High-whiteness and high-transmittance PCR polymer composite material, preparation method and application thereof

By introducing fillers such as nanobarium sulfate, nanozirconium oxide, hollow silica and polarized particles into the polycarbonate material, combining nucleating agents and antioxidants, a composite material with high whiteness, high light transmittance and strong toughness is formed. , solves the light transmittance and durability problems of traditional PC materials in keycap applications, and achieves a comprehensive improvement in performance.

CN118290920BActive Publication Date: 2024-11-01ZHAOQING TEPUAI POLYMER MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410433691.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-11-01
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

The existing polycarbonate (PC) materials have defects such as low light transmittance and yellowing in laptop keycap applications, which are difficult to meet the appearance performance requirements of high-end keyboards. At the same time, PCR polymer materials have complex sources and high impurities, and their performance is It is difficult to take into account high transparency, whiteness and long-term durability.

Method used

80-90 parts by weight of bisphenol A type polycarbonate, 3-5 parts by weight of nanobarium sulfate powder, 0.8-1.5 parts by weight of nanozirconia, 0.8-1.2 parts by weight of hollow silica microspheres, 2-3 parts by weight of polarized particles, 0.3-0.6 parts by weight of ultraviolet absorber, and 0.05-0.2 parts by weight of nucleating agent and antioxidant, form uniform and dense nanometers through synergistic efficiency of multi-components. Composite network structure improves light transmittance and whiteness, and enhances mechanical properties and weather resistance.

Benefits of technology

The high whiteness (up to 98.6%), high light transmittance (up to 91.2%), toughness and heat resistance of polymer materials are achieved, extending service life, simplifying production processes, reducing costs and carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004786483670000031
    Figure BDA0004786483670000031
  • Figure BDA0004786483670000181
    Figure BDA0004786483670000181
Patent Text Reader

Abstract

A high-whiteness and high-transmittance PCR polymer composite material comprises the following components in parts by weight: 80-90 parts by weight of polycarbonate, 3-5 parts by weight of barium sulfate powder, 0.8-1.5 parts by weight of nano zirconium oxide, 0.8-1.2 parts by weight of hollow silica microspheres, 2-3 parts by weight of polarizing particles, 0.3-0.6 parts by weight of ultraviolet light absorber, 0.05-0.2 parts by weight of nucleating agent and 0.1-0.3 parts by weight of antioxidant. A variety of whitening and anti-transmittance functional fillers such as nano zirconium oxide, barium sulfate and hollow silica are introduced into a PC matrix, and new high-efficiency polarizing particles are compounded, so that the whiteness, transmittance, toughness, heat resistance and polarization efficiency of the PC composite material are greatly improved. The preparation method thereof is also disclosed, and the PC composite material is used to make notebook computer keycaps to achieve the integration of high whiteness, high transmittance, toughness and heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of PCR polymers, and in particular to a high-whiteness and high-light-transmittance PCR polymer composite material, a preparation method and an application thereof. Background Art

[0002] Polymer materials have been widely used in the electronic information industry due to their excellent mechanical properties, electrical properties and processability. Among them, polycarbonate (PC), as one of the five general engineering plastics, has been widely used in the shells, buttons, lenses and other parts of consumer electronic products such as laptops and mobile phones due to its high strength, high toughness, high transparency and high flame retardancy.

[0003] Laptop keyboards have always been one of the main application areas of PC materials. As laptops develop towards being thinner and more portable, higher requirements are placed on keycap materials, requiring not only excellent mechanical properties and processability, but also high light transmittance and high whiteness to ensure the luminous effect of the backlight source. At present, most mid-to-high-end laptop keycaps on the market are made of PC materials.

[0004] However, traditional PC materials have defects such as low light transmittance and yellowish color, which makes it difficult to meet the appearance performance requirements of high-end notebook keyboards. In order to improve the light transmittance and whiteness of PC materials, the existing technology mainly adopts methods such as filling with highly transparent inorganic powders (such as silica) or dyes. However, these methods often lead to a decrease in the mechanical properties of PC materials, and the fillers used have poor dispersibility and low coloring uniformity, making it difficult to obtain ideal modification effects.

[0005] In addition, PC materials are prone to degradation and yellowing under high temperature, ultraviolet light and other environments, resulting in a short service life. In order to improve the heat resistance and weather resistance of PC materials, the existing technology mainly adopts methods such as doping thermal stabilizers and ultraviolet absorbers. However, these additives have poor compatibility and are prone to migration and precipitation in the PC matrix. After long-term use, they will cause problems such as cracking and fading of the keycaps, seriously affecting their user experience.

[0006] In addition to PC materials, laptop keycaps also use a large amount of other polymer materials such as acrylonitrile-butadiene-styrene copolymer (ABS) and polymethyl methacrylate (PMMA). These materials are collectively referred to as engineering plastics, and because they are mainly made from fossil resources, they are also called petroleum-based polymers. With the increasing shortage of petrochemical resources and the continuous improvement of environmental awareness, post-consumer recycled polymers (PCR polymers) have become a research hotspot in the field of engineering plastics. PCR polymers refer to polymer materials that are recovered and recycled from waste plastic products, such as waste plastic bottles and discarded home appliance casings. Compared with virgin petroleum-based polymers, PCR polymers have the advantages of low resource consumption, small carbon footprint, and low price, but due to their complex sources and high impurity content, their performance is often not comparable to that of virgin materials.

[0007] As one of the five major general engineering plastics, polycarbonate (PC) has received increasing attention in the industry for its post-consumer recycling and reuse. At present, many companies in the market have launched PCR PC materials, which are used in some notebook computer keycaps and other fields. However, since PCR PC materials are derived from waste PC products, their molecular chain length and branching degree are quite different from those of virgin materials, and the relative molecular mass distribution is also wider, resulting in a decrease in their mechanical properties and appearance properties. In addition, impurities such as dyes and additives remaining in PCR PC materials will also affect their transparency and coloring properties. How to ensure the high transparency and high whiteness of PCR PC materials while improving their mechanical properties and service life is a problem that needs to be solved.

[0008] In view of the excellent resource and environmental benefits of PCR polymer materials, as well as their broad application prospects in fields such as laptop keycaps, the development of PCR PC materials with high transparency, high whiteness, high strength and high durability is of great significance for promoting the green and sustainable development of the laptop industry. Summary of the invention

[0009] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a high-whiteness and high-light-transmittance PCR polymer composite material, a preparation method and an application thereof.

[0010] The object of the present invention is to provide a high-whiteness and high-light-transmittance PCR polymer composite material, comprising the following components: 80-90 parts by weight of polycarbonate, 3-5 parts by weight of barium sulfate powder, 0.8-1.5 parts by weight of nano zirconium oxide, 0.8-1.2 parts by weight of hollow silica microspheres, 2-3 parts by weight of polarizing particles, 0.3-0.6 parts by weight of ultraviolet light absorber, 0.05-0.2 parts by weight of nucleating agent and 0.1-0.3 parts by weight of antioxidant.

[0011] Specifically, the polycarbonate is bisphenol A polycarbonate, has a molecular weight of 25000-35000, and a melt flow rate of 8-15 g / 10 min at 300° C. / 1.2 kg.

[0012] Specifically, the barium sulfate powder is a nano-scale powder with an average particle size of 80-150nm, a whiteness greater than 98.5%, and a bulk density of 0.2-0.5g / cm 3 .

[0013] Specifically, the nano zirconium oxide has a tetragonal phase structure, a purity greater than 99%, an average particle size of 30-50nm, and a specific surface area greater than 50m 2 / g.

[0014] Specifically, the average particle size of the hollow silica microspheres is 0.3-0.8 μm, the hollow ratio is greater than 90%, the shell thickness is 15-25 nm, and the bulk density is 0.12-0.18 g / cm 3 .

[0015] Specifically, the polarizing particles are made of 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraketone, with a particle size of 1-3 μm and a purity of more than 98%. The chemical structure is as follows:

[0016]

[0017] Specifically, the ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

[0018] Specifically, the nucleating agent is any one of 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol, 1,3:2,4-bis-(3,4-dimethylbenzylidene)-sorbitol and 1,3:2,4-bis-(4-propylbenzylidene)-propyl sorbitol, and the antioxidant is tri(2,4-di-tert-butyl)phenyl phosphite.

[0019] Specifically, the preparation method of the high whiteness and high light transmittance PCR polymer composite material comprises the following steps:

[0020] (1) drying polycarbonate plastic pellets in an oven at 80-100° C. for 6-10 hours, and drying barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorbers, nucleating agents, and antioxidants in a vacuum oven at 120° C. for 4 hours;

[0021] (2) Weigh each component according to the formula, place in a high-speed mixer, and mix at a speed of 1500-3000 rpm for 5-10 minutes;

[0022] (3) Add the mixture into a twin-screw extruder, wherein the melt temperature of the twin-screw extruder is 290-310°C, the extrusion rate is 8-15kg / h, the extrudate is filtered through a 180-250 mesh screen, melt-extruded at a screw speed of 150-250rpm and a barrel temperature of 280-300°C, cooled in a water bath, air-dried and granulated, to obtain a high-whiteness and high-transmittance PCR polymer composite material.

[0023] A notebook computer keycap made of a high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0024] (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and performing injection molding at an injection temperature of 280-300° C., a mold temperature of 70-90° C., and an injection pressure of 80-120 MPa, wherein the injection molding pressure holding time is 5-15 seconds, and the mold is demolded after cooling for 30-60 seconds;

[0025] (2) The injection molded part is placed under natural light for 24-48 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance.

[0026] Compared with the prior art, the high-whiteness and high-light-transmittance PCR polymer composite material and its preparation method and its preparation method can achieve the following beneficial effects:

[0027] 1. The modification research of traditional PC materials often falls into the dilemma of "high whiteness-low transmittance" or "high transmittance-high yellowing". This is mainly due to the refractive difference between the filler and the matrix and the poor interface compatibility. However, the present invention takes a unique approach and uses nano-barium sulfate (refractive index 1.64) and nano-zirconia (refractive index 2.15) fillers and hollow silica microspheres (refractive index 1.46) to form a nearly continuous refractive index gradient with the PC matrix (refractive index 1.58), which greatly reduces the light scattering loss. At the same time, the nanofiller has a high specific surface area and is easy to form stable physical entanglements between PC molecular chains. Through surface modification such as silane coupling agents, it further increases the volume and wettability, and finally achieves nano-level uniform dispersion in the PC matrix. This not only inhibits the agglomeration of the system, but also the adsorption orientation of the PC molecular chains on the surface of the nanoparticles will induce the formation of regular and orderly crystalline regions, so the transparency is significantly improved. At the same time, the high refractive index ZrO2 nanoparticles respond quickly to the scattering of incident light, which lengthens the transmission path of light inside the composite material, reduces reflection loss, and further improves the transmittance. The hollow SiO2 microspheres have a low density, have little effect on transparency, and can selectively scatter, preferably scattering ultraviolet light with a shorter wavelength, which reduces the yellowing tendency of the material. It can be seen that the present invention cleverly utilizes multiple synergistic effects such as refractive index matching between multiple components, surface interface wetting and volume expansion, and optical selective scattering, and finally achieves the perfect unity of high whiteness of PC materials, with a whiteness of up to 98.6% and high transmittance, with a transmittance of up to 91.2%, creating a simple and efficient new way to modify PC; in addition, replacing the traditional white primer with light-diffusing PC can save the primer spraying and drying processes, realize "two coatings and two bakings", greatly simplify the spraying process, reduce costs and defective rates, and reduce VOC and carbon emissions.

[0028] 2. The high strength and heat resistance of PC materials are the key to their wide application. However, while pursuing optical properties, how to ensure that its mechanical and thermal properties do not decrease but increase is a major challenge. The nano ZrO2 and hollow SiO2 used in the present invention not only have optically enhanced transmittance and whitening effects, but also can significantly enhance the PC matrix. The specific mechanism is as follows: First, the surface of nano ZrO2 and SiO2 is rich in a large number of exposed Zr-OH and Si-OH groups, which can form strong hydrogen bonds with the ester groups in the PC molecular chain, and with the help of coupling agents to graft PC segments, finally forming a stable physical / chemical cross-linked network in the PC matrix, improving the heat resistance and strength of the material. At the same time, the uniform dispersion of ZrO2 and SiO2 in the PC matrix will hinder the large-scale movement of the PC molecular chain, making the internal stress of the material more balanced, and to a certain extent inhibiting the structural damage during processing, and the toughness and impact resistance are also improved. In addition, ZrO2 nanoparticles have high hardness and SiO2 microspheres have good flexibility. The combination of the two can achieve the best balance between rigidity and toughness, making the strength and modulus of the composite material more than 20% better than pure PC. What is even more valuable is that the invention also pioneered the introduction of nucleating agents and thermal stabilizers to improve the crystal orientation of PC, inhibit high-temperature degradation, and make Tg and Td almost intact compared to pure PC. In short, the present invention is based on the design genes of PC materials, and has made improvements in nano-enhancement, interface capacity expansion, multi-component compounding and auxiliary agent optimization. While ensuring optical properties to the maximum extent, it has achieved a comprehensive transcendence of mechanical and thermal properties, and has brought the comprehensive performance of PC-based composite materials to a new level.

[0029] 3. In the field of laptop keycaps, in addition to requiring materials to have excellent optical and mechanical properties, polarization extinction ratio and weather resistance are also crucial. However, traditional PC materials are not satisfactory in both aspects. In response to this pain point, the present invention once again takes a different approach and introduces high-efficiency polarizing particles into the PC matrix to give it excellent polarization performance. Specifically, the invention uses 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraketone, which is an imide-derived rod-shaped polarizing particle. Its unique chemical structure and geometric anisotropy enable the particles to be arranged and oriented along the melt flow direction during melt blending and extrusion, and to be maintained during the cooling and shaping process, thereby forming a regular parallel polarizing layer on a macro scale, which has extremely high polarization filtering efficiency for incident natural light, and the polarization degree can reach 98.4%. At the same time, the naphthalene diimide molecule contains a large number of aromatic condensed rings and imide groups, which will form n-π* transitions under ultraviolet light excitation, and are efficient ultraviolet absorption groups. In combination with organic ultraviolet absorbers, the light aging resistance of PC composite materials is greatly improved. After 168 hours of xenon lamp exposure, the samples of the embodiment maintained more than 95% of the mechanical properties, and the whiteness change was also controlled within 0.3-1.8%, which is much better than the comparative example and ordinary PC, which means that the PC composite material of the present invention can maintain stable performance even in harsh environments such as high ultraviolet, high temperature, and humidity for a long time. This is undoubtedly a great benefit to the application of laptop keycaps. In addition, polarizing particles also have strong selective absorption of harmful blue light, which can effectively protect the eyes and will also have great potential in health protection products for laptop keycaps. It can be seen that the present invention not only solves the shortcomings of PC optical performance in one fell swoop by introducing new high-efficiency polarizing particles into the PC matrix, but also opens up a new situation for functional applications.

[0030] 4. The nucleating agent forms a large number of uniform and fine nucleation points in the PC melt, inducing the PC molecular chains to arrange regularly and orderly, forming a spherulite structure with smaller size and more number. This not only improves the crystallinity of PC, but also reduces the refractive index difference between spherulites, greatly reduces the light scattering inside the material, and minimizes the transparency loss caused by the filler. At the same time, the density and refractive index of the highly crystallized PC matrix are also closer to the filler, further reducing the interface light scattering; the nucleating agent induces PC to quickly and uniformly nucleate in the mold, forming a spherulite structure with consistent orientation and uniform size, which significantly improves the crystallinity and density of the material. The highly crystallized PC molecular chain has increased rigidity and can withstand external forces, so the mechanical properties are further improved. At the same time, the uniform fine spherulites have small anisotropy when filling the mold, and the molding shrinkage is more balanced, which greatly reduces the warping deformation of the product and significantly improves the dimensional stability. It can be seen that the combination of nucleating agent and inorganic filler not only plays the reinforcing role of the filler, but also overcomes the molding defects easily caused by the filler by inducing high crystallization of PC, and achieves a double improvement in mechanical properties and dimensional stability. This synergistic effect cannot be achieved by using fillers or nucleating agents alone.

[0031] Nucleating agents induce PC to form highly crystalline fine spherulites, with the crystal area size at the nanometer level. Additives such as ultraviolet light absorbers can be selectively dispersed or dissolved in the amorphous area of ​​PC. Since the amorphous area of ​​highly crystalline PC is very small, the additive molecules are confined in a limited space, and migration and precipitation become very difficult. Moreover, the highly regular crystalline area also has a certain barrier effect on the additive molecules, further inhibiting their migration. Therefore, the additives can exist stably in the PC matrix for a long time and continue to play a protective role.

[0032] In addition, the interface between inorganic nanofillers and the crystalline region can form a dense interface layer, which also hinders the migration of additives. The filler surface can also interact with additive molecules through physical adsorption or chemical bonding, further improving its retention rate in the PC matrix.

[0033] It can be seen that the combination of nucleating agent, inorganic filler and additives, through synergistic effect, significantly improves the compatibility and stability of the additives in the PC matrix, so that the long-term use performance of the material such as heat resistance and weather resistance is improved simultaneously, far exceeding people's expectations.

[0034] The addition of nucleating agents greatly improves the processing performance of PC composites. Nucleating agents induce PC to rapidly and uniformly nucleate in the mold, causing the melt to cool and crystallize rapidly, the viscosity to increase rapidly, and the melt elasticity to decrease. This is conducive to the rapid filling and compression of the melt in the mold, reducing the melt residence time, and reducing stress concentration and surface defects caused by melt elasticity.

[0035] At the same time, the highly crystallized PC melt has restricted molecular chain movement and more regular orientation, so the surface finish and glossiness of the product are significantly improved. In addition, crystallization reduces the residual stress of the product, reduces deformation during demolding, and improves dimensional accuracy.

[0036] It can be seen that the nucleating agent not only synergistically improves the mechanical properties and dimensional stability of PC materials with the inorganic filler, but also unexpectedly improves its processing performance, making a qualitative leap in the surface quality and precision of the products.

[0037] In summary, the present invention accurately designs a new polycarbonate composite material from the molecular level, introduces a variety of whitening and anti-transmittance functional fillers such as nano zirconium oxide, barium sulfate and hollow silica into the PC matrix for the first time, and compound new high-efficiency polarizing particles, in order to achieve a comprehensive breakthrough in the optical, mechanical, thermal and weather resistance properties of the material through the synergistic enhancement of multiple components. By systematically optimizing the filler ratio, particle size and surface modification, the present invention successfully constructs a uniform and dense nanocomposite network structure in the PC matrix, which not only greatly improves the wettability of the filler and matrix interface, but also makes the crystal orientation of the PC molecular chain more regular. On this basis, with the precise assistance of a variety of additives, the thermal degradation of PC is inhibited, the crystal nucleation is improved, and the light energy absorption conversion efficiency is improved. Finally, the present invention achieves the improvement of multiple key performances with simple compounding, so that the data such as whiteness, light transmittance, toughness, heat resistance and polarization efficiency of the PC composite material are greatly improved. In-depth analysis of the working mechanism of the present invention shows that the synergistic enhancement of multiple components is the root of the performance leap. For example, nano ZrO2, BaSO4 and hollow SiO2 form perfect complementarity in interface wetting, optical matching and mechanical enhancement; polarizing particles and UV absorbers achieve an organic combination in extinction ratio and anti-aging performance; thermal stabilizers and nucleating agents optimize the thermal performance of PC both inside and outside, and are used in notebook computer keycaps to achieve the combination of high whiteness, high transmittance, toughness and heat resistance. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] The high-whiteness and high-transmittance PCR polymer composite material comprises the following components in parts by weight: 90 parts of polycarbonate, 3 parts of barium sulfate powder, 0.8 parts of nano zirconium oxide, 0.8 parts of hollow silica microspheres, 2 parts of polarized particles, 0.3 parts of ultraviolet light absorber, 0.05 parts of nucleating agent, and 0.1 parts of antioxidant.

[0041] Wherein, the polycarbonate is bisphenol A type, with a molecular weight of 30,000 and a melt flow rate (300°C / 1.2kg) of 10g / 10min;

[0042] The barium sulfate powder has an average particle size of 100 nm, a whiteness of 98.8%, and a bulk density of 0.3 g / cm 3 ;

[0043] The nano zirconium oxide is tetragonal, with a purity of 99.5%, an average particle size of 40 nm, and a specific surface area of ​​60 m 2 / g;

[0044] The hollow silica microspheres have an average particle size of 0.5 μm, a hollow ratio of 95%, a shell thickness of 20 nm, and a bulk density of 0.15 g / cm 3 ;

[0045] The polarizing particles are prepared from 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraone, with a particle size of 2 μm and a purity of 98.5%.

[0046] The ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

[0047] The nucleating agent is 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol.

[0048] The preparation method of the high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0049] (1) The polycarbonate was dried in an oven at 90° C. for 8 hours until the moisture content was less than 0.02%; the barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorber, nucleating agent and antioxidant were placed in a vacuum oven at 120° C. and dried for 4 hours;

[0050] (2) Weigh each component according to the formula, place in a high-speed mixer, and mix at 2000 rpm for 8 min to obtain a homogeneous mixture;

[0051] (3) The mixture is added into a twin-screw extruder, the melt temperature of the twin-screw extruder is 300°C, the extrusion rate is 10kg / h, the extrudate is filtered through a 200-mesh screen, and melt-extruded at a screw speed of 200 rpm and a barrel temperature of 290°C. After water bath cooling and air-drying granulation, a high-whiteness and high-transmittance PCR polymer composite material is obtained.

[0052] A notebook computer keycap made of a high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0053] (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and performing injection molding at an injection temperature of 290° C., a mold temperature of 80° C., and an injection pressure of 100 MPa, wherein the holding time of the injection molding is 10 seconds, and the mold is demolded after cooling for 45 seconds;

[0054] (2) The injection molded part is placed under natural light for 36 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance, with a whiteness of 96% and a total light transmittance of 90%.

[0055] Example 2

[0056] The high-whiteness and high-transmittance PCR polymer composite material comprises the following components in parts by weight: 85 parts of polycarbonate, 4 parts of barium sulfate powder, 1 part of nano zirconium oxide, 1 part of hollow silica microspheres, 2.5 parts of polarized particles, 0.4 parts of ultraviolet light absorber, 0.1 parts of nucleating agent, and 0.2 parts of antioxidant.

[0057] Among them, the polycarbonate is bisphenol A type, with a molecular weight of 28000 and a melt flow rate (300℃ / 1.2kg) of 12g / 10min;

[0058] The average particle size of barium sulfate powder is 120nm, whiteness is 99%, and the bulk density is 0.5g / cm 3 ;

[0059] Nano-zirconia is tetragonal, with a purity of 99.8%, an average particle size of 45nm, and a specific surface area of ​​65m 2 / g; Hollow silica microspheres: average particle size 0.6μm, hollow ratio 92%, shell thickness 18nm, bulk density 0.13g / cm 3 The polarizing particles are made of 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraone, with a particle size of 1.5 μm and a purity of 99%.

[0060] The ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

[0061] The nucleating agent is 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol.

[0062] The preparation method of the high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0063] (1) The polycarbonate was dried in an oven at 100° C. for 10 hours until the moisture content was less than 0.02%; the barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorber, nucleating agent and antioxidant were placed in a vacuum oven at 120° C. and dried for 4 hours;

[0064] (2) Weigh each component according to the formula, place in a high-speed mixer, and mix at 1500 rpm for 10 min to obtain a homogeneous mixture;

[0065] (3) The mixture is added into a twin-screw extruder, the melt temperature of the twin-screw extruder is 290°C, the extrusion rate is 8kg / h, the extrudate is filtered through a 180-mesh screen, and melt-extruded at a screw speed of 150 rpm and a barrel temperature of 280°C. The mixture is cooled in a water bath and air-dried to obtain a PCR polymer composite material with high whiteness and high light transmittance.

[0066] A notebook computer keycap made of a high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0067] (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and performing injection molding at an injection temperature of 295° C., a mold temperature of 85° C., and an injection pressure of 105 MPa, wherein the injection molding pressure holding time is 12 seconds, and the mold is demolded after cooling for 50 seconds;

[0068] (2) The injection molded part is placed under natural light for 36 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance, with a whiteness of 97% and a total light transmittance of 89%.

[0069] Example 3

[0070] The high-whiteness and high-transmittance PCR polymer composite material comprises the following components in parts by weight: 80 parts of polycarbonate, 5 parts of barium sulfate powder, 1.3 parts of nano zirconium oxide, 1.2 parts of hollow silica microspheres, 3 parts of polarized particles, 0.5 parts of ultraviolet light absorber, 0.2 parts of nucleating agent, and 0.3 parts of antioxidant.

[0071] Among them, the polycarbonate is bisphenol A type, with a molecular weight of 25000 and a melt flow rate (300℃ / 1.2kg) of 15g / 10min;

[0072] The average particle size of barium sulfate powder is 80nm, whiteness is 99.2%, and bulk density is 0.2g / cm 3 ;

[0073] Nano-zirconia is tetragonal, with a purity of 99.9%, an average particle size of 35nm, and a specific surface area of ​​70m 2 / g;

[0074] The average particle size of hollow silica microspheres is 0.4 μm, the hollow ratio is 98%, the shell thickness is 15 nm, and the bulk density is 0.12 g / cm3;

[0075] The polarizing particles are prepared from 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraone, with a particle size of 3 μm and a purity of 99.5%.

[0076] The ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

[0077] The nucleating agent is 1,3:2,4-bis-(4-propylbenzylidene)-propyl sorbitol.

[0078] The preparation method of the high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0079] (1) The polycarbonate was dried in an oven at 100° C. for 10 hours until the moisture content was less than 0.02%; the barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorber, nucleating agent and antioxidant were placed in a vacuum oven at 120° C. and dried for 4 hours;

[0080] (2) Weigh each component according to the formula, place in a high-speed mixer, and mix at 3000 rpm for 5 min to obtain a homogeneous mixture;

[0081] (3) The mixture is added into a twin-screw extruder, the melt temperature of the twin-screw extruder is 295°C, the extrusion rate is 8kg / h, the extrudate is filtered through a 180-mesh screen, and melt-extruded at a screw speed of 180 rpm and a barrel temperature of 285°C. After water bath cooling and air-drying granulation, a high-whiteness and high-transmittance PCR polymer composite material is obtained.

[0082] A notebook computer keycap made of a high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0083] (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and injection molding the material under the conditions of an injection temperature of 285° C., a mold temperature of 75° C., and an injection pressure of 95 MPa, wherein the holding time of the injection molding is 8 seconds, and the material is cooled for 40 seconds before demolding;

[0084] (2) The injection molded part is placed under natural light for 36 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance, with a whiteness of 98% and a total light transmittance of 91%.

[0085] Example 4

[0086] The high-whiteness and high-transmittance PCR polymer composite material comprises the following components in parts by weight: 88 parts of polycarbonate, 3.5 parts of barium sulfate powder, 1.2 parts of nano zirconium oxide, 1.1 parts of hollow silica microspheres, 2.2 parts of polarized particles, 0.6 parts of ultraviolet light absorber, 0.12 parts of nucleating agent, and 0.18 parts of antioxidant.

[0087] Among them, the polycarbonate is bisphenol A type, with a molecular weight of 32000 and a melt flow rate (300℃ / 1.2kg) of 8g / 10min;

[0088] The average particle size of barium sulfate powder is 150nm, whiteness is 98.6%, and bulk density is 0.35g / cm 3 ;

[0089] Nano-zirconia is tetragonal, with a purity of 99.6%, an average particle size of 50nm, and a specific surface area of ​​55m2 / g;

[0090] The average particle size of hollow silica microspheres is 0.8 μm, the hollow ratio is 93%, the shell thickness is 25 nm, and the bulk density is 0.18 g / cm 3 The polarizing particles are made from 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraone, with a particle size of 1.8 μm and a purity of 98.8%.

[0091] The ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

[0092] The nucleating agent is 1,3:2,4-bis-(4-propylbenzylidene)-propyl sorbitol.

[0093] The preparation method of the high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0094] (1) The polycarbonate was dried in an oven at 80° C. for 10 hours until the moisture content was less than 0.03%; the barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorber, nucleating agent and antioxidant were placed in a vacuum oven at 120° C. and dried for 4 hours;

[0095] (2) Weigh each component according to the formula, place in a high-speed mixer, and mix at 1800 rpm for 6 min to obtain a homogeneous mixture;

[0096] (3) The mixture is added into a twin-screw extruder, the melt temperature of the twin-screw extruder is 305°C, the extrusion rate is 12kg / h, the extrudate is filtered through a 180-mesh screen, and melt-extruded at a screw speed of 220rpm and a barrel temperature of 295°C. The mixture is cooled in a water bath and air-dried to obtain a PCR polymer composite material with high whiteness and high light transmittance.

[0097] A notebook computer keycap made of a high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0098] (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and performing injection molding at an injection temperature of 300° C., a mold temperature of 90° C., and an injection pressure of 110 MPa, wherein the injection molding pressure holding time is 14 seconds, and the mold is demolded after cooling for 55 seconds;

[0099] (2) The injection molded part is placed under natural light for 36 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance, with a whiteness of 95.5% and a total light transmittance of 88.5%.

[0100] Example 5

[0101] The high-whiteness and high-transmittance PCR polymer composite material comprises the following components in parts by weight: 83 parts of polycarbonate, 4.5 parts of barium sulfate powder, 1.5 parts of nano zirconium oxide, 0.9 parts of hollow silica microspheres, 2.8 parts of polarized particles, 0.35 parts of ultraviolet light absorber, 0.08 parts of nucleating agent, and 0.22 parts of antioxidant.

[0102] Among them, the polycarbonate is bisphenol A type, with a molecular weight of 35000 and a melt flow rate (300℃ / 1.2kg) of 9g / 10min;

[0103] The average particle size of barium sulfate powder is 110nm, whiteness is 99.5%, and bulk density is 0.25g / cm3;

[0104] Nano-zirconia is tetragonal, with a purity of 99.95%, an average particle size of 30nm, and a specific surface area of ​​75m 2 / g; the average particle size of hollow silica microspheres is 0.3μm, the hollow ratio is 97%, the shell thickness is 16nm, and the bulk density is 0.14g / cm 3 ;

[0105] The polarizing particles are prepared from 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8(2H,7H)-tetraone, with a particle size of 2.2 μm and a purity of 99.2%.

[0106] The ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

[0107] The nucleating agent is 1,3:2,4-bis-(4-propylbenzylidene)-propyl sorbitol.

[0108] The preparation method of the high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0109] (1) The polycarbonate was dried in an oven at 85° C. for 10 hours until the moisture content was less than 0.015%; the barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorber, nucleating agent and antioxidant were placed in a vacuum oven at 120° C. and dried for 4 hours;

[0110] (2) Weigh each component according to the formula, place in a high-speed mixer, and mix at 2200 rpm for 9 minutes to obtain a homogeneous mixture;

[0111] (3) The mixture is added into a twin-screw extruder, the melt temperature of the twin-screw extruder is 290°C, the extrusion rate is 9kg / h, the extrudate is filtered through a 180-mesh screen, and melt-extruded at a screw speed of 160rpm and a barrel temperature of 280°C. The mixture is cooled in a water bath and air-dried to obtain a PCR polymer composite material with high whiteness and high light transmittance.

[0112] A notebook computer keycap made of a high-whiteness and high-light-transmittance PCR polymer composite material comprises the following steps:

[0113] (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and injection molding the material under the conditions of an injection temperature of 280° C., a mold temperature of 70° C., and an injection pressure of 90 MPa, wherein the injection molding pressure holding time is 6 seconds, and the material is cooled for 35 seconds before demolding;

[0114] (2) The injection molded part is placed under natural light for 36 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance, with a whiteness of 98.5% and a total light transmittance of 92%.

[0115] Comparative Example 1

[0116] The formula includes the following components in parts by weight: 100 parts of polycarbonate, and no other components are added. The formula simulates unmodified conventional PC materials.

[0117] Preparation method: The polycarbonate drying conditions and injection molding process parameters are the same as those in Example 1.

[0118] Performance test: whiteness 90%, total light transmittance 85%, mechanical properties meet the general level of PC.

[0119] Compared with Example 1, although Comparative Example 1 has better light transmittance, its whiteness is obviously lower, and its mechanical properties are average, which cannot meet the performance requirements of high-end keycaps. This shows that it is difficult to achieve both high whiteness and high light transmittance by simply using PC.

[0120] Comparative Example 2

[0121] The formula includes the following components in parts by weight: 95 parts of polycarbonate, 2 parts of nano zirconium oxide, 1 part of hollow silica microspheres, and 2 parts of polarized particles, and other components are not added.

[0122] Among them, nano zirconium oxide: average particle size 40nm, specific surface area 60m 2 / g; hollow silica microspheres: average particle size 0.5 μm, hollow ratio 95%, shell thickness 20 nm; polarized particles: particle size 2 μm. Raw material specifications, preparation methods and test conditions are the same as those in Example 1.

[0123] Performance test: whiteness 80%, total light transmittance 92%, mechanical properties slightly better than comparative example 1.

[0124] Compared with the examples, the whiteness of comparative example 2 is seriously insufficient due to the lack of barium sulfate, and the transparency is improved but still unsatisfactory due to the addition of more nano zirconium oxide, which shows that zirconium oxide and silicon dioxide are difficult to achieve the purpose of whitening and transparency alone.

[0125] Comparative Example 3

[0126] The formula includes the following components in parts by weight: 88 parts of polycarbonate, 8 parts of barium sulfate powder, 1 part of nano zirconium oxide, 1 part of hollow silica microspheres, and 2 parts of polarized particles, without adding ultraviolet light absorbers, nucleating agents, and antioxidants.

[0127] The average particle size of barium sulfate powder is 200nm, the whiteness is 98%, and the bulk density is 0.5g / cm 3 , the rest of the raw material specifications, preparation methods and test conditions are the same as those in Example 1.

[0128] Performance test: whiteness 94%, total light transmittance 82%, mechanical properties are worse than those of Example 1, heat deformation temperature is low, and weather resistance is poor.

[0129] The high dosage of barium sulfate and the large particle size lead to a significant decrease in transparency; due to the lack of additives, the mechanical properties, heat resistance and aging resistance of the material are also affected. This shows that the content and particle size of each component in the formula must be strictly optimized and neither can be missing.

[0130] Comparative Example 4

[0131] The formula includes the following components in parts by weight: 80 parts of polycarbonate, 3 parts of barium sulfate powder, 0.8 parts of nano zirconium oxide, 2 parts of titanium dioxide, 2 parts of polarizing particles, 0.3 parts of ultraviolet light absorber, 0.05 parts of nucleating agent, and 0.1 parts of antioxidant.

[0132] Among them, titanium dioxide is rutile, with an average particle size of 0.3 μm and a specific surface area of ​​8 m 2 The other raw material specifications, preparation methods and test conditions were the same as those in Example 1, but the injection molding temperature was adjusted to 310°C.

[0133] Performance test: whiteness 97%, total light transmittance 75%, mechanical properties slightly worse than those of the corresponding embodiments.

[0134] Although titanium dioxide is a traditional high-whiteness filler, its large particle size and high refractive index greatly reduce its transparency after adding PC. At the same time, the high processing temperature also affects the overall performance of the material. It can be seen that simply replacing inorganic fillers cannot achieve the desired effect.

[0135] Comparative Example 5

[0136] The formula includes the following components in parts by weight: 86 parts of polycarbonate, 5 parts of barium sulfate powder, 1 part of nano zirconium oxide, 2 parts of hollow silica microspheres, 0.4 parts of ultraviolet light absorber, 0.1 parts of nucleating agent, 0.2 parts of antioxidant, and no polarizing particles are added.

[0137] The raw material specifications, preparation method and test conditions are the same as those in Example 2. The injection molding process parameters are: temperature 300°C, pressure 100 MPa, holding time 8s, and cooling time 60s.

[0138] Performance test: whiteness 96%, total light transmittance 87%, mechanical properties are equivalent to those of Example 2, but glare occurs.

[0139] The formula and process of comparative example 5 are basically the same as those of example 2, except that polarizing particles are missing. Although the performance indicators such as whiteness and light transmittance are good, the finished product has glare, which greatly reduces the visual effect. This shows that polarizing particles are the key component of the present invention and are crucial to eliminating glare and improving display effects.

[0140] It can be seen from the above 5 comparative examples that if unmodified PC is used directly, it is difficult to take into account both high whiteness and high light transmittance; the use of single fillers such as nano-zirconium oxide and silicon dioxide has limited effect on improving whiteness; the use of conventional titanium dioxide particles will greatly reduce transparency; excessive use of barium sulfate or large particle size will also lead to reduced transparency; the lack of key additives such as ultraviolet absorbers will affect the mechanical properties and weather resistance of the product; if polarizing particles are not added, glare will occur in the finished product, and the user experience will be greatly reduced.

[0141] In contrast, the composite modified formula used in the embodiment of the invention is very particular about the selection and proportion of each component. The synergistic effect of barium sulfate, nano zirconium oxide and hollow silica microspheres ensures high whiteness while significantly improving light transmittance; the addition of polarizing particles effectively eliminates the glare problem of the finished product; the reasonable addition of multiple additives ensures the excellent mechanical properties, thermal properties and weather resistance of the material. It can be seen that the formula design and preparation method of the invention are the result of the mutual synergy of multiple components, strong purpose and significant effect, which can never be achieved by simple superposition or conventional substitution.

[0142] In summary, through the systematic comparative tests between the embodiments of the invention and the comparative examples, the superior performance of the high-whiteness and high-light-transmittance polycarbonate composite material of the present invention is fully demonstrated, which reflects the originality and non-obviousness of the formula design, and also highlights the importance of strict ratio optimization and preparation process control.

[0143] The applicant conducted the following tests on Examples 1-5 and Comparative Examples 1-5:

[0144] 1. Performance Test Plan

[0145] 1. Whiteness test: Use WS-3 whiteness meter, refer to ASTM E313 standard, calibrate with standard white board, measure the surface of sample, take 5 points for each sample and calculate the average value.

[0146] 2. Transmittance test: Use HD-9800 haze meter, refer to ASTM D1003 standard, measure the total transmittance Tt and diffuse transmittance Td of the sample at a wavelength of 550nm, and calculate the visual clarity value Tt / Td. Each sample is tested in parallel 3 times and the average value is taken.

[0147] 3. Mechanical properties test: CMT-6104 universal testing machine was used to test the tensile strength, elastic modulus and cantilever beam impact strength of the samples according to ASTM D638 and ASTM D790 standards. At least 5 samples were tested in each group.

[0148] 4. Thermal properties test: PerkinElmer DSC 8000 and TGA 8000 differential scanning calorimeters and thermogravimetric analyzers were used to test the glass transition temperature (Tg), crystallization temperature (Tc) and thermal decomposition temperature (Td) of the samples according to ASTM D3418 and ASTM E1131 standards, with a heating rate of 10°C / min.

[0149] 5. Polarization performance test: Use SGW-820 polarization stress meter, refer to ASTM D4093 standard, measure the transmittance difference of samples under orthogonal polarized light, and characterize the polarization efficiency.

[0150] 6. Weathering performance test: LXD-025 xenon lamp aging test box was used, referring to ASTM D4459 standard, under simulated sunlight (0.35W / m 2 @340nm) for 168h, and the changes in the appearance and mechanical properties of the samples were tested.

[0151] Table 1 shows the whiteness and light transmittance of PC composite materials prepared with different formulations

[0152] formula Whiteness(%) Total light transmittance (%) Haze value Visual clarity Example 1 96.2 89.8 0.32 44.6 Example 2 97.5 88.5 0.28 47.2 Example 3 98.1 90.6 0.25 49.8 Example 4 95.8 88.2 0.36 43.1 Example 5 98.6 91.2 0.22 52.3 Comparative Example 1 90.4 85.6 0.85 28.6 Comparative Example 2 80.3 85.2 0.92 26.2 Comparative Example 3 94.5 82.1 0.56 35.8 Comparative Example 4 97.3 75.6 0.18 57.6 Comparative Example 5 96.4 87.3 0.41 40.8

[0153] Table 1

[0154] From the analysis of the results in Table 1, it can be seen that the whiteness of the PC composite materials of the embodiments of the invention is above 95%, which is much higher than that of the unmodified PC plastic (Comparative Example 1), and the light transmittance is close to 90%, and the visual clarity is excellent. Among them, the whiteness and light transmittance of Examples 3 and 5 are the best, reaching high whiteness of 98.1% and 98.6% respectively, the total light transmittance exceeds 90%, the haze is as low as 0.25 and 0.22, and the visual clarity is as high as 49.8 and 52.3, which is close to or even exceeds the level of ordinary glass (haze 0.3, clarity about 50).

[0155] In contrast, the comparative examples 1 and 2 lacking key fillers either have insufficient whiteness (90.4% and 80.3%) or low transmittance (85.6% and 85.2%), and the haze value is large (>0.8), and the clarity is poor (<30). Due to the excessive amount of barium sulfate used in comparative example 3, although the whiteness is acceptable (94.5%), the transmittance is significantly reduced (82.1%). Comparative example 4 using conventional TiO2 filler, although the whiteness is high (97.3%) and the haze is very low (0.18), the total transmittance is only 75.6%, and the color cast is obvious. Comparative example 5 lacking polarizing particles, although the whiteness and transmittance are high, the haze is large (0.41) and the clarity is not ideal (40.8).

[0156] It can be seen that the compounding of nano-scale barium sulfate, zirconium oxide fillers and hollow SiO2 microspheres used in the embodiment improves whiteness while significantly improving light transmittance; conventional fillers are difficult to achieve both. In addition, the introduction of polarizing particles significantly reduces haze and improves clarity, which is a major innovation of the present invention.

[0157] Table 2 shows the mechanical and thermal properties of PC composites prepared with different formulations.

[0158]

[0159] Table 2

[0160] From the analysis of the results in Table 2, it can be seen that the embodiments of the invention not only have advantages in optical properties, but also have significantly better mechanical and thermal properties than the comparative examples. For example, the tensile strength of Example 3 is 85.8MPa, the elastic modulus is 3.46GPa, and the impact strength is as high as 43.5kJ / m2, which are 25%, 21% and 33% higher than pure PC (Comparative Example 1), respectively. At the same time, the Tg and Td of the composite material are basically maintained at above 145℃ and 430℃, and the thermal stability is good.

[0161] In contrast, the mechanical and thermal properties of Comparative Example 1, which lacks reinforcing fillers, are poor. Although the Td of Comparative Example 4 using conventional TiO2 is higher (442°C), the Tg is significantly reduced (138.6°C), and the improvement of mechanical properties is limited. It can be seen that the nano zirconium oxide used in the embodiment not only has an optical anti-reflection effect, but also can significantly enhance the PC matrix. In addition, the thermal stabilizer and nucleating agent used in the embodiment can also effectively maintain or even improve the thermal properties of PC.

[0162] Table 3 shows the weather resistance of PC composite materials prepared with different formulations

[0163] formula Polarization degree(%) Change in tensile strength after exposure (%) Whiteness change after exposure (%) Example 1 97.2 -2.8 -0.6 Example 2 96.5 -3.2 -1.2 Example 3 98.4 -1.6 -0.3 Example 4 95.8 -4.1 -1.8 Example 5 98.6 -1.2 -0.2 Comparative Example 1 - -12.5 -5.6 Comparative Example 2 85.4 -10.8 -4.2 Comparative Example 3 78.6 -15.2 -6.8 Comparative Example 4 82.2 -8.6 -3.5 Comparative Example 5 - -6.2 -2.4

[0164] Table 3

[0165] From the results in Table 3, it can be seen that the examples with polarizing particles all exhibit good polarization properties, with polarization degrees all above 95%, with Example 5 reaching 98.6%, proving the high efficiency of polarizing particles. After 168 hours of xenon lamp aging, the tensile strength of Examples 3 and 5 only decreased by 1.6% and 1.2%, and the whiteness retention rates were as high as 99.7% and 99.8%, showing excellent anti-aging performance.

[0166] The polarization data of Comparative Examples 1 and 5 are marked as "-", indicating that they do not have polarization performance. This is consistent with the fact that no polarizing particles are added in their formulations.

[0167] The polarization degree of Comparative Example 2 is 85.4%, which is slightly lower than 95.8% of Example 4. This is because the amount of polarizing particles used in Comparative Example 2 (2 parts) is the same as that in Example 4, but Comparative Example 2 does not contain a nucleating agent and other additives, and the amount of nano zirconium oxide used is relatively high, resulting in a decrease in the orientation of the polarizing particles, thereby reducing the polarization degree.

[0168] The polarization degree of Comparative Example 3 is 78.6%, which is significantly lower than that of the embodiment. This is mainly because no nucleating agent and auxiliary agent are added in Comparative Example 3, and the amount of barium sulfate used is relatively high (8 parts), which affects the dispersion and orientation arrangement of polarizing particles, resulting in a decrease in polarization performance.

[0169] The polarization degree of Comparative Example 4 is 82.2%, which is also lower than that of the embodiment. Although the formula of Comparative Example 4 does not contain barium sulfate, more titanium dioxide particles (2 parts) are added, and the titanium dioxide particles are relatively large (0.3 μm), which interferes with the orderly arrangement of polarizing particles, thereby reducing the polarization degree.

[0170] In contrast, the tensile strength of the comparative examples without polarizing particles decreased by more than 6%, and the whiteness decreased significantly (2.4-5.6%). Although comparative examples 2-4 contained a small amount of polarizing particles, the performance degradation after aging was still quite obvious. It can be seen that a high content of polarizing particles can not only give the composite material excellent polarizing properties, but also significantly improve its weather resistance, which is a major innovation and contribution of the present invention. Of course, the UV absorber used in the examples also plays an important role in improving weather resistance.

[0171] The PC composite material prepared in the embodiment of the invention has ultra-high whiteness (>98%), excellent light transmittance (>90%), and clarity (>50), reaching or even exceeding the optical performance of ordinary glass. This is the first time in the field of PC modification, and completely subverts the traditional perception of "high whiteness and low transmittance" or "high transmittance and yellowing" in the industry. This is mainly due to the compounding and volume expansion of multiple nanofillers and the improvement of interface wetting, as well as the efficient regulation of scattered light by polarized particles.

[0172] The present invention not only solves the shortcomings of PC in optical properties, but also significantly improves mechanical strength, thermal stability, anti-aging, etc. For example, the tensile strength of Example 3 is more than 25% higher than that of pure PC, the strength retention rate after 168h aging is as high as 98.4%, and the thermal deformation temperature reaches 146°C, which basically meets the stringent requirements of notebook computer keycaps. This is mainly due to the interface compatibilization effect of nano-zirconia, hollow SiO2 and PC matrix, as well as the synergistic stabilization effect of multiple additives.

[0173] What is more worth mentioning is that the invented material not only has an outstanding glossy appearance, but also can effectively eliminate reflective glare through polarized particles, presenting a high-definition picture quality similar to that of an LCD screen, which is of great significance to the visual experience of notebook computer keycap products. At the same time, polarized particles can also block ultraviolet / blue light and have the effect of protecting the eyes.

[0174] Finally, the raw materials used in the present invention are all commercial products, and the preparation process is also based on traditional melt blending and injection molding, so there is no technical barrier to industrial expansion. Uniform dispersion under high filling of multiple components is the key, and the optimized extrusion temperature, screw speed and other parameters in the embodiment can ensure the repeatability of batch preparation.

[0175] In summary, the present invention pioneered the introduction of nanofillers and polarizing particles into the PC matrix, and accurately optimized the ratio and process, overcoming many pain points of PC in terms of optical properties, mechanical properties and service life. While ensuring high transparency, it also has multiple properties such as ultra-high whiteness, high clarity, high strength and toughness, and excellent weather resistance. In order to change the traditional three-coat and three-bake process to two-coat and two-bake, it would be better to replace the spray white primer.

[0176] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.

Claims

1. High whiteness and high light transmittance PCR polymer composite material, characterized by , comprising the following components: 80-90 parts by weight of polycarbonate, 3-5 parts by weight of barium sulfate powder, 0.8-1.5 parts by weight of nano zirconium oxide, 0.8-1.2 parts by weight of hollow silica microspheres, 2-3 parts by weight of polarizing particles, 0.3-0.6 parts by weight of ultraviolet light absorber, 0.05-0.2 parts by weight of nucleating agent and 0.1-0.3 parts by weight of antioxidant; The barium sulfate powder is a nanometer-grade powder with an average particle size of 80-150 nm, a whiteness greater than 98.5%, and a bulk density of 0.2-0.5 g / cm 3 ; The nano zirconium oxide has a tetragonal structure, a purity greater than 99%, an average particle size of 30-50 nm, and a specific surface area greater than 50 m 2 / g; The hollow silica microspheres have an average particle size of 0.3-0.8 μm, a hollow ratio greater than 90%, a shell thickness of 15-25 nm, and a bulk density of 0.12-0.18 g / cm 3 ; The polarizing particles are composed of 2,7-bis(2,6-diisopropylphenyl)benzo[lmn][3,8]phenanthroline-1,3,6,8( 2H , 7H )-tetraketone, with a particle size of 1-3μm and a purity greater than 98%.

2. The high whiteness and high light transmittance PCR polymer composite material according to claim 1, characterized in that The polycarbonate is bisphenol A type polycarbonate with a molecular weight of 25000-35000 and a melt flow rate of 8-15 g / 10 min at 300°C / 1.2 kg.

3. The high whiteness and high light transmittance PCR polymer composite material according to claim 1, characterized in that , the ultraviolet light absorber is 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole.

4. The high whiteness and high light transmittance PCR polymer composite material according to claim 1, characterized in that , the nucleating agent is any one of 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol, 1,3:2,4-bis-(3,4-dimethylbenzylidene)-sorbitol and 1,3:2,4-bis-(4-propylbenzylidene)-propyl sorbitol, and the antioxidant is tri(2,4-di-tert-butyl)phenyl phosphite.

5. The method for preparing the high-whiteness and high-transmittance PCR polymer composite material according to any one of claims 1 to 4, characterized in that , including the following steps: (1) drying polycarbonate plastic pellets in an oven at 80-100°C for 6-10 hours, and drying barium sulfate powder, nano zirconium oxide, hollow silica microspheres, polarizing particles, ultraviolet light absorbers, nucleating agents and antioxidants in a vacuum oven at 120°C for 4 hours; (2) Weigh each component according to the formula, place it in a high-speed mixer, and mix it at a speed of 1500-3000 rpm for 5-10 minutes; (3) Add the mixture into a twin-screw extruder, wherein the melt temperature of the twin-screw extruder is 290-310°C, the extrusion rate is 8-15kg / h, the extrudate is filtered through a 180-250 mesh screen, melt-extruded at a screw speed of 150-250rpm and a barrel temperature of 280-300°C, cooled in a water bath, air-dried and granulated, to obtain a high-whiteness and high-transmittance PCR polymer composite material.

6. A laptop computer keycap made of the high-whiteness and high-light-transmittance PCR polymer composite material according to claim 1, characterized in that , including the following steps: (1) placing a granulated material of a high-whiteness and high-transmittance PCR polymer composite material in an injection molding machine, and performing injection molding at an injection temperature of 280-300° C., a mold temperature of 70-90° C., and an injection pressure of 80-120 MPa, wherein the holding time of the injection molding is 5-15 seconds, and the mold is demolded after cooling for 30-60 seconds; (2) The injection molded part is placed under natural light for 24-48 hours to stabilize the orientation of the polarized particles, thereby obtaining a notebook computer keycap with high whiteness and high light transmittance.