A hydrophobically modified alkali-swellable associative thickener and preparation method thereof
Through the synthesis of modified polyols and modified styrene, combined with silicone segments and ammonium carboxylate structure, the problem of poor film formation performance of traditional thickeners at low temperatures is solved, and a stable film formation is achieved at low temperatures is achieved The layering and viscosity increase, enhancing the stability and durability of the thickener.
Patent Information
- Application Number
- CN202410568926.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-09
AI Technical Summary
Traditional alkali-swelling associative thickeners have poor film forming performance under low temperature conditions, resulting in cracking and peeling of the coating, affecting the product's use effect and durability.
Through the synthesis of modified polyols and modified styrene, polymers with polyolefin double bond modification and long alkane linear modification are formed, combining silicone segments and ammonium carboxylate structure to improve the viscosity and stability of the thickener enhances its film forming properties at low temperatures.
A uniform and stable film layer is achieved at low temperature, reducing the film formation temperature, improving the viscosity and stability of the thickener, enhancing the interaction and adhesion with the substrate, avoiding the cracking of the coating and Peel off.
Smart Images

Figure CN118290676B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thickener processing, and in particular to a hydrophobically modified alkali-swellable associative thickener and a preparation method thereof. Background Art
[0002] As an important chemical additive, thickeners have been widely used in many fields such as coatings, inks, adhesives and cosmetics. Among the many thickeners, alkali-swellable associative thickeners have attracted widespread attention due to their unique thickening mechanism and excellent performance. However, with the continuous advancement of industrial technology and changes in market demand, traditional alkali-swellable associative thickeners can no longer meet the growing performance requirements.
[0003] In the prior art, a Chinese invention patent with a publication number of CN101787231B discloses a hydrophobically modified associative thickener and a preparation method thereof, which is prepared by free radical emulsion polymerization of a hydrophobically modified monomer (such as SEM-25) and an unsaturated carboxylic acid monomer and a monoethylenically unsaturated monomer without a carboxylic acid group. The obtained associative thickener can effectively increase the viscosity of the water-based coating and improve the shear resistance of the water-based coating. The thickener of the present invention can obtain a better thickening effect at a lower usage amount. The thickener can be added to the water-based coating to meet the different viscosity requirements of the water-based coating during different uses.
[0004] The traditional thickeners for water-based base materials are mainly based on how to improve their viscosity in water-based base materials. Although thickeners can improve the viscosity of water-based base materials, as the temperature decreases, the viscosity of the thickeners will increase, resulting in excessively high viscosity of the system, affecting the workability and stability of the product. Alkali-swellable associative thickeners form a three-dimensional network structure through associative action, thereby giving the system a thickening effect.
[0005] However, the film-forming temperature of the alkali-swellable associative thickener in the prior art is usually around 40°C. At low temperatures, the movement of the alkali-swellable associative thickener molecules slows down, the interaction between the thickener and the solvent or substrate decreases, and the associative effect weakens, causing the network structure to become loose and unable to effectively support the formation of the film layer and maintain its stability. Traditional alkali-swellable associative thickeners are difficult to form a uniform and stable film layer under low temperature conditions, resulting in cracking and peeling of the coating, which seriously affects the use effect and durability of the product. Summary of the invention
[0006] The object of the present invention is to provide a hydrophobically modified alkali-swellable associative thickener and a preparation method thereof, so as to solve the technical problem that the viscosity of the alkali-swellable associative thickener in the prior art is greatly affected by temperature and the film-forming performance is poor in a low temperature environment.
[0007] The object of the present invention can be achieved by the following technical scheme: A method for preparing a hydrophobically modified alkali-swellable associative thickener comprises the following steps:
[0008] S1, adding polyol and toluene into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to 55-65° C., adding 3-isocyanate propylene solution dropwise into the reactor, and after the addition is complete, heat-retaining the reaction for 50-90 minutes, and post-treating to obtain a modified polyol;
[0009] The synthetic reaction principle of the modified polyol is as follows: the hydroxyl group on the polyol is used as the active site, the isocyanate group on 3-isocyanate propylene reacts with the hydroxyl group to form a modified polyol having a polyolefin double bond modified polyol.
[0010] S2, adding 3-(2,4-dichlorophenyl)-1-propylene, stearyl alcohol, N,N-dimethylformamide and potassium carbonate into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to 85-95° C., keeping the temperature for reaction for 22-24 hours, and post-treating to obtain modified styrene propene;
[0011] The synthetic reaction principle of modified styrene is as follows: 3-(2,4-dichlorophenyl)-1-propylene and stearyl alcohol are used as a solution in N,N-dimethylformamide, potassium carbonate is used as a catalyst and an acid-binding agent, and the hydroxyl group on stearyl alcohol undergoes a nucleophilic substitution reaction with the halogen on 3-(2,4-dichlorophenyl)-1-propylene, so that stearyl alcohol replaces the halogen on 3-(2,4-dichlorophenyl)-1-propylene to obtain modified styrene with a long alkane straight chain modified styrene.
[0012] S3. Add emulsion, acrylic acid, modified styrene, modified polyol and initiator into the reactor and stir. Raise the temperature of the reactor to 60-70°C and keep the reaction for 4-6 hours. Lower the temperature of the reactor to room temperature and drop ammonia water into the reactor to adjust the pH of the system to 6-7. Post-treat to obtain a thickener.
[0013] The synthetic reaction principle of the thickener is: under the action of emulsion and initiator, acrylic acid, modified styrene, and modified polyol undergo free radical polymerization to prepare multi-crosslinked polyolefins, and the pH of the reaction system is conditioned by ammonia water to form carboxylic acid ammonium salt on the polyolefin.
[0014] Furthermore, in step S1, the usage ratio of the polyol, toluene and 3-isocyanate propylene solution is 1g:5mL:2g, the 3-isocyanate propylene solution is composed of 3-isocyanate propylene and toluene in a weight ratio of 1:2, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is increased to 75-85°C, and the solvent is evaporated under reduced pressure to obtain a modified polyol.
[0015] Furthermore, in step S2, the amount ratio of the 3-(2,4-dichlorophenyl)-1-propylene and stearyl alcohol is 1 mol:2.1 mol, the amount ratio of the 3-(2,4-dichlorophenyl)-1-propylene, N,N-dimethylformamide and potassium carbonate is 2g:7mL:1g, and the post-treatment operation includes: after the reaction is completed, the reactor is kept warm at 85-95°C, the solvent is evaporated under reduced pressure, the temperature of the reactor is lowered to room temperature, petroleum ether is added to the reactor, the reactor is heated to reflux, the temperature is kept warm and stirred for 20-30 minutes, the temperature of the reactor is lowered to room temperature, and the filter is filtered, the filter cake is washed with petroleum ether 3 times and then dried, and the filter cake is transferred to a drying oven at a temperature of 55-65°C, and dried to constant weight to obtain modified styrene propene.
[0016] Furthermore, in step S3, the emulsion is prepared by mixing purified water, tetrahydrofuran and Span 80 in a ratio of 45-55 mL: 30-40 mL: 1-2 g, the emulsion, acrylic acid, modified styrene, modified polyol and initiator in a ratio of 85-95 mL: 5-7 g: 8-10 g: 12-14 g: 1-2 g, the initiator is ammonium persulfate, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is increased to 70-80° C., and the solvent is evaporated under reduced pressure to obtain a thickener.
[0017] Further, the polyol is processed by the following steps:
[0018] A1, ethylene glycol, glycerol, D-mannitol, modified siloxane, cis-2,3-butylene oxide and potassium hydroxide are added to a nitrogen-protected autoclave and stirred, the temperature of the autoclave is increased to 115-125° C., the pressure is increased to 0.1-0.2 MPa, and the reaction is carried out at this temperature until the hydroxyl value of the reaction system reaches 18-20 mgKOH / g, and the intermediate I is obtained by post-treatment;
[0019] The synthesis reaction principle of intermediate I is as follows: cis-2,3-butylene oxide undergoes a ring-opening reaction under the catalysis of potassium hydroxide, and undergoes nucleophilic addition with the hydroxyl groups on ethylene glycol, glycerol, D-mannitol, and modified siloxane to generate new hydroxyl compounds.
[0020] A2. Add intermediate I, butadiene dioxide and a catalyst into a nitrogen-protected autoclave and stir. Raise the temperature of the autoclave to 140-160° C., control the pressure of the autoclave to be lower than 0.4 MPa, maintain the temperature until the pressure of the autoclave reaches equilibrium, and heat the reaction for 20-24 hours. Post-treat to obtain polyol.
[0021] The synthetic reaction principle of polyol is as follows: intermediate I itself contains multiple hydroxyl groups. During the reaction, the hydroxyl groups between the intermediate I molecules undergo condensation to form longer polymer chain segments. The epoxy groups on butadiene dioxide undergo a ring-opening reaction under the action of a catalyst and react with the hydroxyl groups on the intermediate I or the polymer chain segments, thereby forming a multi-cross-linked polymer structure.
[0022] Further, in step A1, the amount ratio of ethylene glycol, glycerol, D-mannitol, modified siloxane, and cis-2,3-butylene oxide is 2 mol:1 mol:1 mol:1 mol:15 mol, and the weight ratio of ethylene glycol to potassium hydroxide is 3:2. The post-treatment operation includes: after the reaction is completed, the reactor is kept at 115-125°C, low-boiling substances are evaporated under reduced pressure, the temperature of the high-pressure reactor is lowered to room temperature, anhydrous ethanol is added to the high-pressure reactor, stirred at room temperature for 20-30 minutes, filtered, and the filtrate is transferred to a water bath at a temperature of 65-7 5° C., and distilling off the solvent under reduced pressure to obtain intermediate I; in step A2, the weight ratio of the intermediate I, butadiene dioxide and the catalyst is 10-12:4-7:0.2-0.3, and the catalyst is a DMC bimetallic catalyst, and the post-treatment operation includes: after the reaction is completed, distilling off low-boiling substances under reduced pressure, lowering the temperature of the high-pressure reactor to room temperature, adding anhydrous ethanol to the high-pressure reactor, stirring at room temperature for 20-30 minutes, filtering, and transferring the filtrate to a rotary evaporator with a water bath temperature of 65-75° C., and distilling off the solvent under reduced pressure to obtain a polyol.
[0023] Furthermore, the preparation method of modified siloxane is: add 1,11-dihydrododecamethylhexasiloxane, 5-hexene-1,2-diol, toluene and a catalyst into a nitrogen-protected reaction and stir, raise the temperature of the reactor to 75-85°C, keep the reaction warm for 10-12 hours, and post-treat to obtain modified siloxane.
[0024] The synthetic reaction principle of modified siloxane is as follows: under catalyst conditions, the end-capping hydrogen of 1,11-dihydrododecamethylhexasiloxane reacts with the olefin double bond on 5-hexene-1,2-diol to form 1,2-hexanediol modification on the siloxane chain segment.
[0025] Furthermore, the amount ratio of 1,11-dihydrododecylhexasiloxane and 5-hexene-1,2-diol is 1 mol:2 mol, the amount ratio of 1,11-dihydrododecylhexasiloxane, toluene and catalyst is 4 g:15 mL:0.2 g, the catalyst is platinum carbon, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, and the filtrate is transferred to a rotary evaporator at a temperature of 70-80°C, and toluene is evaporated under reduced pressure to obtain modified siloxane.
[0026] A hydrophobically modified alkali-swellable associative thickener is prepared by a method for preparing a hydrophobically modified alkali-swellable associative thickener.
[0027] The present invention has the following beneficial effects:
[0028] 1. The hydrophobically modified alkali-swellable associative thickener of the present invention is prepared by a nucleophilic addition reaction of hydroxyl groups on ethylene glycol, glycerol, D-mannitol or modified siloxane after ring opening of cis-2,3-butylene oxide to form a new intermediate I. The intermediate I and dibutylene dioxide undergo polycondensation and nucleophilic addition reaction under the action of a catalyst to prepare a multi-crosslinked polymer structure having a siloxane segment-modified polyol copolymer structure; by selecting ethylene glycol, glycerol and D-mannitol as polyols, a three-dimensional structure in which polyols containing siloxane blocks are cross-linked with each other is constructed with the spatial configuration of different polyols to improve the viscosity of the polymer, and the siloxane segment usually has a lower polarity and a higher flexibility, which helps to improve the interaction and entanglement between polymers and increase the viscosity of the polymer. The embedding of the polysiloxane segment can also effectively reduce the crystallization of the polyol in a low temperature environment, thereby improving the stability of the thickener at low temperatures.
[0029] 2. The hydrophobically modified alkali-swellable associative thickener of the present invention is obtained by free radical polymerization of modified styrene-propylene modified with long alkane straight chain, modified polyol modified with polyolefin double bond and acrylic acid under the condition of initiator, and neutralization reaction of free ammonia with carboxyl groups on the multipolymer forms carboxylic acid ammonium structure, thereby obtaining a thickener with multi-component associative structure; stearyl alcohol is embedded as a hydrophobic long alkane straight chain, which not only effectively improves the hydrophobic property of the thickener, but also the long alkane straight chain cooperates with polysilane with good flexibility and low temperature resistance to prevent cracking and peeling of the film layer at low temperature, and at the same time, the introduction of polysilane chain segment also improves the wettability and adhesion of the thickener to the substrate, so that the thickener can form a stable interaction with the solvent or substrate at a lower temperature, thereby being easier to form a continuous film structure at low temperature, reducing the film forming temperature of the thickener, and, The introduction of long alkane straight chains and the cross-linked structure of polyolefins increase the interaction force between polymer molecules, so that the polymer solution can generate greater internal friction when subjected to shear force, thereby increasing the viscosity; ammonium carboxylate has good water solubility, which makes the polymer easier to disperse and dissolve in the aqueous system, enhances the hydrophilicity of the thickener, and makes the thickener more evenly distributed in the aqueous system, thereby improving its stability and low-temperature film-forming performance; ammonium carboxylate, as an ionic compound, can dissociate into positively charged ammonium ions and negatively charged carboxylate ions in aqueous solution, so that the thickener has a higher solubility in the solvent, reduces the effect of low temperature on the association of the thickener in the aqueous matrix, and helps to promote the thickener to form a uniform and stable film layer at low temperature. In addition, the interaction between ammonium carboxylate ions produces a charge shielding effect, which enhances the mutual attraction between polymer molecular chains and increases the viscosity of the polymer solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a photograph of the film-forming state of the thickener prepared in Example 3 of the present invention;
[0032] Figure 2 This is a photograph of the film-forming state of the thickener prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment provides a method for preparing a hydrophobically modified alkali-swellable associative thickener, comprising the following steps:
[0036] S1. Preparation of modified siloxane
[0037] Weigh: 43.1 g of 1,11-dihydrododecamethylhexasiloxane, 23.2 g of 5-hexene-1,2-diol, 162 mL of toluene and 2.2 g of platinum carbon, add to a nitrogen-protected reaction mixture and stir, raise the temperature of the reactor to 75°C, and keep the reaction warm for 10 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, and transfer the filtrate to a rotary evaporator at 70°C, and evaporate the toluene under reduced pressure to obtain modified siloxane.
[0038] S2. Preparation of polyols
[0039] Weigh: 124.1 g of ethylene glycol, 92.1 g of glycerol, 182.2 g of D-mannitol, 663.3 g of modified siloxane, 1081.6 g of cis-2,3-butylene oxide and 82.7 g of potassium hydroxide, add them into a nitrogen-protected autoclave and stir, the temperature of the autoclave is increased to 115° C., the pressure is increased to 0.1 MPa, and the reaction is kept warm until the hydroxyl value of the reaction system reaches 18 mgKOH / g. After the reaction is completed, the autoclave is kept warm at 115° C., low-boiling substances are evaporated under reduced pressure, the temperature of the autoclave is lowered to room temperature, 1000 mL of anhydrous ethanol is added to the autoclave, stirred at room temperature for 20 min, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 65° C., and the solvent is evaporated under reduced pressure to obtain intermediate I;
[0040] Weigh: 200g of intermediate I, 80g of butadiene dioxide and 4g of DMC bimetallic catalyst are added to a nitrogen-protected autoclave and stirred. The temperature of the autoclave is increased to 140°C, and the pressure of the autoclave is increased. When the internal pressure of the autoclave is higher than 0.4MPa, the autoclave is depressurized by controlling the autoclave through a valve so that the internal pressure of the autoclave is lower than 0.4MPa. The temperature is maintained. After the pressure of the autoclave reaches equilibrium, the reaction is kept warm for 20h. After the reaction is completed, low-boiling substances are evaporated under reduced pressure. The temperature of the autoclave is lowered to room temperature, 800mL of anhydrous ethanol is added to the autoclave, stirred at room temperature for 20min, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 65°C, and the solvent is evaporated under reduced pressure to obtain a polyol.
[0041] S3. Preparation of modified polyols
[0042] Mix 3-isocyanate propylene and toluene in a weight ratio of 1:2 to obtain a 3-isocyanate propylene solution for later use;
[0043] Weigh: 500 g of polyol and 2500 mL of toluene are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 55° C. 1000 g of 3-isocyanate propylene solution is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 50 minutes. After the reaction is completed, the temperature of the reactor is raised to 75° C., and the solvent is evaporated under reduced pressure to obtain a modified polyol.
[0044] S4. Preparation of modified styrene
[0045] Weigh: 187.1 g of 3-(2,4-dichlorophenyl)-1-propene, 568.0 g of stearyl alcohol, 655 mL of N,N-dimethylformamide and 93.6 g of potassium carbonate, add into a nitrogen-protected reactor and stir, raise the reactor temperature to 85°C, keep warm for 22 hours, after the reaction is completed, keep the reactor warm at 85°C, evaporate the solvent under reduced pressure, lower the reactor temperature to room temperature, add 1200 mL of petroleum ether into the reactor, raise the reactor temperature to system reflux, keep warm and stir for 20 minutes, lower the reactor temperature to room temperature, filter, wash the filter cake with petroleum ether 3 times and then dry, transfer the filter cake to a drying oven at 55°C, dry to constant weight, and obtain modified styrene propene.
[0046] S5. Preparation of thickener
[0047] Mix purified water, tetrahydrofuran and Span 80 in a ratio of 45 mL:30 mL:1 g to obtain an emulsion for later use;
[0048] Weigh: 850 mL of emulsion, 50 g of acrylic acid, 80 g of modified styrene, 120 g of modified polyol and 10 g of ammonium persulfate, add into a reactor and stir, raise the temperature of the reactor to 60°C, keep warm and react for 4 hours, lower the temperature of the reactor to room temperature, add ammonia water dropwise into the reactor, adjust the pH of the system to 6, after the reaction is completed, raise the temperature of the reactor to 70°C, evaporate the solvent under reduced pressure to obtain a thickener.
[0049] Example 2
[0050] This embodiment provides a method for preparing a hydrophobically modified alkali-swellable associative thickener, comprising the following steps:
[0051] S1. Preparation of modified siloxane
[0052] Weigh: 43.1 g of 1,11-dihydrododecamethylhexasiloxane, 23.2 g of 5-hexene-1,2-diol, 162 mL of toluene and 2.2 g of platinum carbon, add to a nitrogen-protected reaction mixture and stir, raise the temperature of the reactor to 80°C, and keep the reaction warm for 11 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, and transfer the filtrate to a rotary evaporator at 75°C, and evaporate the toluene under reduced pressure to obtain modified siloxane.
[0053] S2. Preparation of polyols
[0054] Weigh: 124.1 g of ethylene glycol, 92.1 g of glycerol, 182.2 g of D-mannitol, 663.3 g of modified siloxane, 1081.6 g of cis-2,3-butylene oxide and 82.7 g of potassium hydroxide, add them into a nitrogen-protected autoclave and stir, the temperature of the autoclave is increased to 120° C., the pressure is increased to 0.15 MPa, and the reaction is kept warm until the hydroxyl value of the reaction system reaches 19 mgKOH / g. After the reaction is completed, the autoclave is kept warm at 120° C., low-boiling substances are evaporated under reduced pressure, the temperature of the autoclave is lowered to room temperature, 1000 mL of anhydrous ethanol is added to the autoclave, stirred at room temperature for 25 min, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 70° C., and the solvent is evaporated under reduced pressure to obtain intermediate I;
[0055] Weigh: 220 g of intermediate I, 110 g of butadiene dioxide and 5 g of DMC bimetallic catalyst are added to a nitrogen-protected autoclave and stirred. The temperature of the autoclave is increased to 150° C., and the pressure of the autoclave is increased. When the internal pressure of the autoclave is higher than 0.4 MPa, the autoclave is depressurized by controlling the autoclave through a valve so that the internal pressure of the autoclave is lower than 0.4 MPa. The temperature is maintained. After the pressure of the autoclave reaches equilibrium, the reaction is kept warm for 22 hours. After the reaction is completed, low-boiling substances are evaporated under reduced pressure. The temperature of the autoclave is lowered to room temperature. 800 mL of anhydrous ethanol is added to the autoclave, stirred at room temperature for 25 minutes, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 70° C., and the solvent is evaporated under reduced pressure to obtain a polyol.
[0056] S3. Preparation of modified polyols
[0057] Mix 3-isocyanate propylene and toluene in a weight ratio of 1:2 to obtain a 3-isocyanate propylene solution for later use;
[0058] Weigh: 500 g of polyol and 2500 mL of toluene are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 60° C. 1000 g of 3-isocyanate propylene solution is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 70 minutes. After the reaction is completed, the temperature of the reactor is raised to 80° C., and the solvent is evaporated under reduced pressure to obtain a modified polyol.
[0059] S4. Preparation of modified styrene
[0060] Weigh: 187.1 g of 3-(2,4-dichlorophenyl)-1-propene, 568.0 g of stearyl alcohol, 655 mL of N,N-dimethylformamide and 93.6 g of potassium carbonate, add them into a nitrogen-protected reactor and stir, raise the reactor temperature to 90°C, and keep the temperature for reaction for 23 hours. After the reaction is completed, keep the reactor at 90°C, evaporate the solvent under reduced pressure, lower the reactor temperature to room temperature, add 1200 mL of petroleum ether to the reactor, raise the reactor temperature to system reflux, keep the temperature and stir for 25 minutes, lower the reactor temperature to room temperature, filter, wash the filter cake with petroleum ether 3 times and then dry it, transfer the filter cake to a drying oven at 60°C, and dry it to constant weight to obtain modified styrene propene.
[0061] S5. Preparation of thickener
[0062] Purified water, tetrahydrofuran and Span 80 were mixed uniformly in a ratio of 50 mL:35 mL:1.5 g to obtain an emulsion for later use;
[0063] Weigh: 900 mL of emulsion, 60 g of acrylic acid, 90 g of modified styrene, 130 g of modified polyol and 15 g of ammonium persulfate, add into a reactor and stir, raise the temperature of the reactor to 65°C, keep warm for 5 hours, lower the temperature of the reactor to room temperature, add ammonia water dropwise into the reactor, adjust the pH value of the system to 6.5, raise the temperature of the reactor to 75°C after the reaction is completed, evaporate the solvent under reduced pressure to obtain a thickener.
[0064] Example 3
[0065] This embodiment provides a method for preparing a hydrophobically modified alkali-swellable associative thickener, comprising the following steps:
[0066] S1. Preparation of modified siloxane
[0067] Weigh: 43.1 g of 1,11-dihydrododecamethylhexasiloxane, 23.2 g of 5-hexene-1,2-diol, 162 mL of toluene and 2.2 g of platinum carbon, add to a nitrogen-protected reaction and stir, raise the temperature of the reactor to 85°C, and keep the reaction warm for 12 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, and transfer the filtrate to a rotary evaporator at 80°C, and evaporate the toluene under reduced pressure to obtain modified siloxane.
[0068] S2. Preparation of polyols
[0069] Weigh: 124.1 g of ethylene glycol, 92.1 g of glycerol, 182.2 g of D-mannitol, 663.3 g of modified siloxane, 1081.6 g of cis-2,3-butylene oxide and 82.7 g of potassium hydroxide, add them into a nitrogen-protected autoclave and stir, the temperature of the autoclave is increased to 125° C., the pressure is increased to 0.2 MPa, and the reaction is kept warm until the hydroxyl value of the reaction system reaches 20 mgKOH / g. After the reaction is completed, the autoclave is kept warm at 125° C., low-boiling substances are evaporated under reduced pressure, the temperature of the autoclave is lowered to room temperature, 1000 mL of anhydrous ethanol is added to the autoclave, stirred at room temperature for 30 min, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 75° C., and the solvent is evaporated under reduced pressure to obtain intermediate I;
[0070] Weigh: 240 g of intermediate I, 140 g of butadiene dioxide and 6 g of DMC bimetallic catalyst are added to a nitrogen-protected autoclave and stirred. The temperature of the autoclave is increased to 160° C., and the pressure of the autoclave is increased. When the internal pressure of the autoclave is higher than 0.4 MPa, the autoclave is depressurized by controlling the autoclave through a valve so that the internal pressure of the autoclave is lower than 0.4 MPa. The temperature is maintained. After the pressure of the autoclave reaches equilibrium, the reaction is kept warm for 24 hours. After the reaction is completed, low-boiling substances are evaporated under reduced pressure. The temperature of the autoclave is lowered to room temperature. 800 mL of anhydrous ethanol is added to the autoclave, and the mixture is stirred at room temperature for 30 minutes. The filtrate is transferred to a rotary evaporator with a water bath temperature of 75° C., and the solvent is evaporated under reduced pressure to obtain a polyol.
[0071] S3. Preparation of modified polyols
[0072] Mix 3-isocyanate propylene and toluene in a weight ratio of 1:2 to obtain a 3-isocyanate propylene solution for later use;
[0073] Weigh: 500 g of polyol and 2500 mL of toluene are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 65° C. 1000 g of 3-isocyanate propylene solution is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 90 minutes. After the reaction is completed, the temperature of the reactor is raised to 85° C., and the solvent is evaporated under reduced pressure to obtain a modified polyol.
[0074] S4. Preparation of modified styrene
[0075] Weigh: 187.1 g of 3-(2,4-dichlorophenyl)-1-propene, 568.0 g of stearyl alcohol, 655 mL of N,N-dimethylformamide and 93.6 g of potassium carbonate, add into a nitrogen-protected reactor and stir, raise the reactor temperature to 95°C, keep warm for 24 hours, after the reaction is completed, keep the reactor warm at 95°C, evaporate the solvent under reduced pressure, lower the reactor temperature to room temperature, add 1200 mL of petroleum ether into the reactor, raise the reactor temperature to system reflux, keep warm and stir for 30 minutes, lower the reactor temperature to room temperature, filter, wash the filter cake with petroleum ether 3 times and then dry, transfer the filter cake to a drying oven at 65°C, dry to constant weight, and obtain modified styrene propene.
[0076] S5. Preparation of thickener
[0077] Purified water, tetrahydrofuran and Span 80 were mixed uniformly in a ratio of 55 mL:40 mL:2 g to obtain an emulsion for later use;
[0078] Weigh: 950 mL of emulsion, 70 g of acrylic acid, 100 g of modified styrene, 140 g of modified polyol and 20 g of ammonium persulfate, add into a reactor and stir, raise the temperature of the reactor to 70°C, keep warm for 6 hours, lower the temperature of the reactor to room temperature, add ammonia water dropwise into the reactor, adjust the pH value of the system to 7, after the reaction is completed, raise the temperature of the reactor to 80°C, evaporate the solvent under reduced pressure to obtain a thickener.
[0079] Comparative Example 1
[0080] The difference between this comparative example and Example 3 is that step S1 is omitted and modified siloxane is not added in step S2.
[0081] Comparative Example 2
[0082] The difference between this comparative example and Example 3 is that in step S2, D-mannitol is not added.
[0083] Comparative Example 3
[0084] The difference between this comparative example and Example 3 is that step S4 is eliminated, and the modified styrene propene in step S5 is replaced by styrene propene.
[0085] Comparative Example 4
[0086] The difference between this comparative example and Example 3 is that acrylic acid is not added in step S5.
[0087] Performance Test:
[0088] The thickening performance and film-forming performance of the thickeners prepared in Examples 1-3 and Comparative Examples 1-4 were tested. The thickening performance was measured by referring to the standard GB / T 21089.1-2007 "Test methods for application performance of water-based additives for architectural coatings Part 1: Dispersants, defoamers, thickeners" to determine the initial viscosity, 5°C viscosity, 18°C viscosity and viscosity after 7 days of storage. The film-forming property was measured by referring to the standard GB / T 9267-2008 "Determination of white point temperature and minimum film-forming temperature of emulsions and coatings for coatings and polymer dispersions for plastics" to determine the film-forming state of the sample under a 30°C environment. The specific test results are shown in Table 1:
[0089] Table 1
[0090]
[0091] Performance Test:
[0092] Comparative analysis of the data in Table 1 above shows that the initial viscosity of the thickener prepared in the present invention reaches 61.2KU, the viscosity of the thickener reaches 69.4KU at 5°C, the viscosity of the thickener reaches 63.6KU at 18°C, and the viscosity of the thickener reaches 62.8KU after being placed for 7 days. The thickener has good film-forming properties at 30°C, indicating that the present invention optimizes the composition structure of the polyol, modifies it, and then modifies the long alkane straight chain and ammonium carboxylate on the polyol through free radical polymerization, which not only effectively improves the initial viscosity of the thickener and the effect of temperature on the viscosity of the thickener, but also improves the placement stability and low-temperature film-forming performance of the thickener.
[0093] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0094] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0095] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a hydrophobically modified alkali-swellable associative thickener, characterized in that: The following steps are involved: S1, adding polyol and toluene into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to 55-65° C., adding 3-isocyanate propylene solution dropwise into the reactor, and after the addition is complete, heat-retaining the reaction for 50-90 minutes, and post-treating to obtain a modified polyol; S2, adding 3-(2,4-dichlorophenyl)-1-propylene, stearyl alcohol, N,N-dimethylformamide and potassium carbonate into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to 85-95° C., keeping the temperature for reaction for 22-24 hours, and post-treating to obtain modified styrene propene; S3, adding the emulsion, acrylic acid, modified styrene propylene, modified polyol and initiator into a reactor and stirring, raising the temperature of the reactor to 60-70°C, keeping the temperature for reaction for 4-6h, lowering the temperature of the reactor to room temperature, dropping ammonia water into the reactor, adjusting the pH of the system to 6-7, and post-treating to obtain a thickener, wherein the amount ratio of the emulsion, acrylic acid, modified styrene propylene, modified polyol and initiator is 85-95mL:5-7g:8-10g:12-14g:1-2g; Polyols are processed by the following steps: A1, ethylene glycol, glycerol, D-mannitol, modified siloxane, cis-2,3-butylene oxide and potassium hydroxide are added to a nitrogen-protected autoclave and stirred, the temperature of the autoclave is increased to 115-125° C., the pressure is increased to 0.1-0.2 MPa, and the reaction is carried out at this temperature until the hydroxyl value of the reaction system reaches 18-20 mgKOH / g, and the intermediate I is obtained by post-treatment; A2, adding intermediate I, butadiene dioxide and a catalyst into a nitrogen-protected autoclave with stirring, raising the temperature of the autoclave to 140-160° C., controlling the pressure of the autoclave to be lower than 0.4 MPa, maintaining the temperature until the pressure of the autoclave reaches equilibrium, keeping the temperature for reaction for 20-24 hours, and post-treating to obtain a polyol; The preparation method of modified siloxane is as follows: 1,11-dihydrododecamethylhexasiloxane, 5-hexene-1,2-diol, toluene and a catalyst are added into a nitrogen-protected reactor and stirred, the temperature of the reactor is increased to 75-85°C, the reaction is kept warm for 10-12 hours, and the modified siloxane is obtained by post-treatment.
2. The method for preparing a hydrophobically modified alkali-swellable associative thickener according to claim 1, characterized in that: In step S1, the usage ratio of the polyol, toluene and 3-isocyanate propylene solution is 1g:5mL:2g, and the 3-isocyanate propylene solution is composed of 3-isocyanate propylene and toluene in a weight ratio of 1:
2. The post-treatment operation includes: after the reaction is completed, the temperature of the reactor is increased to 75-85°C, and the solvent is evaporated under reduced pressure to obtain a modified polyol.
3. The method for preparing a hydrophobically modified alkali-swellable associative thickener according to claim 1, characterized in that: In step S2, the amount ratio of the 3-(2,4-dichlorophenyl)-1-propylene and stearyl alcohol is 1 mol:2.1 mol, the amount ratio of the 3-(2,4-dichlorophenyl)-1-propylene, N,N-dimethylformamide and potassium carbonate is 2g:7mL:1g, and the post-treatment operation includes: after the reaction is completed, the reactor is kept warm at 85-95°C, the solvent is evaporated under reduced pressure, the temperature of the reactor is lowered to room temperature, petroleum ether is added to the reactor, the reactor is raised to reflux, the temperature is kept warm and stirred for 20-30min, the temperature of the reactor is lowered to room temperature, and the filter is filtered, the filter cake is washed with petroleum ether 3 times and then dried, and the filter cake is transferred to a drying oven at a temperature of 55-65°C, and dried to constant weight to obtain modified styrene propene.
4. The method for preparing a hydrophobically modified alkali-swellable associative thickener according to claim 1, characterized in that: In step S3, the emulsion is composed of purified water, tetrahydrofuran and Span 80 in a dosage ratio of 45-55mL:30-40mL:1-2g, the initiator is ammonium persulfate, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is increased to 70-80°C, and the solvent is evaporated under reduced pressure to obtain a thickener.
5. The method for preparing a hydrophobically modified alkali-swellable associative thickener according to claim 1, characterized in that: In step A1, the amount ratio of ethylene glycol, glycerol, D-mannitol, modified siloxane, and cis-2,3-butylene oxide is 2 mol:1 mol:1 mol:1 mol:15 mol, and the weight ratio of ethylene glycol to potassium hydroxide is 3:
2. The post-treatment operation includes: after the reaction is completed, the reactor is kept at 115-125°C, low-boiling substances are evaporated under reduced pressure, the temperature of the high-pressure reactor is lowered to room temperature, anhydrous ethanol is added to the high-pressure reactor, stirred at room temperature for 20-30 minutes, filtered, and the filtrate is transferred to a water bath with a temperature of 65-75°C. In a rotary evaporator, the solvent is distilled off under reduced pressure to obtain an intermediate I; in step A2, the weight ratio of the intermediate I, butadiene dioxide and the catalyst is 10-12:4-7:0.2-0.3, the catalyst is a DMC bimetallic catalyst, and the post-treatment operation includes: after the reaction is completed, low-boiling point substances are distilled off under reduced pressure, the temperature of the high-pressure reactor is lowered to room temperature, anhydrous ethanol is added to the high-pressure reactor, stirred at room temperature for 20-30 minutes, filtered, and the filtrate is transferred to a rotary evaporator with a water bath temperature of 65-75° C., and the solvent is distilled off under reduced pressure to obtain a polyol.
6. The method for preparing a hydrophobically modified alkali-swellable associative thickener according to claim 1, characterized in that: The dosage ratio of the 1,11-dihydrododecylhexasiloxane and 5-hexene-1,2-diol is 1 mol:2 mol, the dosage ratio of the 1,11-dihydrododecylhexasiloxane, toluene and catalyst is 4 g:15 mL:0.2 g, the catalyst is platinum carbon, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the filtrate is filtered, the filtrate is transferred to a rotary evaporator at a temperature of 70-80°C, and the toluene is evaporated under reduced pressure to obtain modified siloxane.
7. A hydrophobically modified alkali-swellable associative thickener, characterized in that: The thickener is prepared by the method for preparing a hydrophobically modified alkali-swellable associative thickener as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Hydrophobic modified associative thickener and preparation method thereof
CN101787231B
Hydrophobic modified associative thickener and preparation method thereof
CN101787231A
V-type polydimethyl siloxane hydrophobic association emulsion polymerization printing thickener and preparation method and application thereof
CN110591018A
Anti-shearing alkali-swelling associated thickener and preparation method thereof
CN115160481A
Associative thickener dispersion
US20110230387A1