A kind of quick-drying water-based ink and preparation method thereof

CN118271900BActive Publication Date: 2024-11-19YUEYANG JINGWEI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410492360.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-11-19
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

然而,水性油墨的主要限制在于其干燥速度通常较慢,这在高速印刷操作中可能导致生产效率降低,影响整体工作流程

Benefits of technology

[0020] The quick-drying water-based ink proposed by the present invention significantly reduces the emission of volatile organic compounds (VOCs) by using environmentally friendly materials such as water-based polyurethane resin and biomass nanofibers, making the ink environmentally friendly and providing safer conditions for operators. working environment. Secondly, ethanol and zinc oxide quantum dots are added to the formula of the ink. These ingredients help speed up the evaporation of water and other solvents and improve the drying speed of the ink. Among them, zinc oxide quantum dots have quantum confinement properties, catalytic ability, and can It accelerates the chemical drying process to a certain extent, especially under light conditions, and effectively meets the demand for quick drying in the printing process. In addition, biomass nanofibers accelerate water evaporation and improve the rheological properties of the ink through their high surface area and excellent water absorption properties, making it easier for the ink layer to form a uniform thin layer and dry quickly. At the same time, these nanofibers also enhance the structure of the ink. Stability, preventing cracks or morphological instability during drying, thereby increasing production efficiency and reducing overall workflow time. Generally speaking, the quick-drying water-based ink of the present invention is a new type of ink that is efficient, environmentally friendly and has superior performance, and is suitable for wide application in the modern printing industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118271900B_ABST
    Figure CN118271900B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of printing ink, and specifically provides a quick-drying water-based ink and a preparation method thereof, wherein the water-based ink comprises the following raw materials in parts by weight: 30-40 parts of water-based polyurethane resin, 10-20 parts of methyl methacrylate, 0-8 parts of water-based pigment, 2-4 parts of zinc oxide quantum dots, 2-4 parts of biomass nanofibers, 0.5-0.8 parts of sodium dodecylbenzene sulfonate, 1-1.5 parts of polydimethylsiloxane, 5-7 parts of ethanol, and 15-20 parts of water. The present invention mixes the water-based polyurethane resin with the biomass nanofibers, and simultaneously adds zinc oxide quantum dots with catalytic properties, which can effectively improve the drying speed of the water-based ink while reducing volatile toxic components, and can also improve the structural integrity of the water-based ink, thereby improving the use performance of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printing inks, and in particular to a quick-drying water-based ink and a preparation method thereof. Background Art

[0002] In the printing industry, the drying speed and environmental properties of inks are key factors in determining the wide application and market acceptance of products. Especially at a time when high-speed printing technology is widely used, fast drying can significantly improve production efficiency and reduce waiting time. However, although traditionally used solvent-based inks have advantages in drying speed, they contain a large amount of volatile organic compounds (VOCs), which not only cause significant pollution to the environment, but may also pose a threat to the health of operators. Therefore, although solvent-based inks still have a place in some high-speed printing fields, their environmental and health issues are in urgent need of resolution.

[0003] In response to the above problems, water-based inks have become a popular alternative because they have lower VOC emissions than solvent-based inks and are more friendly to the environment and operators. However, the main limitation of water-based inks is that they usually dry slowly, which may lead to reduced production efficiency in high-speed printing operations and affect the overall workflow. Therefore, it is particularly important to develop a water-based ink that is both environmentally friendly and can dry quickly, which not only meets environmental protection requirements, but also maintains high efficiency in the production process to meet the needs of the rapidly developing printing market. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a quick-drying water-based ink and a preparation method thereof, wherein a water-based polyurethane resin is mixed with biomass nanofibers and zinc oxide quantum dots with catalytic properties are added, thereby reducing volatile toxic components and effectively increasing the drying speed of the water-based ink. At the same time, the structural integrity of the water-based ink can be improved, thereby improving the performance of the product.

[0005] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: The present invention proposes a quick-drying water-based ink, which comprises the following raw materials in parts by weight: 30 to 40 parts of water-based polyurethane resin, 10 to 20 parts of methyl methacrylate, 2 to 6 parts of water-based pigment, 2 to 4 parts of zinc oxide quantum dots, 2 to 4 parts of biomass nanofibers, 0.5 to 0.8 parts of sodium dodecylbenzene sulfonate, 1 to 1.5 parts of polydimethylsiloxane, 5 to 7 parts of ethanol, and 15 to 20 parts of water.

[0006] Preferably, the water-based pigment is any one of titanium dioxide, lemon yellow, phthalocyanine blue, ultrafine carbon black, cobalt green, and iron oxide red.

[0007] Preferably, the method for preparing zinc oxide quantum dots comprises the following steps:

[0008] ① Weigh 10-20 mmol of zinc acetate and dissolve it in 100 mL of ethanol. Stir at 300-400 rpm at room temperature to fully dissolve it to obtain a zinc ion solution.

[0009] ② Add 10 mL of 0.2 mol / L potassium hydroxide ethanol solution dropwise to the zinc ion solution prepared in step ①, stir continuously at 500-600 rpm for 6-8 h, place in a centrifuge at 8000 rpm to remove the supernatant, wash the precipitate twice with ethanol and water alternately, place in a vacuum drying oven at 60° C. and dry for 12 h to obtain zinc oxide quantum dots.

[0010] Preferably, the method for preparing the biomass nanofibers comprises the following steps:

[0011] I. Clean the bamboo with clean water, crush it into powder with a diameter of 1 mm in a crusher, and dry it in a drying oven at 60° C. for 12 h to obtain bamboo powder;

[0012] II. Weigh 2 g of the bamboo powder prepared in step I and put it into a reactor, add 10 mL of 30 wt% hydrogen peroxide solution and 200 mL of 3.2 mol / L nitric acid solution, heat to 40-60 ° C, stir magnetically at 400-500 rpm for 48-60 h, add 1 L of distilled water to terminate the reaction, and obtain a reaction termination solution;

[0013] III. The reaction termination solution prepared in step II was filtered, and the precipitate was washed with distilled water until the filtrate was neutral. The obtained precipitate was redispersed in 100 mL of distilled water, and homogenized using a high-pressure homogenization chamber with a pore size of 87 μm and a homogenization pressure of 1500 bar. The homogenization operation was repeated 4 to 5 times to obtain a product precursor;

[0014] IV. The product precursor prepared in step III was washed three times with distilled water, separated by high-speed centrifugation, and dried in an oven at 40° C. for 24 h to obtain biomass nanofibers.

[0015] The present invention also provides a method for preparing a quick-drying water-based ink, which specifically comprises the following steps:

[0016] S1. Weigh the corresponding weight of raw materials according to the formula and weight parts;

[0017] S2, adding waterborne polyurethane resin, methyl methacrylate, waterborne pigment, zinc oxide quantum dots, biomass nanofibers, ethanol and water into the reactor, and stirring at 300 rpm for 30 min;

[0018] S3. After the stirring in step S2 is completed, sodium dodecylbenzene sulfonate and polydimethylsiloxane are added to the reactor, and stirring is continued at 300 rpm for 40 min to obtain a quick-drying water-based ink.

[0019] The beneficial effects achieved by the present invention are as follows:

[0020] The quick-drying water-based ink proposed by the present invention significantly reduces the emission of volatile organic compounds (VOCs) by adopting environmentally friendly materials such as water-based polyurethane resin and biomass nanofibers, making the ink environmentally friendly and providing a safer working environment for operators. Secondly, ethanol and zinc oxide quantum dots are added to the formula of the ink, and these ingredients help to accelerate the evaporation of water and other solvents and improve the drying speed of the ink; wherein the zinc oxide quantum dots have quantum confinement performance and catalytic ability, and can accelerate the chemical drying process to a certain extent, especially under light conditions, effectively meeting the demand for quick drying in the printing process. In addition, the biomass nanofiber accelerates water evaporation and improves the rheological properties of the ink through its high surface area and excellent water absorption performance, making the ink layer easier to form a uniform thin layer and dry quickly, and these nanofibers also enhance the structural stability of the ink, prevent cracks or unstable morphology during the drying process, thereby improving production efficiency and shortening the time of the overall workflow. In general, the quick-drying water-based ink of the present invention is a new type of ink that is efficient, environmentally friendly and has superior performance, and is suitable for wide application in the modern printing industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 is a transmission electron microscope image of zinc oxide quantum dots prepared in Example 1;

[0023] Figure 2 This is a transmission electron microscope image of the biomass nanofibers prepared in Example 1. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0025] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0026] Example 1: This example proposes a quick-drying water-based ink, which includes the following raw materials in parts by weight: 36 parts of water-based polyurethane resin, 15 parts of methyl methacrylate, 4 parts of titanium dioxide, 3 parts of zinc oxide quantum dots, 3 parts of biomass nanofibers, 0.8 parts of sodium dodecylbenzene sulfonate, 1 part of polydimethylsiloxane, 6 parts of ethanol, and 20 parts of water.

[0027] The method for preparing zinc oxide quantum dots comprises the following steps:

[0028] ① Weigh 16 mmol of zinc acetate and dissolve it in 100 mL of ethanol. Stir at 300 rpm at room temperature to fully dissolve it to obtain a zinc ion solution.

[0029] ② Add 10 mL of 0.2 mol / L potassium hydroxide ethanol solution dropwise to the zinc ion solution prepared in step ①, stir continuously at 500 rpm for 6 h, put it into a centrifuge at 8000 rpm to remove the supernatant, wash the precipitate twice with ethanol and water alternately, put it into a vacuum drying oven at 60°C and dry it for 12 h to obtain zinc oxide quantum dots.

[0030] The method for preparing the biomass nanofibers comprises the following steps:

[0031] I. Clean the bamboo with clean water, crush it into powder with a diameter of 1 mm in a crusher, and dry it in a drying oven at 60° C. for 12 h to obtain bamboo powder;

[0032] II. Weigh 2 g of the bamboo powder prepared in step I and put it into a reactor, add 10 mL of 30 wt% hydrogen peroxide solution and 200 mL of 3.2 mol / L nitric acid solution, heat to 50 ° C, stir magnetically at 450 rpm for 50 h, add 1 L of distilled water to terminate the reaction, and obtain a reaction termination solution;

[0033] III. The reaction termination solution prepared in step II was filtered, and the precipitate was washed with distilled water until the filtrate was neutral. The obtained precipitate was redispersed in 100 mL of distilled water, and homogenized using a high-pressure homogenization chamber with a pore size of 87 μm and a homogenization pressure of 1500 bar. The homogenization operation was repeated 4 times to obtain a product precursor;

[0034] IV. The product precursor prepared in step III was washed three times with distilled water, separated by high-speed centrifugation, and dried in an oven at 40° C. for 24 h to obtain biomass nanofibers.

[0035] This embodiment also provides a method for preparing a quick-drying water-based ink, which specifically comprises the following steps:

[0036] S1. Weigh the corresponding weight of raw materials according to the formula and weight parts;

[0037] S2, adding waterborne polyurethane resin, methyl methacrylate, titanium dioxide, zinc oxide quantum dots, biomass nanofibers, ethanol and water into the reactor, and stirring at 300 rpm for 30 min;

[0038] S3. After the stirring in step S2 is completed, sodium dodecylbenzene sulfonate and polydimethylsiloxane are added to the reactor, and stirring is continued at 300 rpm for 40 min to obtain a quick-drying water-based ink.

[0039] Example 2: This example proposes a quick-drying water-based ink, which includes the following raw materials in parts by weight: 30 parts of water-based polyurethane resin, 20 parts of methyl methacrylate, 2 parts of red iron oxide, 2 parts of zinc oxide quantum dots, 2 parts of biomass nanofibers, 0.6 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polydimethylsiloxane, 5 parts of ethanol, and 18 parts of water.

[0040] The method for preparing zinc oxide quantum dots comprises the following steps:

[0041] ① Weigh 20 mmol of zinc acetate and dissolve it in 100 mL of ethanol. Stir at 400 rpm at room temperature to fully dissolve it to obtain a zinc ion solution.

[0042] ② Add 10 mL of 0.2 mol / L potassium hydroxide ethanol solution dropwise to the zinc ion solution prepared in step ①, stir continuously at 600 rpm for 7 h, put it into a centrifuge at 8000 rpm to remove the supernatant, wash the precipitate twice with ethanol and water alternately, put it into a vacuum drying oven at 60°C and dry it for 12 h to obtain zinc oxide quantum dots.

[0043] The method for preparing the biomass nanofibers comprises the following steps:

[0044] I. Clean the bamboo with clean water, crush it into powder with a diameter of 1 mm in a crusher, and dry it in a drying oven at 60° C. for 12 h to obtain bamboo powder;

[0045] II. Weigh 2 g of the bamboo powder prepared in step I and put it into a reactor, add 10 mL of 30 wt% hydrogen peroxide solution and 200 mL of 3.2 mol / L nitric acid solution, heat to 60 ° C, stir magnetically at 400 rpm for 48 h, add 1 L of distilled water to terminate the reaction, and obtain a reaction termination solution;

[0046] III. The reaction termination solution prepared in step II was filtered, and the precipitate was washed with distilled water until the filtrate was neutral. The obtained precipitate was redispersed in 100 mL of distilled water, and homogenized using a high-pressure homogenization chamber with a pore size of 87 μm and a homogenization pressure of 1500 bar. The homogenization operation was repeated 5 times to obtain a product precursor;

[0047] IV. The product precursor prepared in step III was washed three times with distilled water, separated by high-speed centrifugation, and dried in an oven at 40° C. for 24 h to obtain biomass nanofibers.

[0048] This embodiment also provides a method for preparing a quick-drying water-based ink, which specifically comprises the following steps:

[0049] S1. Weigh the corresponding weight of raw materials according to the formula and weight parts;

[0050] S2, adding waterborne polyurethane resin, methyl methacrylate, red iron oxide, zinc oxide quantum dots, biomass nanofibers, ethanol and water into the reactor, and stirring at 300 rpm for 30 min;

[0051] S3. After the stirring in step S2 is completed, sodium dodecylbenzene sulfonate and polydimethylsiloxane are added to the reactor, and stirring is continued at 300 rpm for 40 min to obtain a quick-drying water-based ink.

[0052] Example 3: This example proposes a quick-drying water-based ink, which includes the following raw materials in parts by weight: 40 parts of water-based polyurethane resin, 10 parts of methyl methacrylate, 6 parts of phthalocyanine blue, 4 parts of zinc oxide quantum dots, 4 parts of biomass nanofibers, 0.5 parts of sodium dodecylbenzene sulfonate, 1.5 parts of polydimethylsiloxane, 7 parts of ethanol, and 15 parts of water.

[0053] The method for preparing zinc oxide quantum dots comprises the following steps:

[0054] ① Weigh 10 mmol of zinc acetate and dissolve it in 100 mL of ethanol. Stir at 350 rpm at room temperature to fully dissolve it to obtain a zinc ion solution.

[0055] ② Add 10 mL of 0.2 mol / L potassium hydroxide ethanol solution dropwise to the zinc ion solution prepared in step ①, stir continuously at 550 rpm for 8 h, put it into a centrifuge at 8000 rpm to remove the supernatant, wash the precipitate twice with ethanol and water alternately, put it into a vacuum drying oven at 60 ° C and dry it for 12 h to obtain zinc oxide quantum dots.

[0056] The method for preparing the biomass nanofibers comprises the following steps:

[0057] I. Clean the bamboo with clean water, crush it into powder with a diameter of 1 mm in a crusher, and dry it in a drying oven at 60° C. for 12 h to obtain bamboo powder;

[0058] II. Weigh 2 g of the bamboo powder prepared in step I and put it into a reactor, add 10 mL of 30 wt% hydrogen peroxide solution and 200 mL of 3.2 mol / L nitric acid solution, heat to 40 ° C, stir magnetically at 500 rpm for 60 h, add 1 L of distilled water to terminate the reaction, and obtain a reaction termination solution;

[0059] III. The reaction termination solution prepared in step II was filtered, and the precipitate was washed with distilled water until the filtrate was neutral. The obtained precipitate was redispersed in 100 mL of distilled water, and homogenized using a high-pressure homogenization chamber with a pore size of 87 μm and a homogenization pressure of 1500 bar. The homogenization operation was repeated 4 times to obtain a product precursor;

[0060] IV. The product precursor prepared in step III was washed three times with distilled water, separated by high-speed centrifugation, and dried in an oven at 40° C. for 24 h to obtain biomass nanofibers.

[0061] This embodiment also provides a method for preparing a quick-drying water-based ink, which specifically comprises the following steps:

[0062] S1. Weigh the corresponding weight of raw materials according to the formula and weight parts;

[0063] S2, adding waterborne polyurethane resin, methyl methacrylate, phthalocyanine blue, zinc oxide quantum dots, biomass nanofibers, ethanol and water into the reactor, and stirring at 300 rpm for 30 min;

[0064] S3. After the stirring in step S2 is completed, sodium dodecylbenzene sulfonate and polydimethylsiloxane are added to the reactor, and stirring is continued at 300 rpm for 40 min to obtain a quick-drying water-based ink.

[0065] Comparative Example 1: This comparative example proposes a quick-drying water-based ink, which differs from Example 1 only in that zinc oxide quantum dots are not added, and the remaining components, component contents, and experimental steps are the same as those of Example 1.

[0066] Comparative Example 2: This comparative example proposes a quick-drying water-based ink, which differs from Example 1 only in that no biomass nanofibers are added, and the remaining components, component contents, and experimental steps are the same as those of Example 1.

[0067] Experimental Example 1: The microscopic morphology of the zinc oxide quantum dots and biomass nanofibers prepared in Example 1 was observed using a transmission electron microscope.

[0068] Figure 1 This is a transmission electron microscope image of the zinc oxide quantum dots prepared in Example 1. As shown in the figure, the zinc oxide quantum dots have a diameter of about 10 nm and are evenly distributed. Figure 2This is a transmission electron micrograph of the biomass nanofibers prepared in Example 1. As shown in the figure, the biomass nanofibers exhibit a high aspect ratio, a certain degree of overlap, and a network structure formed due to the fiberization process, indicating the successful synthesis of the biomass nanofibers.

[0069] Experimental Example 2: Performance Test: The performance of the water-based inks prepared in Examples 1-3 and Comparative Examples 1-2 were tested respectively; the test results are shown in Table 1.

[0070] Gloss: The 60° gloss of water-based ink is tested according to the standard GB / T 9754-2007 "Determination of 20°, 60° and 85° specular gloss of paints and varnishes without metallic pigments".

[0071] Adhesion: Use 710 tape to adhere to the printed sample surface, the adhesion specification is 20mm×60mm, press the tape to remove the bubbles generated during adhesion, ensure that the tape is completely attached, let it stand for 5 minutes, and quickly peel it off from one end of the tape to observe the shedding of the coating on the tape. If there is no coating shedding or the coating shedding area is less than 5mm 2 , recorded as A; if the coating peeling area is 5 to 15 mm 2 , recorded as B, if the coating peeling area is greater than 15mm 2 , denoted as C.

[0072] Weather resistance: Use a xenon lamp artificial weather resistance tester to test for 200 hours at a wavelength of 340nm, an irradiance of 0.51w / m2, a relative humidity of 50%, and a black standard temperature of 60℃. If the coating has no aging phenomena such as discoloration, shedding, and cracks, it is recorded as A. If aging phenomena occur, it is recorded as B.

[0073] Initial drying property: The initial drying property of water-based ink is tested according to the standard GB / T 13217.5-2008 "Test method for initial drying property of liquid ink".

[0074] Water resistance: Use a damp cloth to wipe the printed sample. If it does not fade after wiping, it is marked as A. If it fades after wiping, it is marked as B.

[0075] Table 1 Test data

[0076]

[0077] As shown in Table 1, the glossiness of Examples 1-3 and Comparative Example 2 is relatively high, and the glossiness of Comparative Example 1 is reduced due to the lack of zinc oxide quantum dots; the adhesion of Examples 1-3 and Comparative Example 1 is relatively strong, and the adhesion of Comparative Example 2 is relatively weak, indicating that biomass nanofibers can effectively improve the adhesion of water-based ink, while the weather resistance of Comparative Example 1 is relatively weak, which indicates that zinc oxide quantum dots can improve the performance stability of water-based ink to a certain extent; the number of millimeters of liquid film layer reduced in Examples 1-3 within 30 seconds is larger than that of Comparative Examples 1-2, among which the drying speed of Comparative Example 1 is the slowest, which indicates that the added zinc oxide quantum dots can improve the drying performance of water-based ink to a certain extent due to the quantum confinement catalytic performance and biomass nanofibers; at the same time, the water resistance of Comparative Example 2 is lower than that of Examples 1-3 and Comparative Example 1, indicating that biomass nanofibers can improve the structural stability of water-based ink and improve water resistance.

[0078] The present invention and its implementation methods are described above, and such description is not restrictive, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design methods and embodiments similar to the technical solution without creativity, which should all fall within the protection scope of the present invention.

Claims

1. A quick-drying water-based ink, It is characterized in that The water-based ink comprises the following raw materials in parts by weight: 30-40 parts of water-based polyurethane resin, 10-20 parts of methyl methacrylate, 2-6 parts of water-based pigment, 2-4 parts of zinc oxide quantum dots, 2-4 parts of biomass nanofibers, 0.5-0.8 parts of sodium dodecylbenzene sulfonate, 1-1.5 parts of polydimethylsiloxane, 5-7 parts of ethanol, and 15-20 parts of water; The method for preparing zinc oxide quantum dots comprises the following steps: ① Weigh 10-20 mmol of zinc acetate and dissolve it in 100 mL of ethanol. Stir at 300-400 rpm at room temperature to fully dissolve it to obtain a zinc ion solution. ② Add 10 mL of 0.2 mol / L potassium hydroxide ethanol solution dropwise to the zinc ion solution prepared in step ①, stir continuously at 500-600 rpm for 6-8 h, place in a centrifuge at 8000 rpm to remove the supernatant, wash the precipitate twice with ethanol and water alternately, place in a vacuum drying oven at 60°C and dry for 12 h to obtain zinc oxide quantum dots; The method for preparing the biomass nanofibers comprises the following steps: I. Wash the bamboo with clean water, put it into a crusher to crush it into powder with a diameter of 1 mm, and put it into a drying oven at 60°C for 12 h to obtain bamboo powder; II. Weigh 2 g of the bamboo powder prepared in step I and put it into a reactor, add 10 mL of 30 wt% hydrogen peroxide solution and 200 mL of 3.2 mol / L nitric acid solution, heat to 40-60 ° C, stir magnetically at 400-500 rpm for 48-60 h, add 1 L of distilled water to terminate the reaction, and obtain a reaction termination solution; III. Filter the reaction termination solution prepared in step II, and wash the precipitate with distilled water until the filtrate is neutral. Re-disperse the precipitate in 100 mL of distilled water, and homogenize it using a high-pressure homogenization chamber with a pore size of 87 μm and a homogenization pressure of 1500 bar. Repeat the homogenization operation 4 to 5 times to obtain a product precursor. IV. The product precursor prepared in step III was washed three times with distilled water, separated by high-speed centrifugation, and dried in an oven at 40° C. for 24 h to obtain biomass nanofibers.

2. A quick-drying water-based ink according to claim 1, It is characterized in that The water-based pigment is any one of titanium dioxide, lemon yellow, phthalocyanine blue, ultrafine carbon black, cobalt green and iron oxide red.

3. A method for preparing the quick-drying water-based ink according to any one of claims 1 to 2, It is characterized in that The specific steps include: S1. Weigh the corresponding weight of raw materials according to the formula and weight parts; S2, adding 30-40 parts of waterborne polyurethane resin, 10-20 parts of methyl methacrylate, 2-6 parts of waterborne pigment, 2-4 parts of zinc oxide quantum dots, 2-4 parts of biomass nanofibers, 5-7 parts of ethanol, and 15-20 parts of water into a reactor, and stirring at 300 rpm for 30 min; S3. After the stirring in step S2 is completed, 0.5-0.8 parts of sodium dodecylbenzene sulfonate and 1-1.5 parts of polydimethylsiloxane are added to the reactor, and stirring is continued at 300 rpm for 40 min to obtain a quick-drying water-based ink.