A kind of high-strength glass fiber enameled wire with corrosion resistance and preparation method thereof

By annealing and impregnating bare copper wires, combined with glass fiber wrapping, and using materials such as modified silica and epoxy resin, the corrosion problem of enameled wires in high temperatures and harsh environments has been solved, and its corrosion resistance and strength, and simplifies the production process to achieve excellent insulation and mechanical properties.

CN118280662BActive Publication Date: 2024-10-01XIANGTAN XIACHENG ELECTRICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410390900.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-10-01
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

Existing enameled wires have corrosion problems under high temperatures and harsh environments, and the production process is complex, affecting their performance and efficiency.

Method used

By annealing the bare copper wire, dipping it in paint and baking it, and introducing materials such as nano-silica and epoxy resin into the insulating paint to form modified silica, combined with glass fiber wrapping, a corrosion-resistant and high-strength glass fiber enameled wire.

Benefits of technology

It significantly improves the corrosion resistance and mechanical strength of the enameled wire, extends its service life, simplifies the production process, and improves the insulation performance and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004772284980000121
    Figure BDA0004772284980000121
Patent Text Reader

Abstract

The invention relates to the technical field of enameled wires, and specifically discloses a high-strength glass-fiber-covered enameled wire with corrosion resistance and a preparation method thereof. The conductor is annealed and then dipped in varnish and baked, and the glass fibers are wrapped and baked to obtain the high-strength glass-fiber-covered enameled wire with corrosion resistance. The insulating varnish comprises modified silica, polyamic acid and epoxy resin, and has excellent adhesion and film-forming properties, and can form a dense and uniform insulating varnish on the surface of the conductor. The enameled wire preparation process is simple and easy to process. The glass fibers have excellent insulation and corrosion resistance, and can form an insulating barrier on the conductor to prevent current leakage or short circuit. In addition, the glass fibers also provide good heat resistance and mechanical strength. The synergistic effect of the two improves production efficiency and greatly improves the insulation performance, mechanical properties and corrosion resistance of the enameled wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of enameled wires, in particular to a high-strength glass fiber enameled wire with corrosion resistance and a preparation method thereof. Background Art

[0002] Enameled wire is a main type of winding wire. It is a wire with an insulating structure, consisting of a conductor and an insulating layer. By painting the outer layer of bare copper wire, alloy wire and glass fiber covered wire of various wire diameters, enameled wire with stable performance is obtained. This type of insulating material has become an indispensable material in modern life. With the continuous increase and investment in large-scale industries and large-scale equipment in my country, new requirements have been put forward for my country's electrical auxiliary materials. Different corrosion phenomena occur under water erosion, chemical erosion and high temperature conditions. Therefore, enameled wire needs to have good corrosion resistance to extend its practical life. In addition, its mechanical strength needs to be improved to make it more suitable for use in harsh environments.

[0003] Chinese patent application CN109545452A provides an enameled wire, including a conductor core wire and an insulating coating wrapped on the conductor core wire, wherein the insulating coating includes a polyester imide paint coating and a fluorosilicone paint coating, and the fluorosilicone paint coating is located on the polyester imide paint coating; the fluorosilicone paint coating is composed of fluorosilicone resin, glass fiber, chlorite, isothiazolinone and glycerin. The enameled wire has a simple preparation process and has good high temperature resistance, corrosion resistance and electrical insulation. However, the raw materials in the fluorosilicone paint in the insulating coating have poor dispersibility, which has a great influence on the performance of the enameled wire. Chinese patent CN102034570B discloses a method for preparing a glass fiber-wrapped corona-resistant enameled flat wire and a product thereof. Two types of corona-resistant enameled wire paints are directly used in the enameling process to process the enameled wire into a corona-resistant enameled wire, which is then wrapped with glass fibers, dipped in varnish, and baked to finally obtain a glass fiber-wrapped corona-resistant enameled flat wire with a five-layer insulation structure. The product exhibits excellent insulation properties through the coating and wrapping of glass fibers, and has high mechanical strength. However, the process of coating the enameled wire paint is cumbersome and the production efficiency is reduced. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a high-strength glass-fiber enameled wire with corrosion resistance and a preparation method thereof. By wrapping glass fibers around a metal wire core and dipping it in varnish, an enameled wire with excellent corrosion resistance and high strength is obtained.

[0006] (II) Technical solution

[0007] In order to achieve the above object, the present invention discloses a method for preparing a high-strength glass fiber enameled wire with corrosion resistance, wherein the conductor is annealed and then dipped in varnish, baked, glass fiber wrapped, and baked to obtain a high-strength glass fiber enameled wire with corrosion resistance;

[0008] The conductor is a bare copper wire;

[0009] The corrosion-resistant high-strength glass fiber enameled wire is prepared by the following steps:

[0010] S1. Clean the bare copper wire, dry it, and then anneal it in an annealing furnace at a temperature of 550-580° C. After the annealing is completed, cool it to obtain a pretreated copper wire;

[0011] S2, immersing the pretreated copper wire in insulating varnish to form an insulating layer on the surface of the bare copper wire, and then baking and curing, and after baking, cooling and winding the wire to obtain an insulating enameled wire;

[0012] S3, wrapping the insulating enameled wire with glass fibers, and baking the enameled wire at a temperature of 280-290° C. After baking, a high-strength glass-fiber enameled wire with corrosion resistance is obtained.

[0013] Preferably, in S1, deionized water is used to clean the bare copper wire.

[0014] Preferably, during the annealing process in S1, the bare copper wire is annealed from the upper layer to the lower layer of the annealing furnace, the temperature of the upper layer is 550-565°C, and the temperature of the lower layer is 565-580°C.

[0015] Preferably, during the baking and curing process in S2, the inlet temperature of the oven is 145-155°C, the temperature of the lower layer of the oven is 240-250°C, the curing temperature is 420-430°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace port frequency is 20Hz, and the lower furnace port fan frequency is 15Hz.

[0016] Preferably, during the glass fiber wrapping process in S3, the glass fiber wrapping has no gaps, no accumulation and is smooth.

[0017] Preferably, the glass fibers in S3 are alkali-free glass fibers.

[0018] Preferably, the method for preparing the insulating varnish in S2 comprises the following steps:

[0019] Step 1: Evenly mix N,N-dimethylformamide, nano-silica, hexadecenyl succinic anhydride, 4-dimethylaminopyridine and sodium hydroxide, react at 80-90° C. for 4-8 hours, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60° C. for 12 hours to obtain olefinated silica;

[0020] Step 2: evenly mix anhydrous ethanol and deionized water to obtain a mixed solvent, then add olefinated silica, evenly disperse by ultrasonication, add methyl methacrylate and an initiator, react, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60° C. for 12 hours to obtain modified silica;

[0021] Step 3: Mix N,N-dimethylacetamide and 4,4'-diaminodiphenyl ether in an ice-water bath, and after they are completely dissolved, add diphenyl ether tetracarboxylic dianhydride, stir for about 12 hours at room temperature, heat in a water bath, and after heating, cool to obtain polyamic acid;

[0022] Step 4: Stir and mix the polyamic acid and epoxy resin, then add the modified silicon dioxide and 4,4'-diaminodiphenyl sulfone, stir and mix, then add the defoamer and antioxidant, stir evenly at 70-80° C. to obtain the insulating paint.

[0023] Preferably, in the step 1, the mass ratio of N,N-dimethylformamide, nano-silicon dioxide, hexadecenylsuccinic anhydride, 4-dimethylaminopyridine and sodium hydroxide is 2500-3200:100:72-95:3.5-4.5:1.2-1.5.

[0024] Preferably, in step 2, the volume ratio of anhydrous ethanol to deionized water is 3:1, wherein the mass ratio of the mixed solvent, olefinic silica, methyl methacrylate and initiator is 2100-2400:100:25-38:3-5.

[0025] Preferably, the reaction temperature in step 2 is 75-85° C., and the reaction time is 3-5 h.

[0026] Preferably, the initiator in step 2 is dibenzoyl peroxide.

[0027] Preferably, in step 3, the mass ratio of N,N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 950-1200:100:152-158.

[0028] Preferably, the water bath heating temperature in step 3 is 60-65° C., and the water bath heating time is 35-45 min.

[0029] Preferably, in step 4, the mass ratio of polyamic acid, epoxy resin, modified silica, 4,4'-diaminodiphenyl sulfone, defoaming agent and antioxidant is 100:55-62:9-12:14-20:1-2:1.5-3.

[0030] Preferably, the defoaming agent in step 4 is a silicone defoaming agent.

[0031] Preferably, the antioxidant in step 4 is antioxidant 1010.

[0032] Preferably, the high-strength glass-fiber enameled wire with corrosion resistance is prepared by the method for preparing the high-strength glass-fiber enameled wire with corrosion resistance.

[0033] (III) Beneficial technical effects

[0034] (1) In the preparation process of the insulating varnish of the present invention, hexadecenyl succinic anhydride is first used to modify the nano-silica, and the anhydride on the hexadecenyl succinic anhydride reacts with the hydroxyl group on the surface of the nano-silica to introduce long-chain alkyl, alkenyl and carboxyl groups on the surface of the nano-silica to obtain alkenylated silica. The alkenyl groups on the surface of the alkenylated silica and methyl methacrylate are polymerized in situ under the action of an initiator to introduce polymethyl methacrylate on the nano-silica to obtain modified silica, which effectively improves the dispersibility of the nano-silica and avoids the agglomeration of the nano-silica. The active groups on the polyamic acid, the carboxyl groups on the modified silica and the epoxy resin react to form a cross-linked network structure. The bicontinuous phase structure formed by the interpenetrating reaction is conducive to dispersing stress and can maintain the original performance of each phase. The compatibility between the raw materials is improved to obtain an insulating varnish with excellent comprehensive performance. Furthermore, nano-silicon dioxide has excellent mechanical properties, and the long alkyl chain introduced during the reaction has good hydrophobicity and toughening effect, which can prevent the insulating paint from falling off and bending when the enameled wire is bent, making the enameled wire have excellent mechanical strength. The added nano-silicon dioxide has the ability to resist partial discharge caused by voltage pulses, can eliminate the space charge accumulated under the rapid rise time of the pulse, and improve the corona resistance of the insulating paint.

[0035] (2) In the present invention, the bare copper wire is immersed in the insulating varnish, which has excellent adhesion and can be well attached to the conductor surface. The introduced polymethyl methacrylate further improves the film-forming property, forms a dense and uniform insulating varnish on the conductor surface, has good insulation performance, and has high hardness of the varnish film. It works together with nano-silicon dioxide to effectively improve the corrosion resistance and wear resistance of the enameled wire and extend the service life of the enameled wire. Among them, the epoxy resin has the characteristics of strong adhesion, small shrinkage force, excellent chemical resistance, corrosion resistance, water resistance, thermal stability and electrical insulation, and the polyimide has the characteristics of good heat resistance, electrical insulation, mechanical properties and chemical stability. The insulating varnish formed on the conductor surface has excellent insulation performance and corrosion resistance, and high strength.

[0036] (3) In the present invention, the glass fiber is wrapped on the enameled wire, the preparation process is simple, and the processing is easy. The glass fiber has excellent insulation and corrosion resistance. A layer is coated on the surface of the insulating enameled wire to form an insulation barrier to prevent current leakage or short circuit. In addition, the glass fiber also provides good heat resistance and mechanical strength, and improves the mechanical properties of the enameled wire, so that the glass fiber enameled wire can maintain stable working performance under high temperature or mechanical stress environment, and has the characteristics of high strength. The glass fiber and the insulating paint work together, and the two work synergistically, so that the enameled wire has better toughness and strength, and the obtained enameled wire has excellent insulation performance, mechanical properties and corrosion resistance. DETAILED DESCRIPTION

[0037] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0038] Example 1

[0039] A method for preparing a high-strength glass fiber enameled wire with corrosion resistance, comprising the following steps:

[0040] S1. Clean the bare copper wire, dry it, and then anneal it in an annealing furnace. During the annealing process, the bare copper wire is annealed from the upper layer to the lower layer of the annealing furnace. The upper layer temperature is 550° C. and the lower layer temperature is 565° C. After the annealing is completed, cool it to obtain a pretreated copper wire;

[0041] S2, immersing the pretreated copper wire in insulating varnish, forming an insulating layer on the surface of the bare copper wire, and then baking and curing, the inlet temperature of the oven is 145°C, the temperature of the lower layer of the oven is 240°C, the curing temperature is 420°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace frequency is 20Hz, the lower furnace fan frequency is 15Hz, after baking, cooling, winding, and obtaining an insulating enameled wire;

[0042] S3, wrapping the insulating enameled wire with glass fibers, and baking the enameled wire at a temperature of 280° C. to obtain a high-strength glass-fiber enameled wire with corrosion resistance.

[0043] The preparation method of the insulating varnish comprises the following steps:

[0044] Step 1: Evenly mix N,N-dimethylformamide, nano-silica, hexadecenyl succinic anhydride, 4-dimethylaminopyridine and sodium hydroxide in a mass ratio of 2500:100:72:3.5:1.2, react at 80°C for 8 hours, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12 hours to obtain olefinated silica;

[0045] Step 2: evenly mix anhydrous ethanol and deionized water in a volume ratio of 3:1 to obtain a mixed solvent, add olefinic silica, and after ultrasonic dispersion, add methyl methacrylate and initiator dibenzoyl peroxide, wherein the mass ratio of the added mixed solvent, olefinic silica, methyl methacrylate and dibenzoyl peroxide is 2100:100:25:3, react at 75°C for 5h, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12h to obtain modified silica;

[0046] Step 3, N, N-dimethylacetamide and 4,4'-diaminodiphenyl ether are mixed in an ice water bath, and after they are completely dissolved, diphenyl ether tetracarboxylic dianhydride is added, wherein the mass ratio of N, N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 950:100:152, stirring for about 12 hours at room temperature, heating in a water bath, the water bath heating temperature is 60 ° C, the water bath heating time is 45 minutes, and after the heating is completed, cooling to obtain polyamic acid;

[0047] Step 4: Stir and mix polyamic acid and epoxy resin, add modified silica and 4,4'-diaminodiphenyl sulfone, stir and mix, then add defoamer and antioxidant, wherein the mass ratio of polyamic acid, epoxy resin, modified silica, 4,4'-diaminodiphenyl sulfone, defoamer and antioxidant is 100:55:9:14:1:1.5, stir evenly at 70°C to obtain insulating paint.

[0048] Example 2

[0049] A method for preparing a high-strength glass fiber enameled wire with corrosion resistance, comprising the following steps:

[0050] S1. Clean the bare copper wire, dry it, and then anneal it in an annealing furnace. During the annealing process, the bare copper wire is annealed from the upper layer to the lower layer of the annealing furnace. The temperature of the upper layer is 560° C. and the temperature of the lower layer is 575° C. After the annealing is completed, cool it to obtain a pretreated copper wire;

[0051] S2, immersing the pretreated copper wire in insulating varnish, forming an insulating layer on the surface of the bare copper wire, and then baking and curing, the inlet temperature of the oven is 150°C, the temperature of the lower layer of the oven is 245°C, the curing temperature is 425°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace frequency is 20Hz, the lower furnace fan frequency is 15Hz, after baking, cooling, winding, and obtaining an insulating enameled wire;

[0052] S3, wrapping the insulating enameled wire with glass fibers, and baking the enameled wire at a temperature of 285° C. to obtain a high-strength glass-fiber enameled wire with corrosion resistance.

[0053] The preparation method of the insulating varnish comprises the following steps:

[0054] Step 1: Evenly mix N,N-dimethylformamide, nano-silica, hexadecenyl succinic anhydride, 4-dimethylaminopyridine and sodium hydroxide in a mass ratio of 2800:100:80:3.8:1.3, react at 85°C for 6 hours, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12 hours to obtain olefinated silica;

[0055] Step 2, anhydrous ethanol and deionized water in a volume ratio of 3:1 are mixed evenly to obtain a mixed solvent, and then olefinic silica is added, and after ultrasonic dispersion, methyl methacrylate and initiator dibenzoyl peroxide are added, wherein the mass ratio of the added mixed solvent, olefinic silica, methyl methacrylate and dibenzoyl peroxide is 2160:100:30:3.5, and the reaction is carried out at 80° C. for 4 hours. After the reaction is completed, the mixture is filtered, washed with anhydrous ethanol, and dried in a vacuum drying oven at 60° C. for 12 hours to obtain modified silica;

[0056] Step 3, N, N-dimethylacetamide and 4,4'-diaminodiphenyl ether are mixed in an ice water bath, and after they are completely dissolved, diphenyl ether tetracarboxylic dianhydride is added, wherein the mass ratio of N, N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 1020:100:154, stirring for about 12 hours at room temperature, heating in a water bath, the water bath heating temperature is 62 ° C, the water bath heating time is 40 minutes, and after the heating is completed, cooling to obtain polyamic acid;

[0057] Step 4: Stir and mix polyamic acid and epoxy resin, add modified silica and 4,4'-diaminodiphenyl sulfone, stir and mix, then add defoamer and antioxidant, wherein the mass ratio of polyamic acid, epoxy resin, modified silica, 4,4'-diaminodiphenyl sulfone, defoamer and antioxidant is 100:58:10:16:1.2:2, stir evenly at 75°C to obtain insulating paint.

[0058] Example 3

[0059] The method for preparing a high-strength glass fiber enameled wire with corrosion resistance is the same as the method for preparing the high-strength glass fiber enameled wire with corrosion resistance in Example 2.

[0060] The preparation method of the insulating varnish comprises the following steps:

[0061] Step 1: Evenly mix N,N-dimethylformamide, nano-silica, hexadecenyl succinic anhydride, 4-dimethylaminopyridine and sodium hydroxide in a mass ratio of 3000:100:88:4.2:1.4, react at 85°C for 7 hours, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12 hours to obtain olefinated silica;

[0062] Step 2: evenly mix anhydrous ethanol and deionized water in a volume ratio of 3:1 to obtain a mixed solvent, add olefinic silica, and evenly disperse by ultrasonication, then add methyl methacrylate and initiator dibenzoyl peroxide, wherein the mass ratio of the added mixed solvent, olefinic silica, methyl methacrylate and dibenzoyl peroxide is 2310:100:35:4.2, react at 80°C for 4h, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12h to obtain modified silica;

[0063] Step 3, N, N-dimethylacetamide and 4,4'-diaminodiphenyl ether are mixed in an ice water bath, and after they are completely dissolved, diphenyl ether tetracarboxylic dianhydride is added, wherein the mass ratio of N, N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 1150:100:156, stirring for about 12 hours at room temperature, heating in a water bath, the water bath heating temperature is 62 ° C, the water bath heating time is 40 minutes, and after the heating is completed, cooling to obtain polyamic acid;

[0064] Step 4: Stir and mix polyamic acid and epoxy resin, add modified silica and 4,4'-diaminodiphenyl sulfone, stir and mix, then add defoamer and antioxidant, wherein the mass ratio of polyamic acid, epoxy resin, modified silica, 4,4'-diaminodiphenyl sulfone, defoamer and antioxidant is 100:60:11:18:1.6:2.4, stir evenly at 75°C to obtain insulating paint.

[0065] Example 4

[0066] A method for preparing a high-strength glass fiber enameled wire with corrosion resistance, comprising the following steps:

[0067] S1. Clean the bare copper wire, dry it, and then anneal it in an annealing furnace. During the annealing process, the bare copper wire is annealed from the upper layer to the lower layer of the annealing furnace. The upper layer temperature is 565° C. and the lower layer temperature is 580° C. After the annealing is completed, cool it to obtain a pretreated copper wire;

[0068] S2, immersing the pretreated copper wire in insulating varnish, forming an insulating layer on the surface of the bare copper wire, and then baking and curing, the inlet temperature of the oven is 155°C, the temperature of the lower layer of the oven is 250°C, the curing temperature is 430°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace frequency is 20Hz, the lower furnace fan frequency is 15Hz, after baking, cooling, winding, and obtaining an insulating enameled wire;

[0069] S3, wrapping the insulating enameled wire with glass fibers, and baking the enameled wire at a temperature of 290° C. to obtain a high-strength glass-fiber enameled wire with corrosion resistance.

[0070] The preparation method of the insulating varnish comprises the following steps:

[0071] Step 1: Evenly mix N,N-dimethylformamide, nano-silica, hexadecenyl succinic anhydride, 4-dimethylaminopyridine and sodium hydroxide in a mass ratio of 3200:100:95:4.5:1.5, react at 90°C for 4 hours, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12 hours to obtain olefinated silica;

[0072] Step 2: evenly mix anhydrous ethanol and deionized water in a volume ratio of 3:1 to obtain a mixed solvent, then add olefinic silica, and after ultrasonic dispersion, add methyl methacrylate and initiator dibenzoyl peroxide, wherein the mass ratio of the added mixed solvent, olefinic silica, methyl methacrylate and dibenzoyl peroxide is 2400:100:38:5, react at 85°C for 3h, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 12h to obtain modified silica;

[0073] Step 3, N, N-dimethylacetamide and 4,4'-diaminodiphenyl ether are mixed in an ice water bath, and after they are completely dissolved, diphenyl ether tetracarboxylic dianhydride is added, wherein the mass ratio of N, N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 1200:100:158, stirring for about 12 hours at room temperature, heating in a water bath, the water bath heating temperature is 65 ° C, the water bath heating time is 35 minutes, and after the heating is completed, cooling to obtain polyamic acid;

[0074] Step 4: Stir and mix polyamic acid and epoxy resin, then add modified silica and 4,4'-diaminodiphenyl sulfone, stir and mix, then add defoamer and antioxidant, wherein the mass ratio of polyamic acid, epoxy resin, modified silica, 4,4'-diaminodiphenyl sulfone, defoamer and antioxidant is 100:62:12:20:2:3, stir evenly at 80°C to obtain insulating paint.

[0075] Comparative Example 1

[0076] A method for preparing an enameled wire comprises the following steps:

[0077] S1. Clean the bare copper wire, dry it, and then anneal it in an annealing furnace. During the annealing process, the bare copper wire is annealed from the upper layer to the lower layer of the annealing furnace. The temperature of the upper layer is 560° C. and the temperature of the lower layer is 575° C. After the annealing is completed, cool it to obtain a pretreated copper wire;

[0078] S2. Immerse the pretreated copper wire in insulating varnish to form an insulating layer on the surface of the bare copper wire, and then bake and cure it. The inlet temperature of the oven is 150°C, the temperature of the lower layer of the oven is 245°C, the curing temperature is 425°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace frequency is 20Hz, and the lower furnace fan frequency is 15Hz. After baking, cool and wind up to obtain the enameled wire.

[0079] The preparation method of the insulating varnish used therein is the same as the preparation method of the insulating varnish in Example 3.

[0080] Comparative Example 2

[0081] The preparation method of a glass fiber enameled wire is the same as the preparation method of a corrosion-resistant high-strength glass fiber enameled wire in Example 3.

[0082] The difference from Example 3 is that the preparation method of the insulating varnish used is different, and the preparation method of the insulating varnish used comprises the following steps:

[0083] Step 1, N, N-dimethylacetamide and 4,4'-diaminodiphenyl ether are mixed in an ice water bath, and after they are completely dissolved, diphenyl ether tetracarboxylic dianhydride is added, wherein the mass ratio of N, N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 1150:100:156, stirring for about 12 hours at room temperature, heating in a water bath, the water bath heating temperature is 62° C., the water bath heating time is 40 minutes, and after the heating is completed, cooling to obtain polyamic acid;

[0084] Step 2: Stir and mix polyamic acid and epoxy resin, then add nano-silica and 4,4'-diaminodiphenyl sulfone, stir and mix, then add defoamer and antioxidant, wherein the mass ratio of polyamic acid, epoxy resin, nano-silica, 4,4'-diaminodiphenyl sulfone, defoamer and antioxidant is 100:60:11:18:1.6:2.4, stir evenly at 75°C to obtain insulating paint.

[0085] Comparative Example 3

[0086] A method for preparing an enameled wire comprises the following steps:

[0087] S1. Clean the bare copper wire, dry it, and then anneal it in an annealing furnace. During the annealing process, the bare copper wire is annealed from the upper layer to the lower layer of the annealing furnace. The temperature of the upper layer is 560° C. and the temperature of the lower layer is 575° C. After the annealing is completed, cool it to obtain a pretreated copper wire;

[0088] S2. Immerse the pretreated copper wire in insulating varnish to form an insulating layer on the surface of the bare copper wire, and then bake and cure it. The inlet temperature of the oven is 150°C, the temperature of the lower layer of the oven is 245°C, the curing temperature is 425°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace frequency is 20Hz, and the lower furnace fan frequency is 15Hz. After baking, cool and wind up to obtain the insulating enameled wire.

[0089] The preparation method of the insulating varnish is the same as the preparation method of the insulating varnish in Comparative Example 2.

[0090] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be obtained from commercial sources.

[0091] The performance tests were performed on the samples prepared in Examples 1-4 and Comparative Examples 1-3 of the present invention, and the specific tests were as follows:

[0092] (1) Corrosion resistance test: Salt spray resistance, acid corrosion resistance and alkali corrosion resistance tests were carried out respectively. The salt spray resistance test was carried out in accordance with the test standard of GB / T 1771-2007. The acid corrosion resistance test was carried out by immersing the paint film in 0.1 mol / L sulfuric acid for 7 days, then taking it out to observe the condition of the paint film; the alkali corrosion resistance test was carried out by immersing the paint film in 0.1 mol / L sodium hydroxide for 7 days, then taking it out to observe the condition of the paint film;

[0093] (2) Hardness test: Test the surface hardness of the sample according to GB / T6739-2022;

[0094] The test results are shown in Table 1:

[0095] Table 1

[0096]

[0097] According to the test data in Table 1, it can be seen that the samples corresponding to Examples 1-4 not only have excellent corrosion resistance, but also show good surface hardness, high strength and good water resistance. In Comparative Example 1, the conductor surface is impregnated with insulating paint to obtain enameled wire, but glass filaments are not wrapped, and the corrosion resistance and strength are reduced; in Comparative Example 2, nano silicon dioxide is not modified and directly added to the insulating paint, and the dispersibility and compatibility are greatly reduced, and polymethyl methacrylate is not introduced, which also has a certain effect on the density and film-forming properties of the paint film; in Comparative Example 3, the insulating paint is the same as that in Comparative Example 2, and glass filaments are not wrapped on this basis, and the comprehensive performance is greatly reduced, the corrosion resistance is poor, and the hardness is low.

[0098] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a high-strength glass fiber enameled wire with corrosion resistance, It is characterized in that After the conductor is annealed, it is then dipped in varnish, baked, wrapped with glass fibers, and baked to obtain a high-strength glass-fiber enameled wire with corrosion resistance; The conductor is a bare copper wire; The corrosion-resistant high-strength glass fiber enameled wire is prepared by the following steps: S1. Clean the bare copper wire, and then anneal it in an annealing furnace at a temperature of 550-580° C. After the annealing is completed, cool it to obtain a pretreated copper wire; S2, immersing the pretreated copper wire in insulating varnish to form an insulating layer on the surface of the bare copper wire, and then baking and curing, and after baking, cooling and winding the wire to obtain an insulating enameled wire; S3, wrapping the insulating enameled wire with glass fibers, and baking the enameled wire at a temperature of 280-290° C. to obtain a high-strength glass-fiber enameled wire with corrosion resistance; The method for preparing the insulating varnish in S2 comprises the following steps: Step 1: Evenly mix N,N-dimethylformamide, nano-silica, hexadecenyl succinic anhydride, 4-dimethylaminopyridine and sodium hydroxide, react at 80-90° C. for 4-8 hours, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60° C. for 12 hours to obtain olefinated silica; Step 2: evenly mix anhydrous ethanol and deionized water to obtain a mixed solvent, then add olefinated silica, evenly disperse by ultrasonication, add methyl methacrylate and an initiator, react, filter after the reaction, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60° C. for 12 hours to obtain modified silica; Step 3: Mix N,N-dimethylacetamide and 4,4'-diaminodiphenyl ether in an ice-water bath, and after they are completely dissolved, add diphenyl ether tetracarboxylic dianhydride, stir for 12 hours at room temperature, heat in a water bath, and after heating, cool to obtain polyamic acid; Step 4: Stir and mix the polyamic acid and epoxy resin, then add modified silica and 4,4'-diaminodiphenyl sulfone, stir and mix, then add a defoamer and an antioxidant, stir evenly at 70-80° C. to obtain an insulating paint; In the step 1, the mass ratio of N,N-dimethylformamide, nano-silicon dioxide, hexadecenylsuccinic anhydride, 4-dimethylaminopyridine and sodium hydroxide is 2500-3200:100:72-95:3.5-4.5:1.2-1.5; In the step 2, the volume ratio of anhydrous ethanol to deionized water is 3:1, wherein the mass ratio of the mixed solvent, olefinic silica, methyl methacrylate and initiator is 2100-2400:100:25-38:3-5, the reaction temperature is 75-85°C, and the reaction time is 3-5h; In the step 2, the initiator is dibenzoyl peroxide; In the step 3, the mass ratio of N,N-dimethylacetamide, 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride is 950-1200:100:152-158, the water bath heating temperature is 60-65°C, and the water bath heating time is 35-45min; In the step 4, the mass ratio of polyamic acid, epoxy resin, modified silica, 4,4'-diaminodiphenyl sulfone, defoaming agent and antioxidant is 100:55-62:9-12:14-20:1-2:1.5-3.

2. A method for preparing a corrosion-resistant high-strength glass fiber enameled wire according to claim 1, It is characterized in that During the baking and curing process in S2, the inlet temperature of the oven is 145-155°C, the temperature of the lower layer of the oven is 240-250°C, the curing temperature is 420-430°C, the main circulation fan frequency is 21Hz, the exhaust fan furnace frequency is 20Hz, and the lower furnace fan frequency is 15Hz.

3. The method for preparing a corrosion-resistant high-strength glass fiber enameled wire according to claim 1, It is characterized in that In the process of wrapping the glass fibers in S3, the wrapped fibers are not leaky, not piled up and are smooth.

4. A corrosion-resistant high-strength glass-fiber enameled wire prepared by the method for preparing a corrosion-resistant high-strength glass-fiber enameled wire according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Preparation method of glass fiber covered corona-resistant enameled rectangular wire

    CN102034570B

  • Enameled wire and preparation process thereof

    CN109545452A

  • Manufacturing process of fire-resistant thin dacron glass yarn sintered enameling copper strap wire

    CN101295559A

  • Production process of freon resistant, double glass fiber covered enamelled wire

    CN101615451A

  • Preparation method and product of glass fiber covered corona-resistant enameled rectangular wire