A Low-Temperature Flotation Method for Spodumene Minerals
By using a combination of grinding modifiers, modifying modifiers, and collectors in the flotation of spodumene minerals, the problem of low recovery rate of spodumene minerals at low temperatures was solved, achieving a highly efficient low-temperature flotation effect and reducing energy consumption and operating costs.
Patent Information
- Application Number
- CN202410568639.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-05-09
AI Technical Summary
Existing spodumene mineral flotation technologies have low recovery rates and low grades under low-temperature conditions, and conventional heated flotation has high energy consumption and operating costs, making it difficult to meet the requirements of low-carbon technologies.
The combination of grinding modifiers, modifying modifiers, metal ion activators, and spodumene mineral collectors, including carbonates, percarbonates, caustic alkalis, strong acid salts, lignin sulfonates, anionic surfactants, strong organic electrolyte components, and emulsifiers, enhances mineral collection efficiency by strengthening interfacial electrodynamic forces, improving mineral surface properties, and promoting fine mud settling.
Significantly improves the recovery rate and grade of spodumene minerals at low temperatures, reduces energy consumption and operating costs, and achieves efficient spodumene mineral sorting.
Abstract
Description
Technical Field
[0001] This invention relates to the field of mineral sorting and processing technology, specifically to a low-temperature flotation method for spodumene minerals. Background Technology
[0002] Pegmatite-type spodumene (LiAl(Si2O6)) is the main raw material for lithium metal extraction. Before extracting lithium from the ore, low-Li2O grade spodumene ore is typically beneficiated using mineral processing methods to selectively enrich the spodumene minerals into a lithium concentrate with a Li2O content of 5.0-6.0% before smelting. Currently, spodumene mineral processing technologies mainly include flotation, gravity separation, magnetic separation, heavy media separation, hand sorting, and combined processes. Among these, flotation for selective separation of lithium minerals is currently the most effective mineral enrichment method. However, the target mineral and gangue minerals in pegmatite spodumene ore are mostly in the form of silicate or aluminosilicate minerals. After dissociation, these silicate minerals exhibit similar physicochemical properties. Furthermore, during the mineral grinding and flotation separation process, the mineral floatability tends to converge due to the unavoidable adsorption of ions or fine grinding mud in the slurry solution, leading to difficulties in the selective enrichment of spodumene minerals. In addition, from the perspective of the mineralization belts, many pegmatite-type lithium deposits, both domestically and internationally, are located in high-altitude, arid, and water-scarce regions. These areas are in a low-temperature environment year-round, and the excessively low temperature of the flotation pulp reduces the reactivity of various species in the flotation solution system. Relatively speaking, the disadvantages of low-temperature flotation include: 1) The driving force for hydroxylation or modification of mineral surfaces is relatively weakened at low temperatures, leading to a reduction in the surface property differences between spodumene and gangue minerals; 2) The low scattering activity of various species in the solution medium, such as reduced water reactivity, affects the indiscriminate diffusion of fine mud, meaning that the adverse effects of low-temperature fine mud on lithium recovery are increased; 3) The segregation activity of existing spodumene collectors is greatly limited by low-temperature separation conditions, significantly reducing their performance.
[0003] Current development of spodumene flotation technology focuses primarily on ambient temperature collection systems and related processes. This means that existing separation reagents used in spodumene flotation are not yet efficient in low-temperature slurry systems, as temperature significantly affects the process. The efficiency of adjustment, modification, and collection / mineralization is low, often resulting in severe waste of lithium resources. Heating the slurry for flotation is energy-intensive and costly, requiring additional equipment. Furthermore, using coal-based energy sources for heating results in carbon emissions, making it difficult to meet low-carbon technology requirements. Therefore, effectively and efficiently recovering high-grade spodumene through flotation at low temperatures remains a critical challenge for the spodumene mineral processing industry. Summary of the Invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of low lithium recovery rate and low grade in the existing low-temperature separation of spodumene minerals, and thus provide a low-temperature flotation method for spodumene minerals to solve the above problems.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A low-temperature flotation method for spodumene minerals, comprising:
[0007] The spodumene ore to be sorted is crushed to obtain crushed mineral materials;
[0008] Water is added to crushed mineral materials and the materials are ground to dissociate the minerals. A grinding modifier is added during the grinding process to obtain a grinding slurry. The grinding modifier includes a first modifier component and a strong acid salt. The first modifier component is at least one of carbonate, percarbonate, and caustic alkali.
[0009] The grinding slurry is conditioned, then modified with a modifier, followed by ion activation with a metal ion activator, and finally mineralized with a spodumene mineral collector. The spodumene concentrate and flotation tailings are then obtained. The modifier includes highly active OH groups. - Modifiers and lignin sulfonates; the spodumene mineral collector includes anionic surfactants, strong organic electrolyte components, and emulsifiers.
[0010] Preferably, the first adjusting component is at least one selected from sodium carbonate, potassium carbonate, ammonium carbonate, sodium percarbonate, sodium hydroxide, and potassium hydroxide;
[0011] And / or, the strong acid salt is a sulfate and / or a nitrate; preferably, the strong acid salt is at least one of sodium sulfate, potassium sulfate, sodium nitrate, and potassium nitrate;
[0012] And / or, the maximum particle size of the crushed mineral material is 1-12 mm;
[0013] And / or, the content of minerals with a fineness of -0.074 mm (maximum particle size of 0.074 mm) after grinding is 50-95%;
[0014] And / or, based on 1 t of dry spodumene ore to be sorted, the amount of grinding modifier is 100-4000 g, wherein the amount of the first modifier component is 100-2000 g and the amount of the strong acid salt is 300-3500 g.
[0015] And / or, the mass concentration of the grinding slurry is 50-85%.
[0016] Preferably, the mass concentration of the grinding slurry after the slurry conditioning treatment is 25-50%;
[0017] And / or, the slurry conditioning agent used in the slurry conditioning process is water;
[0018] And / or, the highly active OH - The modifier is at least one of caustic soda, ammonia, and organic amines; preferably, the caustic soda is sodium hydroxide and / or potassium hydroxide.
[0019] And / or, the lignin sulfonate is at least one of sodium lignin sulfonate, potassium lignin sulfonate, calcium lignin sulfonate, magnesium lignin sulfonate, and ammonium lignin sulfonate.
[0020] Preferably, based on 1 ton of dry spodumene ore to be sorted, the amount of the modifier is 100-2000 g, wherein the highly active OH... - The dosage of the modifier is 50-2000g, and the dosage of the lignin sulfonate is 50-2000g;
[0021] And / or, the duration of the modification treatment is 5-30 minutes.
[0022] Preferably, the metal ion activator is a calcium ion modifier and / or a magnesium ion modifier; more preferably, the metal ion activator is at least one selected from calcium sulfate, calcium nitrate, calcium chloride, magnesium sulfate, magnesium nitrate, and magnesium chloride.
[0023] And / or, based on the weight of 1 t of dry spodumene ore to be sorted, the amount of the metal ion activator is 100-1000g;
[0024] And / or, the duration of the ion activation treatment is 2-10 min.
[0025] Preferably, the anionic surfactant is at least one of alkyl carboxylates and their derivatives, alkyl sulfonates and their derivatives, alkyl sulfates and their derivatives, and hydroxamic acid salts and their derivatives;
[0026] And / or, the organic strong electrolyte component is at least one of carbonates, amides, and acrylates;
[0027] And / or, the emulsifier is a neutral oil or / and ester organic compound;
[0028] And / or, the functional groups -CH2- that affect the chain length of organic molecules in the anionic surfactant differ by 4-8 from those in the strong organic electrolyte component.
[0029] Preferably, the anionic surfactant is at least one selected from oleic acid, sodium oleate, stearic acid, palmitic acid, lauric acid, tal oil, naphthenic acid soap, sodium dodecylbenzenesulfonate, sodium dodecyl sulfonate, sodium dodecyl sulfate, benzoyl hydroxamic acid, and salicylic acid.
[0030] And / or, the organic strong electrolyte component is at least one of polycarbonate, dimethyl carbonate, ethyl carbonate, vinylene carbonate, vinyl ethylene carbonate, methylene ethylene carbonate, vinyl ethylene carbonate, N-methylformamide, N,N-dimethylacetamide, conjugated sulfonamide, aminosulfonamide, o-benzoylsulfonylimide, and vinyl sulfite.
[0031] And / or, the emulsifier is at least one of kerosene, diesel oil, propylene glycol monostearate, propylene glycol alginate, ethylene glycol monostearate, glyceryl stearate, and sorbitan fatty acid ester.
[0032] Preferably, the amount of spodumene mineral collector used is 100-4000g, based on 1t of dry spodumene ore to be sorted.
[0033] And / or, the mass ratio of the anionic surfactant, the organic strong electrolyte component, and the emulsifier is 1:(0.05-0.2):(0.02-0.1);
[0034] And / or, the duration of the mineralization treatment is 2-10 min.
[0035] Preferably, the flotation separation adopts a mineral flotation process combining roughing, cleaning, and scavenging.
[0036] And / or, the flotation separation is followed by concentration and compression processing;
[0037] And / or, the temperature of the flotation pulp in the flotation separation is 5-19℃.
[0038] Preferably, the coarse selection process takes 3-6 minutes per segment;
[0039] And / or, the sorting time for each selected segment is 2-4 minutes;
[0040] And / or, the sorting time for each segment of the scanning process is 3-6 minutes.
[0041] In this invention, a frother may be added during the mineralization process. Since the collector generally has a bubble-forming function, a separate frother is often not added during the flotation of spodumene minerals. Therefore, the frother may or may not be added. The frother is at least one of No. 2 oil, MIBC, fusel oil, 2-octanol, and glycerol. The mass ratio of the frother to the spodumene mineral collector is 1:(20-200).
[0042] The technical solution of this invention has the following advantages:
[0043] 1. A low-temperature flotation method for spodumene mineral, comprising: crushing spodumene ore to be separated to obtain crushed ore; adding water to the crushed ore and grinding it to achieve mineral dissociation, while adding a grinding modifier during the grinding process to obtain a grinding slurry; wherein the grinding modifier comprises a first modifier component and a strong acid salt; the first modifier component is at least one selected from carbonate, percarbonate, and caustic alkali; conditioning the grinding slurry, then adding a modifying modifier for modification, then adding a metal ion activator for ion activation, and finally adding a spodumene mineral collector for mineralization and flotation separation to obtain spodumene concentrate and flotation tailings; wherein the modifying modifier comprises highly active OH- - Modifiers and lignin sulfonates; the spodumene mineral collector includes anionic surfactants, strong organic electrolyte components, and emulsifiers. This invention, starting from the electro-driving force of enhanced interfacial reactions in low-temperature flotation, enhances the efficiency of mineral surface modification, reduces the influence of fine mud suspension and dispersion, and strengthens the mineral particle collection and mineralization process, thereby improving the efficiency of spodumene minerals in low-temperature flotation. Specifically: 1) Strong acid salts that enhance interfacial electrochemical properties are added during the mineral grinding and dissociation process to enhance the electrochemical performance of the mineral-water interface, increase the conductivity of the mineral-water interface in the system, and enhance the migration ability of species driven by electro-catalysis, thereby improving the efficiency of mineral surface modification; 2) Based on the presence of strong electrolytes in the grinding slurry solution, the OH content in the modification treatment is effectively increased. - The process enhances the efficiency of dissolving or scrubbing the surface of the target mineral, strengthens the formation of hydroxylated mineral surfaces, and further enhances the low-temperature adsorption of fine mud by lignin sulfonate, increasing the probability of fine mud adsorption and sedimentation, thus providing a favorable foundation for subsequent flotation processes. 3) A low-temperature combined collector is formed using anionic surfactants, organic strong electrolyte components, and emulsifiers. The active groups of the anionic surfactants serve as the mineralization reaction center, while the organic strong electrolyte components further enhance the electrochemical activity of the system species, further improving the conductivity of inter-species interactions during mineralization and pulp conditioning, promoting the separation of anionic surfactants and enhancing their low-temperature activity, and promoting electrostatic forces to catalyze the mineralization and collection reactions between the mineral interface and the collector. Simultaneously, a certain amount of emulsifier is combined to balance the coupling structure-activity relationship between the anionic surfactants and the organic strong electrolyte components, and to balance and stabilize the mineral-liquid-gas three-phase interface, thereby stabilizing froth flotation and improving the separation efficiency of lithium minerals. These process steps complement each other and are interconnected, resulting in a significant improvement in the recovery rate and grade of spodumene minerals under low-temperature flotation. Detailed Implementation
[0044] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0045] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0046] Example 1
[0047] This embodiment provides a low-temperature flotation method for spodumene minerals, used to separate low-grade spodumene ore from a high-altitude coastal area in Sichuan Province. The raw ore has a Li₂O content of 1.10%, and 95% of the lithium-containing minerals are spodumene. The low-temperature flotation pulp temperature is 8℃-12℃, and the method includes the following steps:
[0048] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed by a three-stage jaw crusher to obtain crushed mineral material with a maximum particle size of 2mm;
[0049] (2) Grinding treatment: Water and grinding modifier are added to the crushed mineral material in step (1) and the material is ground by ball mill until the content of the fineness of the material is -0.074mm is 70%. Water is added to adjust the concentration of the grinding slurry to 65%. The amount of grinding modifier is 2500g / t based on the dry spodumene ore. The grinding modifier is composed of 1000g / t sodium carbonate and 1500g / t sodium nitrate. The surface modification and dissolution are controlled by electric driving force enhancement under low temperature environment to obtain the grinding slurry.
[0050] (3) Enhanced surface modification and fine mud regulation preparation: Water is added to the grinding slurry in step (2) to adjust the slurry mass concentration to 30%, and then a modifier of 600 g / t based on the dry spodumene ore to be separated is added. The modifier is composed of 400 g / t sodium hydroxide and 200 g / t sodium lignosulfonate. With the help of the inorganic electrolyte added in the grinding step, the OH is enhanced. - The mineral surface is dissolved or scrubbed, while lignin sulfonate, with its selective action on macromolecules, adsorbs and disperses the settled fine mud to mitigate the effects of fine mud in low-temperature slurry. The stirring modification reaction time is 15 min, yielding surface OH... - Enhanced dissolution modification and fine mud-controlled slurry;
[0051] (4) Preparation of mineral metal ion activation and modification: Add 200g / t of magnesium sulfate as metal ion activator to the slurry of the spodumene ore to be separated in step (3), and react for 5min under stirring conditions to obtain ion-activated slurry.
[0052] (5) Mineral collection and mineralization preparation driven by strong electrodynamics: Add (1000+200)+100+30g / t of (sodium oleate + sodium dodecyl sulfonate) + methylene carbonate + sorbitan fatty acid ester as spodumene mineral collector to the ion-activated slurry in step (4), based on the dry spodumene ore to be separated, to carry out the stirring mineralization process of high conductivity separation of spodumene mineral and enhanced emulsification and stable foam. The stirring collection and mineralization reaction time is 5min, and the mineralized slurry to be separated is obtained.
[0053] (6) Low-temperature flotation separation and recovery of lithium minerals: The slurry to be separated after mineralization in step (5) is separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and two scavenging stages. The resulting spodumene-containing concentrate and flotation tailings are then separated. The roughing stage lasts for 3 minutes per stage, the scavenging stage lasts for 3 minutes per stage, and the cleaning stage lasts for 2 minutes per stage. The resulting spodumene-containing concentrate and flotation tailings are then concentrated and filtered to obtain and recover the spodumene concentrate and flotation tailings. Under low-temperature conditions of 8℃-12℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment is 81.3%, and the Li2O content is 5.60%.
[0054] Example 2
[0055] The difference between this embodiment and Example 1 is that the flotation pulp temperature is 8℃-10℃, and calcium chloride is used as the metal ion activator only in the ion activation treatment; other conditions are the same as in Example 1. In this embodiment, the spodumene concentrate product has a Li₂O recovery rate of 81.7% and a Li₂O content of 5.63%.
[0056] Example 3
[0057] The difference between this embodiment and Example 1 is that the flotation pulp temperature is 8℃-10℃, and the collector used is (sodium oleate + sodium dodecyl sulfonate) + aminosulfonamide + sorbitan fatty acid ester = (1000+200)+100+30g / t. Other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this embodiment, the Li₂O recovery rate is 81.3%, and the Li₂O content is 5.68%.
[0058] Example 4
[0059] The difference between this embodiment and Example 1 is that the flotation pulp temperature is 8℃-10℃, and the collector used is (salicyloxyhydroxamic acid + tal oil) + methylene ethylene carbonate + sorbitan fatty acid ester = (1000+200)+100+30g / t. Other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this embodiment, the Li₂O recovery rate is 81.6%, and the Li₂O content is 5.64%.
[0060] Example 5
[0061] The difference between this embodiment and Example 1 is that the flotation pulp temperature is 8℃-10℃, and the collector used is (sodium oleate + sodium dodecyl sulfonate) + methylene ethylene carbonate + propylene glycol monostearate = (1000 + 200) + 100 + 30 g / t. Other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this embodiment, the Li₂O recovery rate is 80.3%, and the Li₂O content is 5.57%.
[0062] Example 6
[0063] This embodiment provides a low-temperature flotation method for spodumene minerals, used to separate low-grade spodumene ore from a high-altitude coastal area in Sichuan Province. The raw ore has a Li₂O content of 1.10%, and 95% of the lithium-containing minerals are spodumene. The low-temperature flotation pulp temperature is 5℃-10℃, and the method includes the following steps:
[0064] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed by a three-stage jaw crusher to obtain crushed mineral material with a maximum particle size of 1 mm.
[0065] (2) Grinding treatment: Water and grinding modifier are added to the crushed mineral material in step (1) and the material is ground by ball mill until the content of the fineness of the material is -0.074mm is 95%. Water is added to adjust the concentration of the grinding slurry to 50%. The amount of grinding modifier is 3500g / t based on the dry spodumene ore raw material. The grinding modifier is composed of 500g / t sodium carbonate and 3000g / t sodium nitrate. The surface modification and dissolution are controlled by electric driving force enhancement under low temperature environment to obtain the grinding slurry.
[0066] (3) Enhanced surface modification and fine mud regulation preparation: Water is added to the grinding slurry in step (2) to adjust the slurry mass concentration to 25%, and then 2000 g / t of modifier is added based on the dry spodumene ore to be separated. The modifier is composed of 1000 g / t of ammonia water and 1000 g / t of potassium lignin sulfonate. With the help of the inorganic electrolyte added during grinding, the OH- oxidant is enhanced. - The mineral surface is dissolved or scrubbed, while lignin sulfonate, with its selective action on macromolecules, adsorbs and disperses the settled fine mud to mitigate the effects of low-temperature slurry fine mud. The stirring modification reaction time is 5 min, yielding surface OH...- Enhanced dissolution modification and fine mud-controlled slurry;
[0067] (4) Preparation of mineral metal ion activation and modification: Add 100g / t of magnesium sulfate as metal ion activator to the slurry of the spodumene ore to be separated in step (3), and react for 10min under stirring conditions to obtain ion-activated slurry.
[0068] (5) Mineral strong electrodynamic driving collection and mineralization preparation: Add (1000+200)+100+30g / t of (stearic acid + sodium dodecyl sulfate) + o-benzoyl sulfonyl imide + diesel as spodumene mineral collector to the ion-activated slurry in step (4), and carry out the stirring mineralization process of high conductivity separation of spodumene mineral and enhanced emulsification and stable foam. The stirring collection and mineralization reaction time is 2min, and the mineralized slurry to be separated is obtained.
[0069] (6) Low-temperature flotation separation and recovery of lithium minerals: The slurry to be separated after mineralization in step (5) is separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and two scavenging stages. The resulting spodumene-containing concentrate and flotation tailings are then separated. The roughing stage lasts for 3 minutes per stage, the scavenging stage lasts for 3 minutes per stage, and the cleaning stage lasts for 2 minutes per stage. The resulting spodumene-containing concentrate and flotation tailings are then concentrated and filtered to obtain and recover the spodumene concentrate and flotation tailings. Under low-temperature conditions of 5℃-10℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment is 78.2%, and the Li2O content is 5.75%.
[0070] Example 7
[0071] This embodiment provides a low-temperature flotation method for spodumene minerals, used to separate low-grade spodumene ore from a high-altitude coastal area in Sichuan Province. The raw ore has a Li₂O content of 1.10%, and 95% of the lithium-containing minerals are spodumene. The low-temperature flotation pulp temperature is 8℃-15℃, and the method includes the following steps:
[0072] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed by a three-stage jaw crusher to obtain crushed mineral material with a maximum particle size of 12mm;
[0073] (2) Grinding treatment: Water and grinding modifier are added to the crushed mineral material in step (1) and the material is ground by ball mill until the content of the fineness of the material is -0.074mm is 50%. Water is added to adjust the concentration of the grinding slurry to 85%. The amount of grinding modifier is 2500g / t based on the dry spodumene ore. The grinding modifier is composed of 500g / t sodium carbonate and 2000g / t sodium nitrate. The surface modification and dissolution are controlled by electric driving force enhancement under low temperature environment to obtain the grinding slurry.
[0074] (3) Enhanced surface modification and fine mud preparation: Water is added to the grinding slurry in step (2) to adjust the slurry mass concentration to 50%. Then, a modifier of 100 g / t based on the dry spodumene ore to be separated is added. The modifier is composed of 50 g / t sodium hydroxide and 50 g / t calcium lignosulfonate. With the help of the inorganic electrolyte added in the grinding step, the OH is enhanced. - The mineral surface is dissolved or scrubbed, while lignin sulfonate, with its selective action on macromolecules, adsorbs and disperses the settled fine mud to mitigate the effects of fine mud in low-temperature slurry. The stirring modification reaction time is 30 min, yielding surface OH... - Enhanced dissolution modification and fine mud-controlled slurry;
[0075] (4) Preparation of mineral metal ion activation and modification: Add 1000g / t of magnesium sulfate as metal ion activator to the slurry of the spodumene ore to be separated in step (3), and react for 2min under stirring conditions to obtain ion-activated slurry.
[0076] (5) Mineral strong electrodynamic driving collection and mineralization preparation: Add (1000+200)+100+30g / t of (cycloalkane soap + benzoyl hydroxyxamic acid)+N,N-dimethylacetamide + ethylene glycol monostearate as spodumene mineral collector to the ion-activated slurry in step (4), and carry out the high conductivity separation of spodumene mineral, enhanced emulsification and stable foam stirring mineralization process. The stirring collection mineralization reaction time is 10min, and the mineralized slurry to be separated is obtained.
[0077] (6) Low-temperature flotation separation and recovery of lithium minerals: The slurry to be separated after mineralization in step (5) is separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and two scavenging stages. The resulting spodumene-containing concentrate and flotation tailings are then separated. The roughing stage lasts 6 minutes per stage, the scavenging stage lasts 6 minutes per stage, and the cleaning stage lasts 4 minutes per stage. The resulting spodumene-containing concentrate and flotation tailings are then concentrated and filtered to obtain and recover the spodumene concentrate and flotation tailings. Under low-temperature conditions of 8℃-12℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment is 77.5%, and the Li2O content is 5.70%.
[0078] Comparative Example 1
[0079] The difference between this comparative example and Example 1 is that, in the grinding process, the grinding modifier of 1000 g / t sodium carbonate + 1500 g / t sodium nitrate was replaced with 1000 g / t sodium carbonate; other conditions were the same as in Example 1. The spodumene concentrate product obtained in this comparative example had a Li₂O recovery rate of 64.2% and a Li₂O content of 5.20%.
[0080] Comparative Example 2
[0081] The difference between this comparative example and Example 1 is that, in the grinding process, the grinding modifier of 1000 g / t sodium carbonate + 1500 g / t sodium nitrate was replaced with 1000 g / t sodium hydroxide; other conditions were the same as in Example 1. The spodumene concentrate product obtained in this comparative example had a Li₂O recovery rate of 75.7% and a Li₂O content of 5.62%.
[0082] Comparative Example 3
[0083] The difference between this comparative example and Example 1 is that, in the grinding process, the grinding modifier of 1000 g / t sodium carbonate + 1500 g / t sodium nitrate was replaced with 200 g / t sodium lignosulfonate (because a high amount of sodium lignosulfonate would inhibit spodumene mineralization, the amount of sodium lignosulfonate was controlled within the range of 200-400 g / t). Other conditions were the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li2O recovery rate was 77.3%, and the Li2O content was 5.65%.
[0084] Comparative Example 4
[0085] The difference between this comparative example and Example 1 is that sodium lignosulfonate was not added during the modification treatment; all other conditions were the same as in Example 1. The spodumene concentrate product obtained in this comparative example had a Li₂O recovery rate of 80.2% and a Li₂O content of 5.40%.
[0086] Comparative Example 5
[0087] The difference between this comparative example and Example 1 is that only 1000 g / t of sodium carbonate was added during the grinding process, and 1500 g / t of sodium nitrate was added during the modification process after slurry conditioning. All other conditions were the same as in Example 1. The spodumene concentrate product obtained in this comparative example had a Li₂O recovery rate of 76.8% and a Li₂O content of 5.56%.
[0088] Comparative Example 6
[0089] The difference between this comparative example and Example 1 is that, in the mineralization process, the spodumene mineral collector consisting of (1000+200)+100+30 g / t of (sodium oleate + sodium dodecyl sulfonate) + methylene carbonate + sorbitan fatty acid ester was replaced with (1000+200)+30 g / t of (sodium oleate + sodium dodecyl sulfonate) + sorbitan fatty acid ester; that is, the strong organic electrolyte component (methylene carbonate) was not added. All other conditions were the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li2O recovery rate was 74.3%, and the Li2O content was 5.55%.
[0090] Comparative Example 6
[0091] The difference between this comparative example and Example 1 is that, in the mineralization process, the spodumene mineral collector of (1000+200)+100+30 g / t (sodium oleate + sodium dodecyl sulfonate) + ethylene methylene carbonate + sorbitan fatty acid ester is replaced with (1000+200)+100 g / t (sodium oleate + sodium dodecyl sulfonate) + ethylene methylene carbonate; that is, no emulsifier (sorbitan fatty acid ester) is added. Other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li2O recovery rate is 78.3%, and the Li2O content is 5.36%.
[0092] According to the test results of Examples 1-7 and Comparative Examples 1-6, compared with the technical solution of Example 1 of the present invention, the following comparisons show a significant reduction in flotation effect: Comparative Example 1, which adds only sodium carbonate without strengthening acid salts during grinding; Comparative Example 5, which adds strong acid salts during modification; Comparative Example 2, which adds only sodium hydroxide without strengthening acid salts during grinding; Comparative Example 3, which adds only lignin sulfonate without strengthening acid salts during grinding; Comparative Example 4, which does not add sodium lignin sulfonate during modification; Comparative Example 6, which does not add organic strong electrolytes during mineralization; and Comparative Example 7, which does not add emulsifiers.
[0093] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A low-temperature flotation method for spodumene minerals, characterized in that, include: The spodumene ore to be sorted is crushed to obtain crushed mineral materials; Water is added to crushed mineral materials and the materials are ground to dissociate the minerals. A grinding modifier is added during the grinding process to obtain a grinding slurry. The grinding modifier includes a first modifier component and a strong acid salt. The first modifier component is at least one of carbonate, percarbonate, and caustic alkali. The grinding slurry is conditioned, then modified with a modifier, followed by ion activation with a metal ion activator, and finally mineralized with a spodumene mineral collector. The spodumene concentrate and flotation tailings are then obtained. The modifier includes highly active OH groups. - Modifiers and lignin sulfonates; the spodumene mineral collector includes anionic surfactants, strong organic electrolyte components, and emulsifiers; The first adjusting component is at least one of sodium carbonate, potassium carbonate, ammonium carbonate, sodium percarbonate, sodium hydroxide, and potassium hydroxide. The strong acid salt is a sulfate and / or nitrate; the strong acid salt is at least one of sodium sulfate, potassium sulfate, sodium nitrate, and potassium nitrate. The maximum particle size of the crushed mineral material is 1-12 mm; The grinding process is described to achieve a mineral fineness of -0.074 mm, with a content of 50-95%. Based on a weight of 1 t of dry spodumene ore to be sorted, the amount of grinding modifier is 100-4000 g, of which the amount of the first modifier component is 100-2000 g and the amount of strong acid salt is 300-3500 g. And / or, the mass concentration of the grinding slurry is 50-85%.
2. The low-temperature flotation method according to claim 1, characterized in that, The mass concentration of the grinding slurry after the slurry conditioning treatment is 25-50%; And / or, the slurry conditioning agent used in the slurry conditioning process is water; And / or, the highly active OH - The modifier is at least one of caustic soda, ammonia, and organic amines; the caustic soda is sodium hydroxide and / or potassium hydroxide. And / or, the lignin sulfonate is at least one of sodium lignin sulfonate, potassium lignin sulfonate, calcium lignin sulfonate, magnesium lignin sulfonate, and ammonium lignin sulfonate.
3. The low-temperature flotation method according to claim 1, characterized in that, Based on a weight of 1 t of dry spodumene ore to be sorted, the amount of the modifier is 100-2000 g, wherein the highly active OH... - The dosage of the modifier is 50-2000 g, and the dosage of the lignin sulfonate is 50-2000 g; And / or, the duration of the modification treatment is 5-30 min.
4. The low-temperature flotation method according to claim 1, characterized in that, The metal ion activator is a calcium ion modifier and / or a magnesium ion modifier; the metal ion activator is at least one of calcium sulfate, calcium nitrate, calcium chloride, magnesium sulfate, magnesium nitrate, and magnesium chloride. And / or, based on the weight of 1 t of dry spodumene ore to be sorted, the amount of the metal ion activator is 100-1000 g; And / or, the duration of the ion activation treatment is 2-10 min.
5. The low-temperature flotation method according to claim 1, characterized in that, The anionic surfactant is at least one of alkyl carboxylates and their derivatives, alkyl sulfonates and their derivatives, alkyl sulfates and their derivatives, and hydroxamic acid salts and their derivatives; And / or, the organic strong electrolyte component is at least one of carbonates, amides, and acrylates; And / or, the emulsifier is a neutral oil or / and ester organic compound.
6. The low-temperature flotation method according to claim 5, characterized in that, The anionic surfactant is at least one of oleic acid, sodium oleate, stearic acid, palmitic acid, lauric acid, tal oil, naphthenic acid soap, sodium dodecylbenzenesulfonate, sodium dodecyl sulfonate, sodium dodecyl sulfate, benzoyl hydroxamic acid, and salicylic acid. And / or, the organic strong electrolyte component is at least one of polycarbonate, dimethyl carbonate, ethyl carbonate, vinylene carbonate, vinyl ethylene carbonate, methylene ethylene carbonate, vinyl ethylene carbonate, N-methylformamide, N,N-dimethylacetamide, conjugated sulfonamide, aminosulfonamide, o-benzoylsulfonylimide, and vinyl sulfite. And / or, the emulsifier is at least one of kerosene, diesel oil, propylene glycol monostearate, propylene glycol alginate, ethylene glycol monostearate, glyceryl stearate, and sorbitan fatty acid ester.
7. The low-temperature flotation method according to claim 1, characterized in that, Based on a weight of 1 t of dry spodumene ore to be sorted, the amount of spodumene mineral collector used is 100-4000 g. And / or, the mass ratio of the anionic surfactant, the organic strong electrolyte component, and the emulsifier is 1:(0.05-0.2):(0.02-0.1); And / or, the duration of the mineralization treatment is 2-10 min.
8. The low-temperature flotation method according to claim 1, characterized in that, The flotation separation adopts a mineral flotation process combining roughing, cleaning, and scavenging. And / or, the flotation separation is followed by concentration and compression processing; And / or, the temperature of the flotation pulp in the flotation separation is 5-19℃.
9. The low-temperature flotation method according to claim 8, characterized in that, The coarse selection process takes 3-6 minutes per stage. And / or, the sorting time for each selected segment is 2-4 minutes; And / or, the sorting time for each segment of the scanning process is 3-6 minutes.
Citation Information
Patent Citations
Pegmatite-type spodumene flotation collecting agent and preparation method and application thereof
CN109225648A
Method for grinding and floating separation of lithium ore and lithium concentrate product
CN117019407A