A kind of quick vulcanization molding cable silicone rubber and preparation method thereof
By using a combination of composite vulcanization accelerator and coarse and fine particle white carbon black in silicone rubber, the vulcanization process efficiency and mechanical properties are improved, and the problems of low vulcanization efficiency and insufficient performance in the prior art are solved, and are suitable for applications such as cables.
Patent Information
- Application Number
- CN202410598758.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-15
AI Technical Summary
In the prior art, the vulcanization process is low in efficiency and fails to effectively improve the mechanical properties of silicone rubber, resulting in insufficient performance in applications such as cables.
The white carbon black filled component is used to combine composite vulcanization accelerator and coarse and fine particles, and the component ratio is included in the 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and As an auxiliary vulcanization component, liquid ammonia significantly improves the vulcanization process and mechanical properties.
It significantly improves the hardness, tensile strength and elongation of break of silicone rubber, shortens vulcanization time, improves mechanical and electrical properties, and is especially suitable for cable insulation applications.
Smart Images

Figure BDA0004839777200000061 
Figure BDA0004839777200000071 
Figure BDA0004839777200000121
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber composition and manufacturing, and in particular to a rapid vulcanization molding cable silicone rubber and a preparation method thereof. The prepared rubber composition is particularly suitable for application in cables. Background Art
[0002] Silicone rubber materials have attracted wide attention due to their good tensile and insulation properties and reliable mechanical endurance. It is known that the rubber material has a wear resistance, compression resistance, tensile strength and other mechanical properties greatly improved by increasing its cross-linking degree through the vulcanization step.
[0003] However, how to quickly and effectively implement the vulcanization process is a widely concerned topic in this field. A large number of studies have been conducted on the efficiency and effect of vulcanization. For example, Chinese patent publication CN114773741A relates to a thermoplastic hose and its preparation process, which is composed of the following components by weight: 45-55 parts of rubber, 3.5-6.5 parts of accelerator, 0.6-0.9 parts of antioxidant, 3-9 parts of coupling agent, 0.2-0.7 parts of vulcanizing agent, 30-40 parts of white carbon black, 3.2-3.8 parts of methyl silicone oil, 52-58 parts of stearic acid, 3.2-3.8 parts of zinc oxide and 11-14 parts of plasticizer. The thermoplastic hose prepared by this process uses infrared heating to plasticize the outside and end of the hose, eliminating the hidden danger of bubbles in the product, improving the product production quality, simplifying the production process, making it more convenient to operate, with a high degree of mechanization and automation, and being able to achieve high-temperature rapid vulcanization molding of the hose. At the same time, the hose also has a high tear strength, better elasticity, high wear resistance, and low production cost. However, the process and product components in this type of technical solution are complex, and there is no more substantial improvement in the vulcanization efficiency and the mechanical properties of the finished product.
[0004] Therefore, there is still a huge demand for research and development and improvement in related fields and technologies. Summary of the invention
[0005] The present invention focuses on providing a rapid vulcanization molding silicone rubber and a preparation method thereof. The method and the rubber composition are suitable for application in the fields of cables and the like.
[0006] The first aspect of the present invention relates to a silicone rubber composition subjected to a vulcanization process, the silicone rubber composition comprising the following raw materials calculated in parts by weight: 50 to 100 parts by weight of terminal vinyl polysiloxane; 5 to 30 parts by weight of side chain vinyl polysiloxane; 30-60 parts by weight of white carbon; 3-10 parts by weight of a crosslinking agent component; 1-10 parts by weight of a vulcanization auxiliary component, wherein the vulcanization auxiliary component comprises a first vulcanization auxiliary component and a second vulcanization auxiliary component; 1-10 parts by weight of a hydrogen-containing polysiloxane having a Si-H side chain; and 1-5 parts by weight of an inhibitor component.
[0007] In a preferred technical solution, the vinyl-terminated polysiloxane comprises 40-80 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 500,000-600,000 and a vinyl content of 0.01-0.03% (mol), 10-20 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 80,000-100,000 and a vinyl content of 0.01-0.03% (mol), and 5-10 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 30,000-50,000 and a vinyl content of 0.01-0.03% (mol).
[0008] Furthermore, the side chain vinyl polysiloxane includes 1-10 parts by weight of a side chain vinyl polysiloxane with a vinyl content of 0.8-1.0% (mol) and a molecular weight of 950,000-1.1 million, 5-15 parts by weight of a side chain vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol) and a viscosity of 2000-4000 mPa·s, and 1-10 parts by weight of a side chain vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol) and a viscosity of 500-800 mPa·s.
[0009] In a further optional technical solution, the first vulcanization auxiliary component is 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and the second vulcanization auxiliary component is liquid ammonia. Preferably, the vulcanization auxiliary component also includes divinyltetramethyldisiloxane platinum complex.
[0010] In a further optional technical solution, the white carbon black comprises a specific surface area of 300-350m 2 / g of the first white carbon black 30-50 parts by weight, and a specific surface area of 100-150m 2 / g of the second white carbon black 10-20 parts by weight.
[0011] In a preferred embodiment, the crosslinking agent component includes 1 to 5 parts by weight of hexamethyldisilazane, 0.1 to 2 parts by weight of tetramethyldivinylsilazane, and optionally 0.5 to 5 parts by weight of water.
[0012] In a preferred embodiment, the inhibitor component is 1-5 parts by weight, and the inhibitor component includes 1-ethynyl-1-cyclohexanol.
[0013] In a second aspect of the present invention, a method for preparing a silicone rubber composition is provided, the method comprising the following steps in sequence:
[0014] Step 1), preparing a colloidal base component;
[0015] Step 2), preparation of two-component rubber;
[0016] Step 3), a mixing step; and
[0017] Step 4), vulcanization process to obtain the silicone rubber composition, wherein the vulcanization process uses an auxiliary vulcanization component including 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and liquid ammonia.
[0018] In an optional technical solution, the method comprises the following specific steps in sequence:
[0019] Step 1) Preparation of colloidal base components
[0020] The terminal vinyl polysiloxane with a molecular weight of 500,000 to 600,000 and a vinyl content of 0.01 to 0.03% (mol), the side chain vinyl polysiloxane with a vinyl content of 0.8 to 1.0% (mol) and a molecular weight of 950,000 to 1.1 million, and a specific surface area of 300 to 350 m2 measured by the BET method are prepared. 2 / g of the first variety of white carbon black and 100-150m 2 / g of the second variety of white carbon black, hexamethyldisilazane, tetramethyldivinylsilazane and pure water are fully mixed under the protection of an inert atmosphere, and then subjected to heating, mixing and stirring steps to obtain a colloidal base component;
[0021] Step 2) Preparation of two-component rubber
[0022] A portion of the colloidal base component obtained in step 1), a terminal vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol), a side chain vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol), a divinyltetramethyldisiloxane platinum complex, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and liquid ammonia are stirred and dispersed, and then vacuumed to obtain a first addition type liquid rubber; then, a portion of the colloidal base component is taken and the first addition type liquid rubber is obtained; The invention discloses a method for preparing a second addition type liquid rubber comprising the steps of: mixing a first addition type liquid rubber with a first addition type and a second addition type liquid rubber; ...
[0023] Step 3) Mixing step
[0024] mixing the first addition type liquid rubber and the second addition type liquid rubber obtained in step 2) to obtain a mixed liquid rubber composition; and
[0025] Step 4) Vulcanization process
[0026] The obtained mixed liquid adhesive composition is placed or injected into a mold, heated and vulcanized to obtain the rapid vulcanization molding cable silicone rubber of this embodiment.
[0027] In a further preferred technical solution, the method may further specifically include the following steps.
[0028] Step 1) Preparation of colloidal base components
[0029] In a kneader or a mixer, 40-55 parts by weight of a terminal vinyl polysiloxane with a molecular weight of 500,000-600,000 (viscosity of 50,000 to 55,000 mPa·s) and a vinyl content of 0.01-0.03% (mol), 3-6 parts by weight of a side chain vinyl polysiloxane with a vinyl content of 0.8-1.0% (mol) and a molecular weight of 950,000-1.1 million (viscosity of 250,000 to 300,000 mPa·s), and 30-50 parts by weight of a first type of white carbon black (300-350 m 2 / g, BET method) and 5-15 parts by weight of the second type of white carbon black (100-150m 2 / g, BET method), 1-8 parts by weight of hexamethyldisilazane, 0.1-1 parts by weight of tetramethyldivinylsilazane and 1-10 parts by weight of purified water, fully mixed at 50-80°C under inert atmosphere protection for 0.1 to 2 hours, then heated to 120-140°C and began to evacuate, maintaining the temperature at 140-150°C during evacuation, then cooled to 100-120°C, and continuously stirred for 30-60 minutes to obtain a colloidal base component;
[0030] Step 2) Preparation of two-component rubber
[0031] 80-120 parts by weight of the colloidal base component obtained in step 1), 1-10 parts by weight of a vinyl-terminated polysiloxane (viscosity of 10000 mPa·s to 15000 mPa·s) having a vinyl content of 0.01-0.03% (mol) Pa·s, molecular weight of 80000 to 100000), 5-15 parts by weight of side chain vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol) (viscosity of 2000-4000mPa·s), 0.5-3 parts by weight of divinyltetramethyldisiloxane platinum complex with a platinum content of 2000ppm, 0.5-3 parts by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 0.1-2 parts by weight of liquid ammonia, stirred and dispersed in a planetary mixer for 1 to 2 hours, and then vacuumed to obtain a first addition type liquid rubber; then, take 80-120 parts by weight of the above-mentioned colloidal base component, 5-10 parts by weight of terminal vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol) and a molecular weight of 30,000 to 50,000 (viscosity of 10000m Pa·s to 15000m s), 1-10 parts by weight of side chain vinyl polysiloxane (viscosity of 500-800 mPa·s) with a vinyl content of 0.01-0.03% (mol), 0.5-2 parts by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 0.1-2 parts by weight of liquid ammonia, 1-10 parts by weight of hydrogen-containing polysiloxane with a hydrogen content of 10 mmol / g and a side chain containing Si-H, and 0.1-2 parts by weight of 1-ethynyl-1-cyclohexanol, stirring and dispersing in a planetary mixer for 30-60 minutes, mixing evenly, and then vacuuming and degassing to obtain a second addition type liquid rubber;
[0032] Step 3) Mixing step
[0033] The first addition type liquid rubber and the second addition type liquid rubber obtained in step 2) are mixed in a mass ratio of (1:1) to (3:1) to obtain a mixed liquid rubber composition; and
[0034] Step 4) Vulcanization process
[0035] The obtained mixed liquid rubber composition is placed or injected into a mold, and vulcanized and molded at 100-120° C. to obtain the silicone rubber composition.
[0036] The third aspect of the present invention relates to a method for preparing vulcanized rubber, which can be used to prepare any silicone rubber composition described in the technical solution of the present invention.
[0037] According to the technical solution of the present invention, a composite vulcanization accelerator is appropriately used, which significantly and unexpectedly improves the vulcanization process and optimal vulcanization time of the composite silicone rubber, and thereby further improves mechanical indicators such as hardness, tensile strength and elongation at break. In addition, a white carbon black filling component with coarse particles and fine particles is unexpectedly used, which further improves the mechanical, electrical and vulcanization processes.
[0038] For example, in the rapid vulcanization molding process of the present invention, the T 90 It can be less than 60, or even less than 55.
[0039] It should be noted that the product and process of the present invention may include the above steps and other related steps. In an optional or preferred scheme, the scheme of the present invention may only include the above steps or components, no longer include other steps and components, or do not significantly include other main steps or main components. In addition, the steps should be performed in a sequential order in the optional scheme, and the components and steps of the present invention can be implemented independently or arbitrarily superimposed and combined with each other.
[0040] In the following, the technical solutions and advantages of the present invention will be explained and described in more detail in conjunction with specific implementation methods. It should be understood that the contents presented in the specification and specific implementation methods are only for the purpose of more clearly illustrating the technical solutions and advantages of the present invention, and do not limit the protection scope of the present invention. Those skilled in the art can obtain the changed technical solutions based on the disclosure of the specification for various reasonable transformations. As long as they do not deviate from the spirit of the present invention, the various changed technical solutions should be understood to be included in the protection scope of the present invention. DETAILED DESCRIPTION
[0041] The present invention is described in more detail hereinafter to facilitate understanding of the invention.
[0042] Before describing the specific implementation scheme, it should be noted that those skilled in the art can select appropriate raw materials according to the enlightenment and teaching of the present disclosure, and use relevant testing equipment to perform relevant tests and obtain corresponding results. For raw materials without specific manufacturers or pathways, those skilled in the art can select raw materials that meet corresponding requirements as reaction starting materials according to the disclosure and requirements of this specification. The reaction raw materials of the process part compounds are derived from the initial products synthesized in the preamble step of the present invention, which can also be understood according to the present disclosure.
[0043] Table 1 lists the main raw materials used in the present invention and the corresponding acquisition channels or raw material origins. It should be noted that the raw materials not described in the present invention are raw material varieties that can be obtained by those skilled in the art based on common technical knowledge and existing market products.
[0044] Table 1: Description of the main raw materials used in the present invention
[0045]
[0046]
[0047] In the rapid vulcanization process and subsequent testing methods, "process positive vulcanization time" and "scorch time" can be used to characterize. Among them, the process positive vulcanization time can characterize the most suitable vulcanization time in the rubber vulcanization process. In the present invention, the process positive vulcanization time is the time corresponding to the torque of [ML+(MH-ML)×90%] in the vulcanization curve, where ML is the minimum torque and MH is the maximum torque. The positive vulcanization time can usually be expressed by T 90 On the other hand, the scorch time is the time corresponding to the torque [ML+(MH-ML)×10%] in the vulcanization curve. This value usually indicates that the rubber composition has become 10% cross-linked, the plasticity has deteriorated, and it is not suitable for processing. The scorch time is T 10 In this experiment, the above parameters are measured by a rotorless vulcanization tester. Typically, the test temperature is 110°C.
[0048] Example 1
[0049] In a typical embodiment of the present invention, the rubber composition capable of rapid vulcanization molding of the present invention is prepared from the following raw materials. Although the content of each component is described in detail in this embodiment, it is clear to those skilled in the art that, according to the contents disclosed in this specification, those skilled in the art can make corresponding adjustments and changes according to the relevant components, as long as they do not deviate from the essence of the invention of this application.
[0050] Vinyl-terminated polysiloxane, 50 to 100 parts by weight; wherein,
[0051] It may include 40-80 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 500,000-600,000 (viscosity may be 50,000 to 55,000 mPa·s) and a vinyl content of 0.01-0.03% (mol); 10-20 parts by weight of a vinyl-terminated polysiloxane having a viscosity of 10,000 to 15,000 mPa·s and a molecular weight of 80,000 to 100,000; 5-10 parts by weight of a vinyl-terminated polysiloxane having a vinyl content of 0.01-0.03% (mol) (viscosity of 10,000 to 15,000 mPa·s);
[0052] Side chain vinyl polysiloxane, 5 to 30 parts by weight; wherein,
[0053] It may include 1-10 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.8-1.0% (mol) and a molecular weight of 950,000-1.1 million (viscosity may be 250,000 mPa·s to 300,000 mPa·s); 5-15 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.01-0.03% (mol) (viscosity may be 2000-4000 mPa·s); 1-10 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.01-0.03% (mol) (viscosity may be 500-800 mPa·s);
[0054] White carbon black, 30-60 parts by weight; wherein,
[0055] The first variety of white carbon black (300-350m 2 / g, BET method) 30-50 weight parts and the second variety of white carbon black (100-150m 2 / g, BET method) 10-20 parts by weight;
[0056] Crosslinking agent component, 3-10 parts by weight, wherein:
[0057] may include 1 to 5 parts by weight of hexamethyldisilazane, 0.1 to 2 parts by weight of tetramethyldivinylsilazane, and optionally, 0.5 to 5 parts by weight of water;
[0058] Vulcanization auxiliary components, 1-10 parts by weight, wherein:
[0059] 0.1 to 3 parts by weight of divinyltetramethyldisiloxane platinum complex (the platinum content is preferably 1000-2000 ppm, and not more than 3000 ppm at most), 1-8 parts by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and 0.1 to 1 part by weight of liquid ammonia;
[0060] 1-10 parts by weight of hydrogen-containing polysiloxane having Si-H in the side chain;
[0061] An inhibitor component, 1-5 parts by weight, which may include 1-ethynyl-1-cyclohexanol;
[0062] The raw material rubber composition can be prepared by the method described in the following exemplary preparation examples. Those skilled in the art can also modify the corresponding method or steps within an appropriate range according to the different raw material components.
[0063] The rubber composition of the present invention has specific mechanical and electrical isolation properties and is particularly suitable for applications such as cable insulation.
[0064] Preparation Example 1 (E1)
[0065] The preparation process of the rapid vulcanization molding rubber composition of the present invention is described below.
[0066] Step 1) Preparation of colloidal base components
[0067] In a kneader or a mixer, 50 parts by weight of a terminal vinyl polysiloxane with a molecular weight of 500,000 to 600,000 (viscosity of 50,000 to 55,000 mPa·s) and a vinyl content of 0.01 to 0.03% (mol), 5 parts by weight of a side-chain vinyl polysiloxane with a vinyl content of 0.8 to 1.0% (mol) and a molecular weight of 950,000 to 1.1 million (viscosity of 250,000 to 300,000 mPa·s), and 40 parts by weight of a first type of white carbon black (300 to 350 m 2 / g, BET method) and 10 parts by weight of the second type of white carbon black (100-150m 2 / g, BET method), 5 parts by weight of hexamethyldisilazane, 0.5 parts by weight of tetramethyldivinylsilazane and 5 parts by weight of purified water, are fully mixed for 0.5 to 1 hour under the protection of an inert atmosphere (such as nitrogen) at 70°C, and then the temperature is raised to 120-140°C and vacuuming is started. During vacuuming, the temperature is maintained at 140-150°C, and then the temperature is lowered to 100-120°C, and stirring is continued for 30 minutes to obtain a colloidal base component.
[0068] Step 2) Preparation of two-component rubber
[0069] 100 parts by weight of the colloidal base component obtained in step 1), 5 parts by weight of a vinyl-terminated polysiloxane having a vinyl content of 0.01-0.03% (mol) (viscosity of 10000 mPa·s to 15000 mPa·s) Pa·s, molecular weight of 80000 to 100000), 10 parts by weight of side chain vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol) (viscosity can be 2000-4000mPa·s), 1 part by weight of divinyltetramethyldisiloxane platinum complex with a platinum content of 2000ppm, 1 part by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 0.5 parts by weight of liquid ammonia, stirred and dispersed in a planetary mixer for 1 to 2 hours, and then vacuumed to obtain a first addition type liquid rubber; then, 100 parts by weight of the above-mentioned colloidal base component, 8 parts by weight of terminal vinyl polysiloxane with a vinyl content of 0.01-0.03% (mol) and a molecular weight of 30000 to 50000 (viscosity can be 10000m Pa·s to 15000m Pa·s) are taken. The invention discloses a method for preparing a second addition type liquid rubber comprising the following steps: preparing the first addition type liquid rubber comprising: a ...
[0070] Step 3) Mixing step
[0071] The first addition type liquid rubber and the second addition type liquid rubber obtained in step 2) are mixed in a mass ratio of 1:1 to obtain a mixed liquid rubber composition.
[0072] Step 4) Vulcanization process
[0073] The obtained mixed liquid adhesive composition is placed or injected into a mold, and vulcanized and molded at 110-120° C. to obtain the rapid vulcanization molding cable silicone rubber of this embodiment.
[0074] Optionally, according to the subsequent application steps, other composite plastic components can be placed in the mold to produce a composite component of rapid vulcanization molding cable silicone rubber and plastic.
[0075] Comparative Example (C)
[0076] The comparative examples adopt the same preparation process as that of Preparation Example 1, but some components added in each step are adjusted. In order to avoid unnecessary redundancy, only the parts that are different from the preparation examples or embodiments of each comparative example are described below, and the same parts will be omitted from repeated description.
[0077] Comparative Example 1 (C1)
[0078] In C1, the step of adding 1 part by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and 0.5 part by weight of liquid ammonia twice in step 2) of the preparation example is adjusted to add only 1 part by weight of liquid ammonia each time without using 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane.
[0079] Comparative Example 2 (C2)
[0080] In C2, the step of adding 1 part by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and 0.5 parts by weight of liquid ammonia twice in step 2) of the preparation example is adjusted so that only 1.5 parts by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane is added in each of the two additions, and no liquid ammonia is used.
[0081] Comparative Example 3 (C3)
[0082] In C3, the step of adding 1 part by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and 0.5 part by weight of liquid ammonia twice in step 2) of the preparation example is omitted; in other words, the vulcanization auxiliary component in C3 only uses divinyltetramethyldisiloxane platinum complex.
[0083] Comparative Example 4 (C4)
[0084] In C4, 40 parts by weight of the first type of white carbon black (300-350 m 2 / g, BET method) and 10 parts by weight of the second type of white carbon black (100-150m 2 / g, BET method) was adjusted to add 50 parts by weight of the first variety of white carbon black (300-350m 2 / g, BET method), without using the second variety of white carbon black.
[0085] Test Case
[0086] In this test example, the rubber compositions of various schemes obtained in the examples and comparative examples were tested for performance, and the tests performed were in compliance with the corresponding industry or national standards. The test results are shown in Table 2 below.
[0087] Table 2: Insulation resistance type silicone rubber performance test obtained in the examples and comparative examples
[0088]
[0089] According to the results of the experimental examples and comparative examples, it can be seen that the three-phase composite vulcanization accelerator of divinyltetramethyldisiloxane platinum complex, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and liquid ammonia significantly and unexpectedly improves the vulcanization process and optimal vulcanization time of the silicone rubber of the composition, and further improves the mechanical indicators such as hardness, tensile strength and elongation at break. Although there are reports that aminodicyclohexylmethane can be used in the synthesis of resin compositions, there has never been a report recording or describing the use of aminodicyclohexylmethane in the vulcanization auxiliary component of silicone rubber, and there is no existing research and development technology that combines aminodicyclohexylmethane with liquid ammonia and a platinum catalyst as a composite silicone rubber vulcanization auxiliary component to promote the vulcanization rate and mechanical properties.
[0090] In this regard, the inventor does not want the improvements and effects achieved by the invention to be subject to any theoretical explanation. In the typical molecular structure of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, two benzene rings and N molecules separated by carbon chains form a planar stable structure (as shown below), which can stably hold ammonia molecules that assist in accelerating the vulcanization rate. This allows the ammonia molecules to play a greater role in assisting the vulcanization rate without being free from the rubber phase, and also avoids premature volatilization to the environment outside the system. At the same time, the curing (or possible complexation and attachment) of ammonia molecules can also reduce the release of toxic components in the process:
[0091]
[0092] The planar molecular structure of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane is exemplarily expressed above. Combining the test results of the embodiment and the comparative example, it can be seen that compared with the use of liquid ammonia alone, the combination of the two auxiliary components allows the rubber composition to reach the optimal vulcanization state during vulcanization more quickly and pass the inappropriate vulcanization point (T 10 ). In a typical embodiment, the mass ratio of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane to liquid ammonia can be (1:1) to (3:1), that is, a small amount of liquid ammonia and dimethyl-4,4'-diaminodicyclohexylmethane can significantly increase the vulcanization rate while stabilizing and reducing harmful substance emissions. Compared with the use of dimethyl-4,4'-diaminodicyclohexylmethane or liquid ammonia alone, the vulcanization rate is significantly and unexpectedly improved.
[0093] In addition, the inventors unexpectedly discovered that the use of two-component silica in the rubber composition of the present invention can help improve the mechanical strength and vulcanization rate, which can be seen in the comparison between C4 and E1. One possible explanation is that the coarse-grained silica increases the proportion and volume of the insulating part in the rubber system during the filling process. On the other hand, the coarse and fine silica can also be better integrated with the two raw rubber components with different cross-linking ratios, and the various components are mixed more fully and evenly during the vulcanization process. Compared with the related art that usually only uses fine-grained silica, the technical solution of the present invention further improves the electrical properties such as volume resistivity and helps improve the vulcanization performance and other compressive and tensile strengths.
[0094] According to the implementation scheme and technical contents recorded in the specification of the present invention, the present invention can at least provide the following technical solutions: Although the present disclosure includes specific embodiments, it is obvious to those skilled in the art that various formal and detailed replacements or changes can be made to these embodiments without departing from the gist and scope of the invention of the present claims and their equivalent technical solutions. The embodiments described herein should be considered to be illustrative only and not for the purpose of limitation. The description of the features and aspects in each embodiment is considered to be applicable to similar features and aspects in other embodiments. Therefore, the scope of the present disclosure should not be limited by the specific description, but by the technical solutions of the claims, and all changes within the scope of the claims and their equivalents are interpreted as being included in the technical solutions of the present disclosure.
Claims
1. A silicone rubber composition subjected to a vulcanization process, characterized in that: The silicone rubber composition comprises the following raw materials calculated by weight: Vinyl-terminated polysiloxane, 50 to 100 parts by weight; Side chain vinyl polysiloxane, 5 to 30 parts by weight; White carbon black, 30-60 parts by weight; Cross-linking agent component, 3-10 parts by weight; A vulcanization auxiliary component, 1-10 parts by weight, wherein the vulcanization auxiliary component comprises a first vulcanization auxiliary component and a second vulcanization auxiliary component; 1-10 parts by weight of hydrogen-containing polysiloxane having Si-H in the side chain; as well as an inhibitor component, 1-5 parts by weight; and The vinyl-terminated polysiloxane comprises 40-80 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 500,000-600,000 and a vinyl content of 0.01-0.03 mol%, 10-20 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 80,000-100,000 and a vinyl content of 0.01-0.03 mol%, and 5-10 parts by weight of a vinyl-terminated polysiloxane having a molecular weight of 30,000-50,000 and a vinyl content of 0.01-0.03 mol%. The side chain vinyl polysiloxane comprises 1-10 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.8-1.0 mol% and a molecular weight of 950,000-1.1 million, 5-15 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.01-0.03 mol% and a viscosity of 2000-4000 mPa·s, and 1-10 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.01-0.03 mol% and a viscosity of 500-800 mPa·s; and The first vulcanization auxiliary component is 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and the second vulcanization auxiliary component is liquid ammonia.
2. The silicone rubber composition according to claim 1, characterized in that The white carbon black comprises a specific surface area of 300-350m 2 / g of the first white carbon black 30-50 parts by weight, and a specific surface area of 100-150m 2 / g of the second white carbon black 10-20 parts by weight.
3. The silicone rubber composition according to claim 1, characterized in that: The crosslinking agent component includes 1 to 5 parts by weight of hexamethyldisilazane, 0.1 to 2 parts by weight of tetramethyldivinylsilazane, and 0.5 to 5 parts by weight of water.
4. The silicone rubber composition according to claim 1, characterized in that: The inhibitor component includes 1-ethynyl-1-cyclohexanol.
5. A method for preparing a silicone rubber composition, characterized in that: The method comprises the following steps in sequence: Step 1), preparing a colloidal basic component; Step 2), preparation of two-component rubber; Step 3), a mixing step; and Step 4), a vulcanization process to obtain the silicone rubber composition, wherein the vulcanization process uses an auxiliary vulcanization component including 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and liquid ammonia; and The method comprises the following specific steps in sequence: Step 1) Preparation of colloidal base components In a kneader or a mixer, 40-55 parts by weight of a terminal vinyl polysiloxane having a molecular weight of 500,000-600,000, a viscosity of 50,000 to 55,000 mPa·s and a vinyl content of 0.01-0.03 mol%, 3-6 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.8-1.0 mol%, a molecular weight of 950,000-1.1 million, and a viscosity of 250,000 to 300,000 mPa·s, and 30-50 parts by weight of a first type of white carbon black are added, wherein the first type of white carbon black has a specific surface area of 300-350 m2 measured by a BET method. 2 / g; 5-15 parts by weight of a second type of white carbon black, wherein the second type of white carbon black has a specific surface area of 100-150m 2 / g, and 1-8 parts by weight of hexamethyldisilazane, 0.1-1 parts by weight of tetramethyldivinylsilazane and 1-10 parts by weight of pure water, fully mixed at 50-80°C under inert atmosphere protection for 0.1 to 2 hours, then heated to 120-140°C and began to evacuate, while maintaining the temperature at 140-150°C, then cooled to 100-120°C, and continuously stirred for 30-60 minutes to obtain a colloidal base component; Step 2) Preparation of two-component rubber 80-120 parts by weight of the colloidal base component obtained in step 1) and 1-10 parts by weight of a vinyl-terminated polysiloxane having a vinyl content of 0.01-0.03 mol% and a viscosity of 10000 mPa·s to 15000 mPa·s are added. Pa·s, molecular weight of 80000 to 100000; 5-15 parts by weight of side chain vinyl polysiloxane with a vinyl content of 0.01-0.03 mol% and a viscosity of 2000-4000 mPa·s; and 0.5-3 parts by weight of divinyltetramethyldisiloxane platinum complex with a platinum content of 2000ppm, 0.5-3 parts by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 0.1-2 parts by weight of liquid ammonia, stirred and dispersed in a planetary mixer for 1 to 2 hours, and then vacuumed to obtain a first addition type liquid rubber; then, take 80-120 parts by weight of the above-mentioned colloidal base component, 5-10 parts by weight of terminal vinyl polysiloxane with a vinyl content of 0.01-0.03 mol% and a molecular weight of 30,000 to 50,000, and a viscosity of 10000 mPa·s to 15000 mPa·s. Pa·s; 1-10 parts by weight of a side chain vinyl polysiloxane having a vinyl content of 0.01-0.03 mol% and a viscosity of 500-800 mPa·s; 0.5-2 parts by weight of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 0.1-2 parts by weight of liquid ammonia, 1-10 parts by weight of a hydrogen-containing polysiloxane having a hydrogen content of 10 mmol / g and a side chain containing Si-H, and 0.1-2 parts by weight of 1-ethynyl-1-cyclohexanol, stirred and dispersed in a planetary mixer for 30-60 minutes, mixed evenly, and then vacuumed and degassed to obtain a second addition type liquid rubber; Step 3) Mixing step The first addition type liquid rubber and the second addition type liquid rubber obtained in step 2) are mixed in a mass ratio of (1:1) to (3:1) to obtain a mixed liquid rubber composition; and Step 4) Vulcanization process The obtained mixed liquid rubber composition is placed or injected into a mold, and vulcanized and molded at 100-120° C. to obtain the silicone rubber composition.
Citation Information
Patent Citations
Thermoplastic rubber tube and preparation process thereof
CN114773741A
Double-component addition-type liquid silicone rubber as well as preparation method of same
CN108219671A
Rapid vulcanization addition type silicone rubber and preparation method thereof
CN113913023A
Addition type liquid silicone rubber, vulcanized rubber and preparation methods of addition type liquid silicone rubber and vulcanized rubber
CN113913024A
Silicone rubber elastomer
JP1993032898A