A high-temperature resistant optical diffusion layer thin film and its preparation method
By using SU-8 negative photoresist and polyacrylic acid resin to form a multilayer structure with a vertical phase gradient distribution in the optical diffusion layer film, combined with nano-silica particles, the problem of the diffusion film's poor high-temperature resistance was solved, achieving the effects of improved high-temperature resistance and brightness.
Patent Information
- Application Number
- CN202410438422.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-12
AI Technical Summary
Existing diffusion membranes are not resistant to high temperatures, and their performance is easily affected or even damaged in high-temperature environments.
A high-temperature resistant optical diffusion layer film was prepared by using SU-8 negative photoresist and polyacrylic acid resin to form a multilayer structure with a vertical phase gradient distribution, combined with nano-silica particles.
It improves the high-temperature resistance of the optical diffusion film, extends the standby time of the LCD screen, increases brightness and reduces glare, and lowers power consumption.
Smart Images

Figure CN118295169B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of liquid crystal display technology, specifically relating to a high-temperature resistant optical diffusion layer thin film and its preparation method. Background Technology
[0002] In the field of liquid crystal displays (LCDs), optical diffusion films are widely used in various types of LCDs, including smartphones, tablets, televisions, and monitors. The main function of diffusion films is to control and regulate light by scattering and refracting it, enabling LCDs to display clear and bright images. Furthermore, diffusion films can help reduce reflections and glare, improving the visual quality and comfort of the display. Located above the light guide plate inside the backlight of the module, optical diffusion films are mainly divided into microlens arrays and coated particle types. Microlens arrays are a common type of diffusion film, composed of many tiny lenses that scatter and refract light at an optical level, thereby controlling and regulating the light. Microlens array diffusion films typically have high optical efficiency and uniformity, effectively improving the visual quality and brightness of LCDs and reducing glare and reflections to some extent. However, the manufacturing process of microlens arrays is relatively complex, requiring high-precision processing and fabrication, resulting in high costs, which may limit their application in large-scale production.
[0003] Particle-coated diffusion films achieve optical scattering by coating a layer of material containing tiny particles onto the surface of a substrate. This type of diffusion film has the advantages of simple preparation process and low cost, making it suitable for large-scale production.
[0004] Traditional diffusion films are composed of a single polyacrylic acid resin or polybutylene adipate / terephthalate. These materials have relatively low glass transition temperatures (<400K), which means that diffusion films are usually not resistant to high temperatures. This means that the performance of the diffusion layer may be affected or even damaged in high-temperature environments. Summary of the Invention
[0005] To address the problems mentioned in the background art, the present invention provides a high-temperature resistant optical diffusion layer film and its preparation method, thereby solving the problem that existing diffusion films are not resistant to high temperatures, and the performance of the diffusion layer may be affected or even damaged in high-temperature environments.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] A high-temperature resistant optical diffusion layer thin film, comprising:
[0008] High-temperature resistant layer; SU-8 negative photoresist layer is deposited at the bottom of the high-temperature resistant layer, and the constituent molecules of the high-temperature resistant layer and the SU-8 negative photoresist molecules form a multilayer structure with a vertical phase gradient distribution;
[0009] Optical diffusion layer; the optical diffusion layer is disposed on the high temperature resistant layer.
[0010] Preferably, the upper part of the optical diffusion layer is a silica particle layer, and the lower part is made of polyacrylic resin.
[0011] Preferably, the high-temperature resistant layer is made of polyacrylic acid resin, and the polyacrylic acid resin molecules and SU-8 negative photoresist molecules form a multilayer structure with a vertical phase gradient distribution.
[0012] The method for preparing an optical diffusion layer thin film includes the following steps:
[0013] S1: Cleaning and drying the glass substrate;
[0014] S2: Modify the surface of the dried glass substrate using a trimethylchlorosilane solution;
[0015] S3: Spin-coating, printing or spraying the first mixed solution onto the surface of the modified glass substrate. The first mixed solution is a mixture of SU-8 negative photoresist and polyacrylic resin.
[0016] S4: Spin-coating, printing or spraying a second mixed solution onto the surface of the first mixed solution and then performing thermal annealing to form a mixed film, wherein the second mixed solution is a mixed solution of silica particles and polyacrylic acid resin;
[0017] S5: After exposing the hybrid film to ultraviolet light, it is then developed with a developer to obtain the processed hybrid film.
[0018] S6: The mixed film is cleaned and dried to obtain a cured high-temperature resistant optical diffusion film.
[0019] Preferably, the cleaning and drying process in S1 specifically involves cleaning the glass substrate with a solution of deionized water, isopropanol, and acetone, and then drying the cleaned glass substrate with nitrogen.
[0020] Preferably, the modification operation in S2 is as follows:
[0021] A glass substrate is placed face down above a trimethylchlorosilane solution, and the surface of the glass substrate is modified by a fumigation process.
[0022] The fumigation process takes place at a temperature of 15-30℃ for 2-3 hours.
[0023] Preferably, the diameter of the silica particles in S4 is 100-200 nm.
[0024] Preferably, the ultraviolet light used in S5 is 365nm ultraviolet light, and the optical power of the ultraviolet light is greater than 10mW / cm². 2 .
[0025] Preferably, the temperature for heat annealing in S4 is 65-95℃ and the time is 5-10 min.
[0026] Preferably, the developer in S5 is a mixture of 99.5% propylene glycol methyl ether acetate and 0.5% 2-methylpropanol acetate.
[0027] Compared with the prior art, the beneficial effects of the present invention are:
[0028] This application involves coating SU-8 negative photoresist with polyacrylic acid resin in a solvent, then coating nano-silica particles and polyacrylic acid solution onto the mixed solution, and finally exposing the film with ultraviolet light. Due to the huge molecular weight difference between polyacrylic acid resin and SU-8, the smaller SU-8 is deposited at the bottom of the solution, while the larger polyacrylic acid resin is enriched at the top of the solution, resulting in a multilayer structure with a vertical phase gradient distribution of polyacrylic acid resin and SU-8 during the exposure process.
[0029] SU-8 has a high glass transition temperature (>500K). Therefore, the lower region of the high-temperature resistant layer, which is rich in SU-8, acts as a protective layer for the upper layer, which is rich in polyacrylic resin. This protects the upper layer from the heat and ultraviolet radiation of the backlight source, thus improving the high-temperature resistance of the optical diffusion film. At the same time, since the high transparency and high refractive index of SU-8 do not change the transmittance of the backlight source, it can extend the standby time of the LCD screen, increase brightness, reduce glare, and reduce power consumption. Attached Figure Description
[0030] Figure 1 This is a schematic diagram of the optical diffusion layer thin film;
[0031] Figure 2 This is a schematic diagram of the process for preparing an optical diffusion layer thin film.
[0032] The attached figures are labeled as follows:
[0033] 1-SU-8 negative photoresist layer; 2-High temperature resistant layer; 3-Optical diffusion layer; 4-Silica particle layer. Detailed Implementation
[0034] To facilitate understanding of the technical content of this invention by those skilled in the art, the invention will be further described in detail below with reference to the accompanying drawings and specific examples. It should be understood that the specific examples described herein are merely illustrative and not intended to limit the scope of the invention.
[0035] like Figure 1As shown, a high-temperature resistant optical diffusion layer thin film includes:
[0036] High temperature resistant layer 2; SU-8 negative photoresist layer 1 is deposited at the bottom of high temperature resistant layer 2. The material of high temperature resistant layer 2 is polyacrylic resin. Polyacrylic resin molecules and SU-8 negative photoresist molecules form a multilayer structure with vertical phase gradient distribution.
[0037] Optical diffusion layer 3; the optical diffusion layer 3 is disposed on the high temperature resistant layer 2, the upper part of the optical diffusion layer 3 is a silica particle layer 4, and the lower part is made of polyacrylic resin.
[0038] The aforementioned polyacrylic resin is a thermoplastic acrylic resin with a molecular weight of 75,000-120,000; the SU-8 negative photoresist is model SU-8 2000.5 or SU-8 2010.
[0039] like Figure 2 As shown, the method for preparing the optical diffusion layer thin film includes the following steps:
[0040] S1: Clean the glass substrate with deionized water, isopropanol and acetone solution, and then dry the cleaned glass substrate with nitrogen gas.
[0041] S2: The glass substrate is placed face down above the trimethylchlorosilane solution, and the surface of the glass substrate is modified by fumigation.
[0042] The fumigation process involves a temperature of 15-30℃ and a duration of 2-3 hours.
[0043] S3: Spin-coating, printing or spraying the first mixed solution onto the surface of the modified glass substrate. The first mixed solution is a mixture of SU-8 negative photoresist and polyacrylic resin. The mass percentage of SU-8 negative photoresist and polyacrylic resin is 1:20-1:1, and the concentration after mixing is 10-40 mg / ml.
[0044] S4: Spin-coating, printing or spraying a second mixed solution onto the surface of the first mixed solution and then performing thermal annealing to form a mixed film. The second mixed solution is a mixture of silica particles and polyacrylic acid resin. The diameter of the silica particles is 100-200 nm. The thermal annealing temperature is 65-95℃ and the time is 5-10 min.
[0045] S5: After exposing the hybrid film to ultraviolet light, it is then developed using a developer to obtain the processed hybrid film. The ultraviolet light used is 365nm ultraviolet light, and the light power of the ultraviolet light is greater than 10mW / cm². 2 The developer is a mixture of 99.5% propylene glycol methyl ether acetate and 0.5% 2-methylpropanol acetate;
[0046] S6: The mixed film is cleaned and dried, and the cured mixed solution is peeled off from the glass substrate using a vacuum chuck to obtain a cured high-temperature resistant optical diffusion film.
[0047] This application involves coating SU-8 negative photoresist with polyacrylic acid resin in a solvent, then coating nano-silica particles and polyacrylic acid solution onto the mixed solution, and finally exposing the mixture to ultraviolet light to form a film. Due to the huge molecular weight difference between polyacrylic acid resin and SU-8 negative photoresist, the smaller SU-8 negative photoresist molecules are deposited at the bottom of the solution, while the larger polyacrylic acid resin molecules are enriched at the top of the solution. This results in a multilayer structure with a vertical phase gradient distribution between the polyacrylic acid resin molecules and the SU-8 negative photoresist molecules during the exposure process.
[0048] SU-8 negative photoresist has a high glass transition temperature (>500K). Therefore, the lower region of the high-temperature resistant layer 2, which is rich in SU-8 negative photoresist, acts as a protective layer for the upper polyacrylic resin-rich layer, protecting it from heat and ultraviolet damage from the backlight source. This improves the high-temperature resistance of the optical diffusion film. At the same time, since the high transparency and high refractive index of SU-8 negative photoresist do not change the transmittance of the backlight source, it can extend the standby time of the LCD screen, increase brightness, reduce glare, and reduce power consumption.
[0049] Example 1 (Control Group):
[0050] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0051] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0052] 3. Spin-coat a polyacrylic acid resin with a molecular weight of 80,000 (1000 rpm, 60 s, 100 μm) onto the surface of a surface-modified transparent glass substrate, and then spin-coat a solution of silica and polyacrylic acid resin (molecular weight 80,000) with a molecular weight of 100-200 nm onto the surface to form a thin film. The formed thin film is then subjected to thermal annealing treatment (90℃, 5 min).
[0053] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0054] Example 2 (Control Group):
[0055] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0056] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0057] 3. Spin-coat a polyacrylic acid resin with a molecular weight of 120,000 (1000 rpm, 60 s, 300 μm) onto the surface of a surface-modified transparent glass substrate, and then spin-coat a solution of silica and polyacrylic acid resin (molecular weight 120,000) with a molecular weight of 100-200 nm onto the surface to form a thin film, and then perform a heat annealing treatment on the formed film (90℃, 5 min).
[0058] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0059] Example 3:
[0060] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0061] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0062] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82000.5 and polyacrylic acid resin with a molecular weight of 80000 at a mass ratio of 1:10 (1000 rpm, 60 s, 200 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm silica and polyacrylic acid resin solution (molecular weight of 120000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0063] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0064] Example 4:
[0065] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0066] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0067] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82000.5 and polyacrylic acid resin with a molecular weight of 80000 at a mass ratio of 1:5 (1000 rpm, 60 s, 200 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm silica and polyacrylic acid resin solution (molecular weight of 80000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90℃, 5 min).
[0068] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0069] Example 5:
[0070] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0071] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0072] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82000.5 and polyacrylic acid resin with a molecular weight of 120000 at a mass ratio of 1:10 (1000 rpm, 60 s, 300 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm silica and polyacrylic acid resin solution (molecular weight of 120000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0073] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0074] Example 6:
[0075] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0076] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0077] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82000.5 and polyacrylic acid resin with a molecular weight of 120000 at a mass ratio of 1:5 (1000 rpm, 60 s, 300 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm silica and polyacrylic acid resin solution (molecular weight of 120000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0078] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0079] Example 7:
[0080] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0081] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0082] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82010 and polyacrylic acid resin with a molecular weight of 80,000 at a mass ratio of 1:10 (1000 rpm, 60 s, 200 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm silica and polyacrylic acid resin solution (molecular weight of 80,000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0083] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0084] Example 8:
[0085] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0086] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0087] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82010 and polyacrylic acid resin with a molecular weight of 80,000 at a mass ratio of 1:5 (1000 rpm, 60 s, 200 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm silica and polyacrylic acid resin solution (molecular weight of 80,000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0088] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0089] Example 9:
[0090] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0091] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0092] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82010 and polyacrylic acid resin with a molecular weight of 120,000 at a mass ratio of 1:10 (1000 rpm, 60 s, 300 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm layer of silica and polyacrylic acid resin solution (molecular weight of 120,000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0093] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0094] Example 10:
[0095] 1. Clean the transparent glass substrate with a surface roughness of less than 1 nm, and then dry it with nitrogen gas;
[0096] 2. Invert the transparent glass substrate to be treated and fumigate it with trimethylchlorosilane solution for 2 hours. Then clean it with isopropanol and deionized water and dry it with nitrogen.
[0097] 3. A high-temperature resistant layer 2 was prepared by spin-coating a mixed solution of SU-82010 and polyacrylic acid resin with a molecular weight of 120,000 at a mass ratio of 1:5 (1000 rpm, 60 s, 300 μm) onto the surface of a surface-modified transparent glass substrate. A 100-200 nm layer of silica and polyacrylic acid resin solution (molecular weight of 120,000) was then spin-coated onto the surface of the high-temperature resistant layer 2 to form a thin film. The formed thin film was then subjected to thermal annealing treatment (90 °C, 5 min).
[0098] 4. Expose the thin film to 365nm ultraviolet light (10mW / cm). 2 10 min), soak in developer for 5 min, rinse with deionized water and dry (90℃, 5 min).
[0099] The test results of the high-temperature resistant diffusion films of Examples 1 and 2 (control groups) and Examples 3-10 are shown in Table 1.
[0100] Table 1 Comparison of Test Results for Each Example
[0101] It can be seen that the high-temperature resistant optical diffusion layer 3 film prepared by a photocrosslinking curing process (i.e., Examples 3-10) exhibits significantly enhanced brightness, uniformity, and glass transition temperature compared to the untreated optical diffusion layer 3 film (i.e., Examples 1-2), indicating a significant improvement in high-temperature resistance. Furthermore, comparing Examples 1, 3-4, 7-8 and Examples 2, 5-6, 9-10, it is evident that increasing the proportion of SU-8 negative photoresist further increases the glass transition temperature but decreases mechanical properties. The optimal ratio of SU-8 negative photoresist to polyacrylic acid resin is 1:10. Comparing Examples 3, 5, 7, 9 and Examples 4, 6, 8, 10, it is indicated that the optimal molecular weight of polyacrylic acid is approximately 120,000. This is because during exposure, the higher molecular weight of polyacrylic acid allows for a more pronounced gradient distribution with the SU-8 negative photoresist molecules, resulting in more SU-8 negative photoresist deposited at the bottom, forming a thicker high-temperature resistant layer. On the other hand, higher molecular weight polyacrylic resins can better match the elastic modulus with SU-8 negative photoresist, thus improving mechanical durability.
[0102] The present invention has been described through the above embodiments. However, it should be understood that the above embodiments are for illustrative purposes only and are not intended to limit the invention to the scope of the described embodiments. Furthermore, those skilled in the art will understand that the present invention is not limited to the above embodiments, and many more variations and modifications can be made based on the teachings of the present invention, all of which fall within the scope of protection claimed by the present invention. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an optical diffusion layer thin film, the optical diffusion layer thin film comprising a high-temperature resistant layer (2), wherein an SU-8 negative photoresist layer (1) is deposited at the bottom of the high-temperature resistant layer (2), the high-temperature resistant layer (2) is made of polyacrylic acid resin, and the polyacrylic acid resin molecules and the SU-8 negative photoresist molecules form a multilayer structure with a vertical phase gradient distribution, the optical diffusion layer thin film further comprising an optical diffusion layer (3), the optical diffusion layer (3) being disposed on the high-temperature resistant layer (2), the upper part of the optical diffusion layer (3) being a silicon dioxide particle layer (4), and the lower part being made of polyacrylic acid resin, characterized in that, The preparation method includes the following steps: S1: Cleaning and drying the glass substrate; S2: Modify the surface of the dried glass substrate using a trimethylchlorosilane solution; S3: Spin-coating, printing or spraying the first mixed solution onto the surface of the modified glass substrate. The first mixed solution is a mixture of SU-8 negative photoresist and polyacrylic resin. S4: Spin-coating, printing or spraying a second mixed solution onto the surface of the first mixed solution and then performing thermal annealing to form a mixed film, wherein the second mixed solution is a mixed solution of silica particles and polyacrylic acid resin; S5: After exposing the hybrid film to ultraviolet light, it is then developed with a developer to obtain the processed hybrid film. S6: The mixed film is cleaned and dried to obtain a cured high-temperature resistant optical diffusion film.
2. The method for preparing the optical diffusion layer thin film according to claim 1, characterized in that, The cleaning and drying process in S1 is as follows: the glass substrate is cleaned with deionized water, isopropanol and acetone solution, and then the cleaned glass substrate is dried with nitrogen.
3. The method for preparing the optical diffusion layer thin film according to claim 1, characterized in that, The modification operation in S2 is as follows: A glass substrate is placed face down above a trimethylchlorosilane solution, and the surface of the glass substrate is modified by a fumigation process. The fumigation process takes place at a temperature of 15-30℃ for 2-3 hours.
4. The method for preparing the optical diffusion layer thin film according to claim 1, characterized in that, The silica particles in S4 have a diameter of 100-200 nm.
5. The method for preparing the optical diffusion layer thin film according to claim 1, characterized in that, The ultraviolet light used in S5 is 365nm ultraviolet light, and the optical power of the ultraviolet light is greater than 10mW / cm². 2 .
6. The method for preparing the optical diffusion layer thin film according to claim 1, characterized in that, The heat annealing temperature in S4 is 65-95℃, and the time is 5-10 minutes.
7. The method for preparing the optical diffusion layer thin film according to claim 1, characterized in that, The developer in S5 is a mixture of 99.5% propylene glycol methyl ether acetate and 0.5% 2-methylpropanol acetate.
Citation Information
Patent Citations
method of lime recovery from filter-press mud of sugar refineries
SU82010A1
Lambert reflector diffusion piece and application
CN108983336A
A Method for Manufacturing a Optical Film
KR101187751B1