A preparation process of high temperature resistant silicone rubber composite material
Cross-chain silicone rubber composites were prepared by mixing branched polysiloxanes, organosilicon polymers and other raw materials and curing them under vacuum with ultraviolet light. This solved the problem of insufficient tear resistance of silicone rubber at high temperatures and improved its heat resistance and tear resistance.
Patent Information
- Application Number
- CN202410549884.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-06
AI Technical Summary
Existing silicone rubber materials exhibit reduced tear strength at high temperatures, failing to meet the mechanical properties and weather resistance requirements of extreme environments.
A cross-chain structured silicone rubber composite material was prepared by mixing branched polysiloxane, organosilicon polymer, tetramethylammonium, triarylsiloxane and silica fiber, and then curing and kneading it under vacuum.
It improves tear resistance and heat resistance at high temperatures, reduces the brittleness of the material, and meets the requirements for use in extreme environments.
Smart Images

Figure GDA0005050315360000041 
Figure GDA0005050315360000042 
Figure GDA0005050315360000052
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicone rubber composite materials, and in particular relates to a preparation process of a high-temperature resistant silicone rubber composite material. Background Art
[0002] Silicone rubber is a typical semi-inorganic and semi-organic polymer material with a -Si-O- repeating structure as the main chain and organic groups such as methyl, ethyl and vinyl as the side chains. The main chain is an inorganic structure and the side chain is an organic group. It has the high temperature resistance of inorganic materials and the flexibility of organic materials. It has the advantages of high and low temperature resistance, weather resistance, low glass transition temperature, flexibility, good elasticity, electrical insulation and biocompatibility. It also has excellent properties such as a wide operating temperature range, small compression permanent deformation and low cost. Therefore, silicone rubber has been widely used in industrial fields such as transportation, chemical industry, medical and health care, construction and electronic appliances. It also has important applications in cutting-edge technology fields such as aviation and rockets. Although silicon materials have many advantages and can be applied to many fields, they still have deficiencies in oil resistance, solvent resistance, acid and alkali resistance, steam resistance, mechanical properties and mechanical strength, especially tensile strength and tear strength, which seriously limits their practical application. For example: under the influence of environmental factors such as pressure vessels in chemical applications, high temperature and high pressure workshops, and daily durable products, traditional silicone rubber materials cannot simultaneously meet the mechanical properties, high temperature resistance, weather resistance and tear resistance requirements of these relatively extreme environments. Therefore, it is necessary to carry out certain physical and chemical modifications on the silicone rubber material to further improve its various properties. The large steric hindered group is introduced into the main chain of the silicone rubber, and the adjacent groups are shielded from each other, which can improve the stability of the group, inhibit the cyclization degradation reaction, and improve the heat resistance of the silicone rubber. By introducing benzene rings, improving the performance of silicone rubber has been widely used. Chinese patent application CN202310432021.X is a kind of high tear resistance and high temperature resistant organic silicone rubber and its preparation method, which adopts the preparation method of introducing bisphenol fluorene structure into silicone rubber, but bisphenol fluorene is basically imported and expensive, and is a toxic and polluting substance, so the inventor believes that the preparation of high temperature resistant composite materials needs to find an auxiliary agent to replace bisphenol fluorene, and play at least the same technical effect as adding bisphenol fluorene. Summary of the invention
[0003] The purpose of the present invention is to provide a preparation process of a high temperature resistant silicone rubber composite material in view of the problem that the tear strength of silicone rubber decreases at high temperatures in the prior art.
[0004] To achieve the above purpose, the specific plan is as follows: A preparation process for a high-temperature resistant silicone rubber composite material, specifically: branched polysiloxane, silicone polymer, tetramethylammonium, triaryl siloxane, and silica fiber are mixed evenly, added into a container and heated to 150-180°C while evacuating, in a vacuum environment, cured with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain a silicone rubber composite material.
[0005] Preferably, the branched polysiloxane is a mixture of hydroxyl-terminated polydimethyl-co-methylvinylsiloxane and hydroxyl-terminated polymethylphenylsiloxane.
[0006] In the present invention, the weight ratio of the hydroxyl-terminated polydimethyl-co-methylvinylsiloxane to the hydroxyl-terminated polymethylphenylsiloxane is 1:20-30.
[0007] The present invention is further preferred, and the preparation method of the organosilicon polymer is: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, irradiated with ultraviolet light for reaction, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, the reaction is carried out at 80-90°C for 60-80min, and the solvent is distilled off to obtain an organosilicon polymer.
[0008] It is further preferred that the mixture of ethanol and ether comprises ethanol in a volume ratio of 1-3 and ether in a volume ratio of 6-9.
[0009] In the present invention, the weight ratio of vinylphenyl cyclosiloxane to methyltrifluoropropyl cyclosiloxane is 8-20:1.
[0010] In the present invention, the weight ratio of the mixture of vinylphenyl cyclosiloxane and methyltrifluoropropyl cyclosiloxane to the mixed solution (mixture of ethanol and diethyl ether) is 2-5:1.
[0011] In the present invention, the weight ratio of the 1,3-butadiene to the mixed solution (mixed solution of ethanol and diethyl ether) is 1:20-30.
[0012] In the present invention, the ultraviolet light irradiation intensity is further preferably: 1500-2200LEX.
[0013] In the present invention, the weight ratio of the photoinitiator TPO to the mixed solution (mixture of ethanol and ether) is 1:50-80.
[0014] In the present invention, the weight ratio of the dimer acid to the mixed solution (mixture of ethanol and ether) is 1:40-60.
[0015] In the present invention, the volume ratio of the preliminary polymer to the mixed solution (mixed solution of ethanol and acetone) is 3-6:1.
[0016] The present invention is further preferably composed of 70-80 parts by weight of branched polysiloxane, 10-20 parts by weight of silicone polymer, 1-3 parts by weight of tetramethylammonium, 2-5 parts by weight of triaryl siloxane, 3-6 parts by weight of silica fiber, and 1-3 parts by weight of vulcanizing agent DMDS.
[0017] In the present invention, the silica fiber has a diameter of 3-5 μm and a length of 20-50 μm.
[0018] The difference from the prior art is that the present invention achieves the following technical effects:
[0019] 1. The present invention not only improves the tear strength at high temperature by adding silica fiber and dimer acid, but also the dimer acid is a cross-chain, which effectively improves the network cross-linking of the organic silicone rubber composite material and improves the heat resistance of the material.
[0020] 2. The present invention prepares the organosilicon polymer by using low-intensity ultraviolet light, and then increases the ultraviolet intensity for curing when preparing the composite material, so that the curing stress of the prepared composite material is reduced and the brittleness is reduced.
[0021] 3. The present invention requires strict control of the ratio between the raw materials to achieve the technical effect of high tear strength at high temperature. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Part I:
[0024] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer A.
[0025] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0026] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0027] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0028] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0029] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0030] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0031] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0032] Weigh the raw materials according to the following weight parts:
[0033]
[0034] The branched polysiloxane, silicone polymer A, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 1-5.
[0035] Part II:
[0036] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1800LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer B.
[0037] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0038] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 15:1.
[0039] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0040] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0041] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0042] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0043] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 3:1.
[0044] Weigh the raw materials according to the following weight parts:
[0045]
[0046]
[0047] The branched polysiloxane, silicone polymer B, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added for vacuum kneading for 10-50 minutes to obtain the silicone rubber composite materials of Examples 6-10.
[0048] Part III:
[0049] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 2200LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer C.
[0050] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0051] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 20:1.
[0052] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0053] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0054] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0055] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0056] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 6:1.
[0057] Weigh the raw materials according to the following weight parts:
[0058]
[0059] The branched polysiloxane, silicone polymer C, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 11-15.
[0060] Part 4:
[0061] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 2300LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer D.
[0062] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0063] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 8:1.
[0064] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0065] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0066] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0067] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0068] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0069] Weigh the raw materials according to the following weight parts:
[0070]
[0071] The branched polysiloxane, silicone polymer D, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added for vacuum kneading for 10-50 minutes to obtain the silicone rubber composite materials of Examples 16-20.
[0072] Part V:
[0073] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer E.
[0074] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0075] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 5:1.
[0076] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0077] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0078] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0079] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0080] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0081] Weigh the raw materials according to the following weight parts:
[0082]
[0083] The branched polysiloxane, silicone polymer E, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 21-25.
[0084] Part VI:
[0085] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer F.
[0086] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0087] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0088] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:2.
[0089] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0090] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0091] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0092] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0093] Weigh the raw materials according to the following weight parts:
[0094]
[0095] The branched polysiloxane, silicone polymer F, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added for vacuum kneading for 10-50 minutes to obtain the silicone rubber composite materials of Examples 26-30.
[0096] Part VII:
[0097] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer G.
[0098] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0099] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0100] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0101] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:10.
[0102] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0103] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0104] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0105] Weigh the raw materials according to the following weight parts:
[0106]
[0107] The branched polysiloxane, silicone polymer G, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added for vacuum kneading for 10-50 minutes to obtain the silicone rubber composite materials of Examples 31-35.
[0108] Part 8:
[0109] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1200LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer H.
[0110] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0111] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0112] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0113] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0114] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0115] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0116] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0117] Weigh the raw materials according to the following weight parts:
[0118]
[0119] The branched polysiloxane, silicone polymer H, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under ultraviolet light of 3600-4000lex intensity for 3-10 minutes in a vacuum environment, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 36-40.
[0120] Part IX:
[0121] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer I.
[0122] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0123] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0124] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0125] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0126] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:40.
[0127] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0128] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0129] Weigh the raw materials according to the following weight parts:
[0130]
[0131]
[0132] The branched polysiloxane, silicone polymer I, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under ultraviolet light of 3600-4000lex intensity for 3-10 minutes in a vacuum environment, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 41-45.
[0133] Part 10:
[0134] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer J.
[0135] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0136] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0137] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0138] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0139] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:85.
[0140] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0141] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0142] Weigh the raw materials according to the following weight parts:
[0143]
[0144] The branched polysiloxane, silicone polymer J, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 46-50.
[0145] Part 11:
[0146] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer K.
[0147] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0148] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0149] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0150] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0151] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:85.
[0152] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0153] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 4:1.
[0154] Weigh the raw materials according to the following weight parts:
[0155]
[0156] The branched polysiloxane, silicone polymer K, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 51-55.
[0157] Part 12:
[0158] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer L.
[0159] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0160] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0161] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0162] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0163] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0164] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0165] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 2:1.
[0166] Weigh the raw materials according to the following weight parts:
[0167]
[0168] The branched polysiloxane, silicone polymer L, tetramethylammonium, triaryl siloxane and silica fiber are mixed evenly, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3600-4000lex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added and vacuum kneaded for 10-50 minutes to obtain the silicone rubber composite materials of Examples 56-60.
[0169] Part 13:
[0170] Preparation of silicone polymer: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixture of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light at an intensity of 1500LEX is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixture of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain silicone polymer M.
[0171] Wherein: the mixed liquid of ethanol and ether includes a volume ratio of ethanol: ether = 1:4.
[0172] The weight ratio of vinyl phenyl cyclosiloxane to methyl trifluoropropyl cyclosiloxane is 12:1.
[0173] The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid (mixed liquid of ethanol and ether) is 3:1.
[0174] The weight ratio of the 1,3-butadiene to the mixed liquid (a mixed liquid of ethanol and ether) is 1:26.
[0175] The weight ratio of the photoinitiator TPO to the mixed solution (a mixed solution of ethanol and ether) is 1:60.
[0176] The weight ratio of the dimer acid to the mixed solution (a mixed solution of ethanol and ether) is 1:50.
[0177] The volume ratio of the preliminary polymer to the mixed solution (a mixed solution of ethanol and acetone) is 7:1.
[0178] Weigh the raw materials according to the following weight parts:
[0179]
[0180] Mix branched polysiloxane, silicone polymer M, tetramethylammonium, triaryl siloxane and silica fiber evenly, add into a container, heat to 150-180°C and evacuate at the same time, cure with ultraviolet light of 3600-4000lex intensity for 3-10min in a vacuum environment, then cool to 130-150°C, add vulcanizing agent and perform vacuum kneading for 10-50min to obtain the silicone rubber composite materials of Examples 61-65.
[0181] The organic silicon rubber composite materials prepared in Examples 1 to 65 were processed in accordance with a unified standard to obtain a thin layer with a thickness of 1.5 mm. The thin layer was tested for tear resistance and tensile strength at room temperature and 90° C. The test standard was based on ASTM D624. The results are as follows:
[0182]
[0183]
[0184]
[0185] According to the test results of the above examples, the raw material formula and preparation process of the organic silicon polymer have a great influence on the performance of the composite material. The organic silicon polymers prepared within the protection scope of the present invention in Examples 1-20 have the best performance for the composite material prepared therefrom.
[0186] Compared with Example 1, Example 66 has the same raw materials, except that the intensity of ultraviolet light is reduced when preparing the silicone composite material. Specifically, the branched polysiloxane, silicone polymer A, tetramethylammonium, triaryl siloxane, and silica fiber are evenly mixed, added into a container, heated to 150-180°C and evacuated at the same time, cured under a vacuum environment with ultraviolet light of 3000ex intensity for 3-10 minutes, then cooled to 130-150°C, and a vulcanizing agent is added for vacuum kneading for 10-50 minutes to obtain the silicone rubber composite material of Example 66.
[0187] Compared with Example 36, Example 67 has the same raw materials for the organic silicon polymer, but is prepared at an ultraviolet intensity of 3000LEX, and then the silicone rubber composite material is prepared using the same raw materials as in Example 36.
[0188] The materials of Examples 66 and 67 were tested and the structures were as follows:
[0189]
[0190] The data show that the UV intensity in the preparation process of the silicone polymer cannot be higher than the range of the present invention, while the processing of the silicone rubber material always requires a UV intensity of 3000-3600LEX.
[0191] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the claims of the present invention.
Claims
1. A method for preparing a high thermal conductivity organic silicone rubber composite material, specifically: branched polysiloxane, organic silicon polymer, tetramethyl ammonium, triaryl siloxane, and silicon dioxide fiber are uniformly mixed, added into a container, heated to 150-180° C., and evacuated at the same time, cured for 3-10 minutes under a vacuum environment with ultraviolet light of 3600-4000lex intensity, then cooled to 130-150° C., and a vulcanizing agent is added for vacuum kneading for 10-50 minutes to obtain an organic silicone rubber composite material; 70-80 parts by weight of branched polysiloxane, 10-20 parts by weight of organic silicon polymer, 1-3 parts by weight of tetramethyl ammonium, 2-5 parts by weight of triaryl siloxane, 3-6 parts by weight of silicon dioxide fiber, and 1-3 parts by weight of a vulcanizing agent DMDS; the branched polysiloxane is a mixture of hydroxyl-terminated polydimethyl-co-methylvinylsiloxane and hydroxyl-terminated polymethylphenylsiloxane; the hydroxyl-terminated polydimethyl-co- -The weight ratio of methyl vinyl siloxane and hydroxyl-terminated polymethylphenyl siloxane is 1:20-30; the preparation method of the silicone polymer is as follows: in a helium environment, vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane are dissolved in a mixed solution of ethanol and ether, 1,3-butadiene and photoinitiator TPO are added and stirred evenly, ultraviolet light is irradiated to react, and ethanol and ether are distilled off to obtain a preliminary polymer; in a helium environment, the preliminary polymer is dissolved in a mixed solution of ethanol and acetone, dimer acid is added, and the reaction is carried out at 80-90°C for 60-80 minutes, and the solvent is distilled off to obtain an silicone polymer; the mixed solution of ethanol and ether includes 1 volume ratio of ethanol and 4 volume ratios of ether; the weight ratio of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane is 8-20:1; the ultraviolet light irradiation intensity is: 1500-2200LEX; the volume ratio of the preliminary polymer to the mixed solution of ethanol and acetone is 3-6:1; The weight ratio of the mixture of vinyl phenyl cyclosiloxane and methyl trifluoropropyl cyclosiloxane to the mixed liquid of ethanol and diethyl ether is 3:1; the weight ratio of 1,3-butadiene to the mixed liquid of ethanol and diethyl ether is 1:26; the weight ratio of the photoinitiator TPO to the mixed liquid of ethanol and diethyl ether is 1:60; the weight ratio of the dimer acid to the mixed liquid of ethanol and diethyl ether is 1:
50.
2. The method for preparing the high thermal conductivity organic silicon rubber composite material according to claim 1, characterized in that: The silica fiber has a diameter of 3-5 μm and a length of 20-50 μm.