity copper-nickel recovery has been achieved, the process has been simplified and the recovery rate has been improved.

CN118241041BActive Publication Date: 2024-10-22YANGJIANG FEDERAL METAL CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410354151.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-22
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

In the existing copper-nickel recovery technology, the copper-nickel sludge contains high chromium, which results in a high melting point of the slag in the recycling smelting process, making slag difficult, and poor separation of matte and slag, resulting in a low copper-nickel recovery rate.

Method used

The waste materials are soaked in a microbial pool, using microorganisms such as Sulfobacillus thermophilus, Bifidobacterium thermophilus and Thiobacillus thermophilus, combined with glycerol and glutathione, through solid-liquid separation and electrolytic extraction, and using dodecane Benzene sulfonic acid, polyethylene glycol and EDTA work synergistically to improve the recovery efficiency of copper and nickel.

Benefits of technology

It achieves efficient copper and nickel recovery, simplifies the treatment process, reduces the impurity content, improves the recovery rate, ensures the health of cells in the microbial pool, and improves the enrichment capacity of copper and nickel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004760751150000091
    Figure BDA0004760751150000091
  • Figure BDA0004760751150000101
    Figure BDA0004760751150000101
Patent Text Reader

Abstract

The present invention relates to a method for recovering copper and nickel from waste materials, and belongs to the technical field of metal recovery. The method comprises the following steps: W1. crushing the waste materials, placing them in a microbial pool for immersion, and separating the solid and liquid to obtain a filtrate and a filter residue; W2. copper extraction; W3. copper back extraction, electrolytic treatment, and obtaining copper at the cathode; W4. nickel extraction; W5. nickel back extraction; W6. electrolytic treatment, and obtaining nickel at the cathode. The microorganisms in the microbial pool provided by the present invention are thermophilic sulfur oxidizing sulfur bacillus, thermophilic bifidobacterium, and thermophilic sulfur bacillus, which can leach metal ions, simplify the treatment process, and do not need to perform special removal treatment on resins or fibers; in addition, glycerol and glutathione are contained, and the synergistic effect of the two helps microbial cells to eliminate excessive copper ions and nickel ions, reduce their damage to cells, and maintain the cells in the microbial pool at a higher cell number concentration, thereby ensuring the efficiency of copper and nickel leaching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal recovery and relates to a method for recovering copper and nickel from waste materials. Background Art

[0002] Copper-nickel waste has a wide range of sources and complex compositions. In addition to copper and nickel, it also contains iron, chromium, aluminum or resin, etc. At present, copper-nickel recovery is mainly through reduction smelting to produce alloy phase and matte phase, and the alloy phase and matte phase are further recovered through conventional impurity removal process. However, copper-nickel sludge contains high chromium, which easily leads to high melting point of slag in conventional recovery smelting process, difficult slag making, poor separation effect of matte and slag, resulting in low copper-nickel recovery rate.

[0003] Copper ions and nickel ions are heavy metal ions that can bind to bacterial cell proteins to denature them, or bind to a base on an enzyme after entering the cell to inactivate it, or bind to metabolic intermediates to block metabolism or replace the main elements in the cell structure, turning normal metabolites into invalid compounds, thereby inhibiting the growth of microorganisms or causing death. However, bacteria have the ability to regulate their metabolic pathways. When there is a high concentration in the environment, the bacteria will change or adjust their metabolic pathways after a period of adjustment to adapt to the new environment. This adaptability may be temporary, permanent, or limited. Too high a concentration can easily make it difficult for microorganisms to tolerate or even lose their activity and cannot grow.

[0004] Invention CN115386730B discloses a method for recovering copper and nickel from copper-nickel sludge, belonging to the technical field of waste resource utilization. The method comprises: if the chromium content in the copper-nickel sludge to be treated is ≥3wt% or the mass percentage of copper to nickel is <2, the copper-nickel sludge to be treated is subjected to medium-low temperature reduction sulfidation roasting, and then copper-nickel and chromium are separated by ore dressing; if the chromium content in the copper-nickel sludge to be treated is <3wt% and the content ratio of copper to nickel is 2≤≤5, the copper-nickel sludge to be treated is mixed with a sulfidizing agent, and high-temperature reduction sulfidation smelting is performed to obtain copper-nickel matte; if the chromium content in the copper-nickel sludge to be treated is <3wt% and the content ratio of copper to nickel is >5, copper-nickel alloy and matte are recovered by pyrometallurgical reduction smelting.

[0005] Invention CN113477404B discloses a method for efficiently recovering nickel and copper metal from nickel smelting slag. The method comprises the following steps: (1) crushing: crushing the nickel smelting slag to obtain nickel slag particles; (2) reduction-sulfurization roasting: adding a certain amount of pyrite to the fine-grained nickel slag and mixing, spreading a certain amount of carbon powder on the surface, and roasting at 1400°C; (3) recovery: grinding the obtained roasted modified slag and recovering it by flotation operation, and finally obtaining a copper-nickel mixed concentrate. Summary of the invention

[0006] The object of the present invention is to provide a method for recovering copper and nickel from waste materials, which has the characteristics of high recovery rate and low impurity content.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for recovering copper-nickel from waste materials comprises the following steps:

[0009] W1. crushing the waste to obtain waste particles, and then soaking the waste particles in a microbial pool for 20 to 30 days, and performing solid-liquid separation to obtain a filtrate and a filter residue;

[0010] W2. The resulting filtrate was extracted with a copper extractant Lix984 to obtain a copper raffinate and a copper-containing organic phase;

[0011] W3. adding a sulfuric acid solution at a concentration of 190 g / L as a copper stripping agent to the copper-containing organic phase to obtain a copper-containing stripping solution; electrolyzing the copper-containing stripping solution to obtain copper at the cathode;

[0012] W4. A nickel extractant HBL110 was added to the copper raffinate for extraction to obtain a nickel raffinate and a nickel-containing organic phase;

[0013] W5. In the nickel-containing organic phase, a sulfuric acid solution was added at a concentration of 75g / L as a nickel stripping agent to obtain a nickel-containing stripping solution;

[0014] W6. Electrolysis is carried out using the nickel-containing stripping solution as the electrolyte to obtain nickel at the cathode.

[0015] As a preferred technical solution of the present invention, the microorganisms in the microbial pool described in step W1 include thermophilic sulfur oxidizing bacteria, thermophilic bifidobacterium and thermophilic sulfur bacillus.

[0016] As a preferred technical solution of the present invention, the concentration of the thermophilic sulfur oxidizing bacillus is 15-25×106cell / ml;

[0017] The concentration of the thermophilic bifidobacterium is 10-20×106cell / ml;

[0018] The concentration of the thermophilic sulfur bacillus is 20-30×106cell / ml.

[0019] As a preferred technical solution of the present invention, the microbial pool also contains glycerol and glutathione.

[0020] As a preferred technical solution of the present invention, the mass concentration of glycerol is 8-10%;

[0021] The mass concentration of the glutathione is 3-5%.

[0022] As a preferred technical solution of the present invention, the feeding ratio of the waste particles described in step W1 is 100-200 g / L.

[0023] As a preferred technical solution of the present invention, the pH of the microbial pool described in step W1 is 1.0-4.0.

[0024] As a preferred technical solution of the present invention, the temperature of the microbial pool described in step W1 is 40-50°C.

[0025] As a preferred technical solution of the present invention, the electrolyte for the electrolytic treatment described in step W3 and step W6 contains dodecylbenzenesulfonic acid, polyethylene glycol and EDTA.

[0026] As a preferred technical solution of the present invention, the mass ratio of dodecylbenzenesulfonic acid, polyethylene glycol and EDTA is 20-25:8-10:15-20.

[0027] Beneficial effects of the present invention:

[0028] (1) The method for recovering copper and nickel from waste provided by the present invention uses a microbial pool to immerse the copper and nickel-containing waste to leach metal ions, thereby simplifying the treatment process and eliminating the need for special removal treatment of resins or fibers.

[0029] (2) In the method for recovering copper and nickel from waste provided by the present invention, glycerol and glutathione are added to the microbial pool, and the synergistic effect of the two helps the microbial cells to eliminate excess copper ions and nickel ions, reducing their damage to the cells, and maintaining the cells in the microbial pool at a higher cell number concentration, thereby ensuring the efficiency of copper and nickel leaching.

[0030] (3) In the method for recovering copper and nickel from waste provided by the present invention, the components of dodecylbenzenesulfonic acid, polyethylene glycol, and EDTA with a unique formula ratio can effectively improve the enrichment capacity of copper or nickel at the cathode through synergistic enhancement, thereby improving the yield of copper and nickel recovery. The specific principle is to improve the wettability of the electrode surface, reduce the interfacial resistance during the electrolysis process, and allow the impurity metal ions to form a complex to reduce the interference of impurities on the electrolysis process. DETAILED DESCRIPTION

[0031] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0032] Example 1

[0033] A method for recovering copper-nickel from waste materials comprises the following steps:

[0034] W1. The waste is crushed to obtain waste particles, wherein the copper content of the waste particles is ≥5wt% and the nickel content is ≥3wt%, and then the waste particles are immersed in a microbial pool for 20 days, and solid-liquid separation is performed to obtain a filtrate and a residue;

[0035] The feeding ratio of the waste particles is 100g / L;

[0036] The microorganisms in the microorganism pool include thermophilic sulfur oxidizing bacteria, thermophilic bifidobacterium and thermophilic sulfur bacteria;

[0037] The concentration of the thermophilic sulfur oxidizing bacillus is 15×10 6 cell / ml;

[0038] The concentration of the thermophilic bifidobacterium is 10×10 6 cell / ml;

[0039] The concentration of the thermophilic sulfur bacillus is 20×10 6 cell / ml;

[0040] The microbial pool also contains glycerol and glutathione;

[0041] The mass concentration of the glycerol is 8%;

[0042] The mass concentration of glutathione is 3%;

[0043] The pH of the microbial pool is 1.0;

[0044] The temperature of the microbial pool is 40°C;

[0045] W2. The resulting filtrate was extracted with a copper extractant Lix984 to obtain a copper raffinate and a copper-containing organic phase;

[0046] W3. adding a sulfuric acid solution at a concentration of 190 g / L as a copper stripping agent to the copper-containing organic phase to obtain a copper-containing stripping solution; electrolyzing the copper-containing stripping solution to obtain copper at the cathode;

[0047] W4. A nickel extractant HBL110 was added to the copper raffinate for extraction to obtain a nickel raffinate and a nickel-containing organic phase;

[0048] W5. In the nickel-containing organic phase, a sulfuric acid solution was added at a concentration of 75g / L as a nickel stripping agent to obtain a nickel-containing stripping solution;

[0049] W6. Electrolysis is carried out using the nickel-containing stripping solution as the electrolyte to obtain nickel at the cathode.

[0050] The electrolyte of the electrolytic treatment described in step W3 and step W6 contains dodecylbenzenesulfonic acid, polyethylene glycol and EDTA, and the dodecylbenzenesulfonic acid, polyethylene glycol and EDTA account for 15% of the mass of the electrolyte.

[0051] The mass ratio of dodecylbenzenesulfonic acid, polyethylene glycol and EDTA is 20:8:15.

[0052] Example 2

[0053] A method for recovering copper-nickel from waste materials comprises the following steps:

[0054] W1. The waste is crushed to obtain waste particles, wherein the copper content of the waste particles is ≥5wt%, and the nickel content is ≥3wt%, and then the waste particles are immersed in a microbial pool for 25 days, and solid-liquid separation is performed to obtain a filtrate and a residue;

[0055] The feeding ratio of the waste particles is 150g / L;

[0056] The microorganisms in the microorganism pool include thermophilic sulfur oxidizing bacteria, thermophilic bifidobacterium and thermophilic sulfur bacteria;

[0057] The concentration of the thermophilic sulfur oxidizing bacillus is 20×10 6 cell / ml;

[0058] The concentration of the thermophilic bifidobacterium is 15×10 6 cell / ml;

[0059] The concentration of the thermophilic thiobacillus is 25×10 6 cell / ml;

[0060] The microbial pool also contains glycerol and glutathione;

[0061] The mass concentration of the glycerol is 9%;

[0062] The mass concentration of glutathione is 4%;

[0063] The pH of the microbial pool is 3.0;

[0064] The temperature of the microbial pool is 45°C;

[0065] W2. The resulting filtrate was extracted with a copper extractant Lix984 to obtain a copper raffinate and a copper-containing organic phase;

[0066] W3. adding a sulfuric acid solution at a concentration of 190 g / L as a copper stripping agent to the copper-containing organic phase to obtain a copper-containing stripping solution; electrolyzing the copper-containing stripping solution to obtain copper at the cathode;

[0067] W4. A nickel extractant HBL110 was added to the copper raffinate for extraction to obtain a nickel raffinate and a nickel-containing organic phase;

[0068] W5. In the nickel-containing organic phase, a sulfuric acid solution was added at a concentration of 75g / L as a nickel stripping agent to obtain a nickel-containing stripping solution;

[0069] W6. Electrolysis is carried out using the nickel-containing stripping solution as the electrolyte to obtain nickel at the cathode.

[0070] The electrolyte of the electrolytic treatment described in step W3 and step W6 contains dodecylbenzenesulfonic acid, polyethylene glycol and EDTA, and the dodecylbenzenesulfonic acid, polyethylene glycol and EDTA account for 17% of the electrolyte mass.

[0071] The mass ratio of dodecylbenzenesulfonic acid, polyethylene glycol and EDTA is 22:9:17.

[0072] Example 3

[0073] A method for recovering copper-nickel from waste materials comprises the following steps:

[0074] W1. The waste is crushed to obtain waste particles, wherein the copper content of the waste particles is ≥5wt%, and the nickel content is ≥3wt%, and then the waste particles are immersed in a microbial pool for 30 days, and solid-liquid separation is performed to obtain a filtrate and a residue;

[0075] The feeding ratio of the waste particles is 200g / L;

[0076] The microorganisms in the microorganism pool include thermophilic sulfur oxidizing bacteria, thermophilic bifidobacterium and thermophilic sulfur bacteria;

[0077] The concentration of the thermophilic sulfur oxidizing bacillus is 25×10 6 cell / ml;

[0078] The concentration of the thermophilic bifidobacterium is 20×10 6 cell / ml;

[0079] The concentration of the thermophilic thiobacillus is 30×10 6 cell / ml;

[0080] The microbial pool also contains glycerol and glutathione;

[0081] The mass concentration of the glycerol is 10%;

[0082] The mass concentration of glutathione is 5%;

[0083] The pH of the microbial pool is 4.0;

[0084] The temperature of the microbial pool is 50°C;

[0085] W2. The resulting filtrate was extracted with a copper extractant Lix984 to obtain a copper raffinate and a copper-containing organic phase;

[0086] W3. adding a sulfuric acid solution at a concentration of 190 g / L as a copper stripping agent to the copper-containing organic phase to obtain a copper-containing stripping solution; electrolyzing the copper-containing stripping solution to obtain copper at the cathode;

[0087] W4. A nickel extractant HBL110 was added to the copper raffinate for extraction to obtain a nickel raffinate and a nickel-containing organic phase;

[0088] W5. In the nickel-containing organic phase, a sulfuric acid solution was added at a concentration of 75g / L as a nickel stripping agent to obtain a nickel-containing stripping solution;

[0089] W6. Electrolysis is carried out using the nickel-containing stripping solution as the electrolyte to obtain nickel at the cathode.

[0090] The electrolyte of the electrolytic treatment described in step W3 and step W6 contains dodecylbenzenesulfonic acid, polyethylene glycol and EDTA, and the dodecylbenzenesulfonic acid, polyethylene glycol and EDTA account for 20% of the mass of the electrolyte.

[0091] The mass ratio of dodecylbenzenesulfonic acid, polyethylene glycol and EDTA is 25:10:20.

[0092] Comparative Example 1

[0093] The biological pond leaching was replaced by 98% sulfuric acid leaching, and the sulfuric acid was replaced every 5 days. The remaining operations were carried out in accordance with Example 3.

[0094] Comparative Example 2

[0095] The microorganisms in the microbial pool are thermophilic sulfur oxidizing bacteria and thermophilic bifidobacterium. The concentration of thermophilic sulfur oxidizing bacteria is 40×10 6 cell / ml; the concentration of the thermophilic bifidobacterium is 35×10 6 cell / ml; the rest of the operations refer to Example 3.

[0096] Comparative Example 3

[0097] The microorganisms in the microbial pool are thermophilic sulfur oxidizing sulfur bacillus and thermophilic sulfur bacillus. The concentration of thermophilic sulfur oxidizing sulfur bacillus is 35×10 6 cell / ml; the concentration of the thermophilic sulfur bacillus is 40×10 6 cell / ml. The rest of the operations refer to Example 3.

[0098] Comparative Example 4

[0099] The microorganisms in the microbial pool are thermophilic bifidobacterium and thermophilic thiobacterium. The concentration of the thermophilic bifidobacterium is 35×10 6 cell / ml; the concentration of the thermophilic sulfur bacillus is 40×10 6 cell / ml. The rest of the operations refer to Example 3.

[0100] Comparative Example 5

[0101] The microbial pool does not contain glycerol and glutathione, and the remaining operations are the same as those in Example 3.

[0102] Comparative Example 6

[0103] The microbial pool does not contain glycerol, the mass concentration of glutathione is 11%, and the remaining operations are referred to Example 3.

[0104] Comparative Example 7

[0105] The microbial pool does not contain glutathione, the mass concentration of glycerol is 11%, and the remaining operations refer to Example 3.

[0106] Comparative Example 8

[0107] The electrolytic cell does not contain dodecylbenzenesulfonic acid and polyethylene glycol, and the remaining operations are the same as those in Example 3.

[0108] Comparative Example 9

[0109] The electrolytic cell does not contain dodecylbenzenesulfonic acid and EDTA, and the remaining operations are the same as those in Example 3.

[0110] Comparative Example 10

[0111] The electrolytic cell does not contain polyethylene glycol or EDTA, and the remaining operations are the same as those in Example 3.

[0112] Comparative Example 11

[0113] The electrolytic cell does not contain dodecylbenzenesulfonic acid, polyethylene glycol, or EDTA, and the remaining operations are the same as those in Example 3.

[0114] Performance Testing

[0115] 1.0 kg of waste samples were accurately weighed as the waste raw materials of Examples 1 to 3 and Comparative Examples 1 to 11, and the copper and nickel contents were determined according to the test method described in HJ766-2015; the copper and nickel precipitated at the cathode were accurately weighed, and their yields were calculated and recorded as shown in Table 1.

[0116] Table 1

[0117]

[0118]

[0119] As can be seen from Table 1, the copper and nickel yield of Comparative Example 1, which uses sulfuric acid instead of microbial pool soaking, is slightly lower than that of Examples 1 to 3;

[0120] The copper and nickel yields of Comparative Examples 2 to 4, in which the microorganisms in the microorganism pool are any two of Thermosulfur Sulfobacillus, Thermobifidobacterium and Thermothiobacterium, are significantly lower than those of Examples 1 to 3;

[0121] The copper-nickel yields of Comparative Examples 5 to 7, which contained no or only any one of glycerol and glutathione in the microbial pool, were significantly lower than those of Examples 1 to 3, and the copper-nickel yields of Comparative Example 5, which contained no glycerol and glutathione, were lower than those of Comparative Examples 6 and 7, which contained only any one of glycerol or glutathione.

[0122] The copper-nickel yield of Comparative Examples 8 to 11 in which the electrolytic cell does not contain or contains only any two of dodecylbenzenesulfonic acid, polyethylene glycol, and EDTA is lower than that of Examples 1 to 3, and the copper-nickel yield of Comparative Example 11 in which do not contain dodecylbenzenesulfonic acid, polyethylene glycol, and EDTA is lower than that of Comparative Examples 8 to 10 in which only any two of dodecylbenzenesulfonic acid, polyethylene glycol, and EDTA are contained.

[0123] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for recovering copper and nickel from waste materials, characterized in that: The following steps are involved: W1. crushing the waste to obtain waste particles, and then soaking the waste particles in a microbial pool for 20 to 30 days, and performing solid-liquid separation to obtain a filtrate and a filter residue; W2. The resulting filtrate was extracted with a copper extractant Lix984 to obtain a copper raffinate and a copper-containing organic phase; W3. adding a sulfuric acid solution at a concentration of 190 g / L as a copper stripping agent to the copper-containing organic phase to obtain a copper-containing stripping solution; electrolyzing the copper-containing stripping solution to obtain copper at the cathode; W4. A nickel extractant HBL110 was added to the copper raffinate for extraction to obtain a nickel raffinate and a nickel-containing organic phase; W5. In the nickel-containing organic phase, a sulfuric acid solution was added at a concentration of 75g / L as a nickel stripping agent to obtain a nickel-containing stripping solution; W6. Electrolysis is performed using a nickel-containing stripping solution as an electrolyte to obtain nickel at the cathode; The microorganisms in the microorganism pool described in step W1 include thermophilic sulfur oxidizing sulfur bacteria, thermophilic bifidobacterium and thermophilic sulfur bacteria; The concentration of the thermophilic sulfur oxidizing bacillus is 15 to 25×10 6 cell / ml; The concentration of the thermophilic bifidobacterium is 10 to 20×10 6 cell / ml; The concentration of the thermophilic thiobacillus is 20 to 30×10 6 cell / ml; The microbial pool also contains glycerol and glutathione; The mass concentration of the glycerol is 3-5%; The mass concentration of glutathione is 1-3%; The electrolyte of the electrolytic treatment described in step W3 and step W6 contains dodecylbenzenesulfonic acid, polyethylene glycol and EDTA, and the dodecylbenzenesulfonic acid, polyethylene glycol and EDTA account for 15-20% of the mass of the electrolyte; The mass ratio of dodecylbenzenesulfonic acid, polyethylene glycol and EDTA is 20-25:8-10:15-20.

2. A method for recovering copper and nickel from waste materials according to claim 1, characterized in that: The feed ratio of the waste particles described in step W1 is 100-200 g / L.

3. A method for recovering copper and nickel from waste materials according to claim 1, characterized in that: The pH of the microbial pool described in step W1 is 1.0-4.

0.

4. A method for recovering copper and nickel from waste materials according to claim 1, characterized in that: The temperature of the microbial pool described in step W1 is 40-50°C.