A water-resistant and weather-resistant polymer composite film for waterproofing roll and its preparation process

The combination of polysiloxane copolymer and lanthanum stabilizer solves the problem of decomposition of polyvinyl chloride under the action of light and heat, significantly improves its thermal stability and weather resistance, enhances waterproof and water-resistant properties, and is suitable for waterproofing roll material.

CN118256016BActive Publication Date: 2024-10-11ALPHA NEW MATERIALS JIANGSU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410243478.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-04
Publication Date
2024-10-11
Estimated Expiration
2044-03-04

AI Technical Summary

Technical Problem

Polyvinyl chloride decomposes under the action of light and heat to produce hydrogen chloride, which results in poor thermal stability and weather resistance, affecting its application in waterproofing membranes.

Method used

Adopting a preparation process, N,N-dimethylformamide, 4,4'-methylene bis(phenyl isocyanate) and amino-terminated polysiloxane and 2-(pyridinedicarboxylic acid)-4 , the copolymerization reaction of 6-diamino-s-triazine to form a polysiloxane copolymer, and combined with lanthanum nitrate to form a polysiloxane copolymer-lanthanum stabilizer to improve the thermal stability and water-resistant and waterproof properties of polyvinyl chloride .

Benefits of technology

It improves the thermal stability and weather resistance of the polyvinyl chloride composite film, extends the thermal stability time, enhances the tensile properties and hydrophobicity, and significantly improves the waterproof and water-resistant properties, making it more widely used in waterproof membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256016B_ABST
    Figure CN118256016B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polyvinyl chloride, and discloses a water-resistant and weather-resistant polymer composite film and a preparation process for waterproof coiled material. The polysiloxane copolymer of the present invention contains a nitrogen-containing triazine group and a dicarboxyl pyridine structure, which can form a stable coordination effect with lanthanum ions, thereby loading lanthanum ions to the polysiloxane copolymer to form a polysiloxane copolymer-lanthanum stabilizer. At the same time, maleic anhydride grafted polyvinyl chloride and the like are added as a compatibilizer, so that the composite film has a higher thermal stability time and shows excellent thermal stability performance. The composite film has a good toughening and modification effect, and the tensile properties are significantly improved. And the thermal stability and weather resistance of the composite film are excellent, the hydrophobicity is high, and the waterproof and water-resistant performance are better. Make the polyvinyl chloride-based polymer composite film have more practical applications in waterproof coiled material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyvinyl chloride, in particular to a water-resistant and weather-resistant polymer composite film used for waterproof coiled materials and a preparation process thereof. Background Art

[0002] Polyvinyl chloride has the advantages of low cost, excellent flame retardancy, and good chemical resistance. It is widely used in waterproof coils, packaging films, plastic bottles, and transportation pipelines. However, polyvinyl chloride has poor thermal stability and weather resistance. Under the action of light, heat, etc., it will decompose to produce hydrogen chloride, and the produced hydrogen chloride will further accelerate the decomposition of polyvinyl chloride, resulting in discoloration, mechanical properties, and reduced service life. Compared with traditional calcium zinc stabilizers and lead salt stabilizers, rare earth stabilizers such as lanthanum have the advantages of low toxicity, good stability, and diverse preparation methods, and have broad development prospects. Patent CN114196135B discloses a preparation of ultrasonic radiation calcium and lanthanum-based polyvinyl chloride polymer heat stabilizers and their application in soft products. Calcium and lanthanum-based metal oxides are blended and modified by bonding with PVC to obtain calcium and lanthanum-based polyvinyl chloride polymer heat stabilizers, which can improve the heat resistance and stability of the polymer and improve the compatibility of the blend with polyvinyl chloride. However, the patent does not further improve the water resistance, waterproofness, and mechanical properties of polyvinyl chloride. It is not conducive to the practical application of polyvinyl chloride in waterproof membranes. Summary of the invention

[0003] Technical problems solved: Improved the weather resistance, thermal stability and water resistance of polyvinyl chloride-based polymer film materials.

[0004] Technical solution:

[0005] A preparation process of a water-resistant and weather-resistant polymer composite film:

[0006] (1) Add N,N-dimethylformamide and 4,4'-methylenebis(phenyl isocyanate) into a reaction flask, raise the temperature to 65-75°C, dropwise add N,N-dimethylformamide solution containing amino-terminated polysiloxane and 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine, control the dropping time to 30-60 minutes, react for 2-4 hours, remove N,N-dimethylformamide by vacuum distillation, wash the product with acetone, and dry to obtain a polysiloxane copolymer.

[0007] (2) adding ethanol and polysiloxane copolymer into a reaction kettle, mixing well, and then adding an ethanol solution containing lanthanum nitrate. After the reaction, the ethanol is concentrated to remove the ethanol, thereby obtaining a polysiloxane copolymer-lanthanum stabilizer.

[0008] (3) 50-75 parts by weight of polyvinyl chloride, 14-20 parts by weight of plasticizer, 0.2-0.5 parts by weight of antioxidant, 5-15 parts by weight of filler, 0.4-2 parts by weight of compatibilizer, and 2-10 parts by weight of polysiloxane copolymer-lanthanum stabilizer are added into a mixer and mixed evenly, then placed in a double-roll open mill for mixing, and finally filmed by a two-roll calender to obtain a water-resistant and weather-resistant polymer composite film.

[0009] Wherein, the filler is calcium carbonate, montmorillonite or diatomaceous earth.

[0010] The compatibilizer is maleic anhydride grafted polyvinyl chloride, maleic anhydride grafted chlorinated polyvinyl chloride, and maleic anhydride grafted polyethylene wax.

[0011] The weights of (1) mid-terminal amino polysiloxane and 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine are 160-220% and 42-60% of the weight of 4,4'-methylenebis(phenyl isocyanate), respectively.

[0012] The mass of lanthanum nitrate in (2) is 4-12% of the mass of the polysiloxane copolymer.

[0013] Wherein, in (2), the reaction temperature is controlled at 60-85°C and the reaction time is 6-12h.

[0014] The preparation process of 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine in (2) is as follows:

[0015] Add 1,4-dioxane solvent, 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester and 2-chloro-4,6-diamino-1,3,5-triazine into a reaction flask, wherein the mass of 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester is 145-170% of the mass of 2-chloro-4,6-diamino-1,3,5-triazine; introduce nitrogen and heat to 100-105° C., reflux for reaction for 18-24 hours, concentrate the solvent, wash the crude product with petroleum ether, add it into methanol, add potassium hydroxide, heat to 35-45° C., react for 4-10 hours, then add potassium hydroxide, continue to react for 6-12 hours, cool, add hydrochloric acid solution to the solution to adjust the pH to 3-4, then concentrate the solvent, add water and ethyl acetate, extract and separate, dry the organic phase to remove water, and concentrate to remove ethyl acetate to obtain 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine.

[0016] Among them, water-resistant and weather-resistant polymer composite films are used in waterproof membranes.

[0017] Technical effect: The present invention utilizes 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester and 2-chloro-4,6-diamino-1,3,5-triazine for substitution and hydrolysis reaction to obtain 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine, and then copolymerizes with 4,4'-methylenebis(phenyl isocyanate) and amino-terminated polysiloxane to obtain a novel polysiloxane copolymer.

[0018] The polysiloxane copolymer of the present invention contains nitrogen-containing triazine groups and dicarboxyl pyridine structures, which can form a stable coordination with lanthanum ions, thereby loading lanthanum ions into the polysiloxane copolymer to form a polysiloxane copolymer-lanthanum stabilizer. At the same time, maleic anhydride grafted polyvinyl chloride and the like are added as a compatibilizer, and the anhydride groups contained therein can react with the amino groups of the polysiloxane copolymer, thereby improving the compatibility between the polysiloxane copolymer-lanthanum stabilizer and the polyvinyl chloride, so that the lanthanum stabilizer can be evenly distributed in the polyvinyl chloride composite film; at high temperatures, polyvinyl chloride is pyrolyzed to produce hydrogen chloride, which can be captured by the lanthanum ions in the stabilizer, thereby inhibiting hydrogen chloride from accelerating the decomposition of the polyvinyl chloride composite film. In addition, polysiloxane has high heat resistance and a high thermal decomposition temperature, so that the composite film has a higher thermal stability time and exhibits excellent thermal stability performance.

[0019] The polysiloxane copolymer-lanthanum stabilizer of the present invention contains a unique organosiloxane segment, has the advantages of high toughness, good weather resistance, strong hydrophobicity, etc., and the addition of a compatibilizer can improve the compatibility between the polysiloxane copolymer and polyvinyl chloride, so that the polysiloxane copolymer-lanthanum stabilizer has a good toughening and modification effect on the composite film, and the tensile property is significantly improved. In addition, the thermal stability and weather resistance of the composite film are excellent, and the tensile property decreases very little after accelerated thermal aging experiments. At the same time, the water contact angle reaches 116.9-122.4°, the hydrophobicity is high, and the waterproof and water-resistant properties are better. The polyvinyl chloride-based polymer composite film has more practical applications in waterproof coiled materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The invention is a preparation reaction route of 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine.

[0021] Figure 2 The reaction mechanism of the preparation of polysiloxane copolymers DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The CAS number of the dimethyl 4-aminopyridine-2,6-dicarboxylate of the present invention is 150730-41-9.

[0024] 2-Chloro-4,6-diamino-1,3,5-triazine has a CAS number of 3397-62-4.

[0025] The CAS number of 4,4'-methylenebis(phenyl isocyanate) is 101-68-8.

[0026] The structural formula of amino-terminated polysiloxane is:

[0027] Example 1

[0028] (1) Add 40 mL of 1,4-dioxane solvent, 3.2 g of 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester, and 2 g of 2-chloro-4,6-diamino-1,3,5-triazine to a reaction flask, introduce nitrogen and heat to 105° C., reflux for 24 h, concentrate the solvent, wash the crude product with petroleum ether, add it to 100 mL of methanol, add 1.1 g of potassium hydroxide, heat to 45° C., react for 4 h, then add 0.7 g of potassium hydroxide, continue to react for 6 h, cool, add hydrochloric acid solution to the solution to adjust the pH to 3, then concentrate the solvent, add water and ethyl acetate, extract and separate, dry the organic phase to remove water, and concentrate to remove ethyl acetate to obtain 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine.

[0029] (2) Add 100 mL of N,N-dimethylformamide and 5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction flask, raise the temperature to 70°C, dropwise add 100 mL of an N,N-dimethylformamide solution containing 11 g of amino-terminated polysiloxane and 2.1 g of 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine, control the dropping time to 30 min, react for 4 h, remove N,N-dimethylformamide by distillation under reduced pressure, wash the product with acetone, and dry to obtain a polysiloxane copolymer.

[0030] (3) Add 120 mL of ethanol and 10 g of polysiloxane copolymer to the reactor, mix well, add 20 mL of ethanol solution containing 0.4 g of lanthanum nitrate, heat to 85° C. and react for 6 h. After the reaction, concentrate to remove ethanol to obtain a polysiloxane copolymer-lanthanum stabilizer.

[0031] (4) 500 g of polyvinyl chloride, 140 g of plasticizer dioctyl phthalate, 2 g of antioxidant 1076, 150 g of filler calcium carbonate, 20 g of compatibilizer maleic anhydride grafted polyethylene wax, and 20 g of polysiloxane copolymer-lanthanum stabilizer are added to a mixer and mixed at a mixing temperature of 50°C; then placed in a double-roll open mill for mixing at a mixing temperature of 160°C; finally, a film is formed by a two-roll calender to obtain a water-resistant and weather-resistant polymer composite film.

[0032] Example 2

[0033] (1) Add 30 mL of 1,4-dioxane solvent, 2.9 g of 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester, and 2 g of 2-chloro-4,6-diamino-1,3,5-triazine to a reaction flask, introduce nitrogen and heat to 100° C., reflux for 24 h, concentrate the solvent, wash the crude product with petroleum ether, add it to 150 mL of methanol, add 1.1 g of potassium hydroxide, heat to 40° C., react for 10 h, then add 0.7 g of potassium hydroxide, continue to react for 6 h, cool, add hydrochloric acid solution to the solution to adjust the pH to 3, then concentrate the solvent, add water and ethyl acetate, extract and separate, dry the organic phase to remove water, and concentrate to remove ethyl acetate to obtain 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine.

[0034] (2) Add 80 mL of N,N-dimethylformamide and 5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction flask, raise the temperature to 65°C, dropwise add 80 mL of an N,N-dimethylformamide solution containing 10 g of amino-terminated polysiloxane and 2.4 g of 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine, control the dropping time to 60 min, react for 2 h, remove N,N-dimethylformamide by vacuum distillation, wash the product with acetone, and dry to obtain a polysiloxane copolymer.

[0035] (3) Add 180 mL of ethanol and 10 g of polysiloxane copolymer to the reactor, mix well, add 30 mL of ethanol solution containing 0.8 g of lanthanum nitrate, heat to 65° C. and react for 12 h. After the reaction, concentrate to remove ethanol to obtain a polysiloxane copolymer-lanthanum stabilizer.

[0036] (4) 600 g of polyvinyl chloride, 150 g of plasticizer dioctyl phthalate, 5 g of antioxidant 1076, 50 g of filler montmorillonite, 12 g by weight of compatibilizer maleic anhydride grafted chlorinated polyvinyl chloride, and 60 g of polysiloxane copolymer-lanthanum stabilizer are added to a mixer and mixed at a mixing temperature of 50°C, then placed in a double-roll open mill for mixing at a mixing temperature of 160°C; finally, a film is formed by a two-roll calender to obtain a water-resistant and weather-resistant polymer composite film.

[0037] Example 3

[0038] (1) Add 40 mL of 1,4-dioxane solvent, 3.4 g of 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester, and 2 g of 2-chloro-4,6-diamino-1,3,5-triazine to a reaction flask, introduce nitrogen and heat to 100° C., reflux for 24 h, concentrate the solvent, wash the crude product with petroleum ether, add it to 150 mL of methanol, add 1.1 g of potassium hydroxide, heat to 35° C., react for 4 h, then add 0.7 g of potassium hydroxide, continue to react for 12 h, cool, add hydrochloric acid solution to the solution to adjust the pH to 4, then concentrate the solvent, add water and ethyl acetate, extract and separate, dry the organic phase to remove water, and concentrate to remove ethyl acetate to obtain 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine.

[0039] (2) Add 80 mL of N,N-dimethylformamide and 5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction flask, raise the temperature to 75°C, dropwise add 80 mL of an N,N-dimethylformamide solution containing 8 g of amino-terminated polysiloxane and 3 g of 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine, control the dropping time to 60 min, react for 2 h, remove N,N-dimethylformamide by distillation under reduced pressure, wash the product with acetone, and dry to obtain a polysiloxane copolymer.

[0040] (3) Add 180 mL of ethanol and 10 g of polysiloxane copolymer to the reactor, mix well, add 40 mL of ethanol solution containing 1.2 g of lanthanum nitrate, heat to 85° C. and react for 8 h. After the reaction, concentrate to remove ethanol to obtain a polysiloxane copolymer-lanthanum stabilizer.

[0041] (4) 750 g of polyvinyl chloride, 200 g of plasticizer dioctyl phthalate, 5 g of antioxidant 1076, 50 g of filler diatomaceous earth, 20 g of compatibilizer maleic anhydride grafted polyvinyl chloride, and 100 g of polysiloxane copolymer-lanthanum stabilizer are added to a mixer and mixed at a mixing temperature of 50°C, then placed in a double-roll open mill for mixing at a mixing temperature of 160°C; finally, a film is formed by a two-roll calender to obtain a water-resistant and weather-resistant polymer composite film.

[0042] Comparative Example 1

[0043] 500g of polyvinyl chloride, 140g of plasticizer dioctyl phthalate, 2g of antioxidant 1076, 150g of filler calcium carbonate, and 20g by weight of compatibilizer maleic anhydride grafted polyethylene wax are added into a mixer and mixed evenly at a mixing temperature of 50°C; then placed in a double-roll open mill for mixing at a mixing temperature of 160°C; finally, a film is formed through a two-roll calender to obtain a polymer composite film.

[0044] Comparative Example 2

[0045] 500g of polyvinyl chloride, 140g of plasticizer dioctyl phthalate, 2g of antioxidant 1076, 150g of filler calcium carbonate, 20g of compatibilizer maleic anhydride grafted polyethylene wax, and 20g of polysiloxane copolymer (prepared according to the method of Example 1) are added to a mixer and mixed at a mixing temperature of 50°C; then placed in a double-roll open mill for mixing at a mixing temperature of 160°C; finally, a film is formed by a two-roll calender to obtain a polymer composite film.

[0046] The Congo red method was used to test the thermal stability of the polymer composite film: the composite film was made into a 3mm×3mm sample, placed in a test tube and heated to 190°C, and the Congo red test paper was placed at the mouth of the test tube. The time when the Congo red test paper turned blue was recorded, which was the thermal stability time. The test results are shown in the following table.

[0047]

[0048] The polymer composite film was made into a sample of 80 mm × 10 mm × 4 mm, and the tensile properties were tested according to the method of GB / T 1040.1-2006 at a test speed of 50 mm / min.

[0049] After testing, the thermal stability time of Examples 1-3 reached 33-58min, because the polysiloxane copolymer contains nitrogen-containing triazine groups and dicarboxyl pyridine structures, which can form a stable coordination with lanthanum ions, thereby loading lanthanum ions to the polysiloxane copolymer to form a polysiloxane copolymer-lanthanum stabilizer. At the same time, maleic anhydride grafted polyvinyl chloride and the like are added as compatibilizers, and the anhydride groups contained therein can react with the amino groups of the polysiloxane copolymer, thereby improving the compatibility between the polysiloxane copolymer-lanthanum stabilizer and polyvinyl chloride, so that the lanthanum stabilizer can be evenly distributed in the polyvinyl chloride composite film; at high temperatures, polyvinyl chloride is pyrolyzed to produce hydrogen chloride, which can be captured by the lanthanum ions in the stabilizer, thereby inhibiting hydrogen chloride from accelerating the decomposition of the polyvinyl chloride composite film. And polysiloxane has high heat resistance and a large thermal decomposition temperature, so that the composite film has a higher thermal stability time and exhibits excellent thermal stability.

[0050] Comparative Examples 1 and 2 do not contain lanthanum stabilizer, and the thermal stability time is very low.

[0051] The sample was placed in an accelerated thermal aging test chamber for 240 hours at a thermal aging temperature of 80°C, and then the tensile properties were tested. The test results are shown in the following table.

[0052]

[0053] The water contact angle of the film was tested according to the method of GB / T 30693-2014.

[0054]

[0055] After testing, the tensile strength of the polymer composite membranes of Examples 1-3 reached 26.3-33.9MPa; the elongation at break reached 272.3-362.7%. This is because the added polysiloxane copolymer-lanthanum stabilizer contains a unique organic siloxane segment, which has the advantages of high toughness, good weather resistance, strong hydrophobicity, etc., and the addition of a compatibilizer can improve the compatibility between the polysiloxane copolymer and polyvinyl chloride, so that the polysiloxane copolymer-lanthanum stabilizer has a good toughening and modification effect on the composite membrane, and the tensile properties are significantly improved. In addition, the thermal stability and weather resistance of the composite membrane are excellent, and after accelerated thermal aging experiments, the tensile properties decrease very little.

[0056] At the same time, the water contact angle reaches 116.9-122.4°, with high hydrophobicity and better waterproof and water-resistant properties.

[0057] Comparative Example 1 does not contain polysiloxane copolymer, and the tensile properties of the composite film material are poor. Comparative Example 2 adds polysiloxane copolymer, and the tensile properties of the composite film material are significantly improved, but there is no coordination effect with lanthanum, and no lanthanum stabilizer is contained. After the accelerated aging test, the tensile properties are significantly reduced.

Claims

1. A process for preparing a water-resistant and weather-resistant polymer composite film, characterized in that: The water-resistant and weather-resistant polymer composite film comprises 50-75 parts by weight of polyvinyl chloride, 14-20 parts by weight of plasticizer, 0.2-0.5 parts by weight of antioxidant, 5-15 parts by weight of filler, 0.4-2 parts by weight of compatibilizer, and 2-10 parts by weight of polysiloxane copolymer-lanthanum stabilizer; the preparation process is as follows: (1) Add N,N-dimethylformamide and 4,4'-methylenebis(phenyl isocyanate) into a reaction flask, raise the temperature to 65-75° C., dropwise add N,N-dimethylformamide solution containing amino-terminated polysiloxane and 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine, control the dropping time to 30-60 min, react for 2-4 h, remove N,N-dimethylformamide by vacuum distillation, wash the product with acetone, and dry to obtain a polysiloxane copolymer; (2) adding ethanol and polysiloxane copolymer to a reaction kettle, mixing and then adding an ethanol solution containing lanthanum nitrate, and concentrating and removing ethanol after the reaction to obtain a polysiloxane copolymer-lanthanum stabilizer; (3) adding polyvinyl chloride, plasticizer, antioxidant, filler, compatibilizer, and polysiloxane copolymer-lanthanum stabilizer into a mixer and mixing them evenly, then placing them in a double-roll mill for mixing, and finally forming a film through a two-roll calender to obtain a water-resistant and weather-resistant polymer composite film; The preparation process of 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine in (1) is as follows: Add 1,4-dioxane solvent, 4-aminopyridine-2,6-dicarboxylic acid dimethyl ester, and 2-chloro-4,6-diamino-1,3,5-triazine to a reaction flask, introduce nitrogen and heat to 100-105° C., reflux for 18-24 hours, concentrate the solvent, wash the crude product with petroleum ether, add it to methanol, add potassium hydroxide, heat to 35-45° C., react for 4-10 hours, then add potassium hydroxide, continue to react for 6-12 hours, cool, add hydrochloric acid solution to the solution to adjust the pH to 3-4, then concentrate the solvent, add water and ethyl acetate, extract and separate, dry the organic phase to remove water, and concentrate to remove ethyl acetate to obtain 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine; The mass of the dimethyl 4-aminopyridine-2,6-dicarboxylate is 145-170% of the mass of 2-chloro-4,6-diamino-1,3,5-triazine.

2. The process for preparing the water-resistant and weather-resistant polymer composite film according to claim 1, characterized in that: The filler is calcium carbonate, montmorillonite or diatomaceous earth.

3. The process for preparing the water-resistant and weather-resistant polymer composite film according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polyvinyl chloride, maleic anhydride grafted chlorinated polyvinyl chloride, and maleic anhydride grafted polyethylene wax.

4. The process for preparing the water-resistant and weather-resistant polymer composite film according to claim 1, characterized in that: The masses of the (1) mid-terminal amino polysiloxane and 2-(pyridinedicarboxylic acid)-4,6-diamino-s-triazine are 160-220% and 42-60% of the mass of 4,4'-methylenebis(phenyl isocyanate), respectively.

5. The process for preparing the water-resistant and weather-resistant polymer composite film according to claim 1, characterized in that: The mass of lanthanum nitrate in (2) is 4-12% of the mass of the polysiloxane copolymer.

6. The process for preparing the water-resistant and weather-resistant polymer composite film according to claim 1, characterized in that: In the step (2), the reaction temperature is controlled to be 60-85°C and the reaction time is 6-12h.

7. Use of the water-resistant and weather-resistant polymer composite film obtained by the preparation process according to any one of claims 1 to 6 in waterproof roll materials.