Positive electrode lithium supplement material and preparation method thereof, positive electrode sheet and battery

By coating the surface of lithium ferrite material with MOFs material and potassium tetratitanate whiskers to form a core-shell structure, the problem of gas production and polarization during the decomposition process of lithium ferrite material is solved, and the cycle and power performance of the battery are improved. , and reduce storage gas production.

CN118299691BActive Publication Date: 2024-10-29JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410725510.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-29
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Lithium ferrite materials have serious gas production and polarization problems during the process of decomposing to produce active lithium, which leads to reduced battery cycle performance, increased internal resistance, reduced power and battery safety.

Method used

A lithium ferrite material whose coating layer includes MOFs material and potassium tetratitanate whiskers is used. The MOFs material absorbs oxygen and potassium tetratitanate whiskers to reduce polarization and form a core-shell structure to improve the structural stability of the material.

Benefits of technology

It significantly improves the cycle performance and power performance of the positive electrode lithium supplement material, effectively reduces the storage gas production, and improves the electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118299691B_ABST
    Figure CN118299691B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and specifically to a positive electrode lithium supplement material and a preparation method thereof, a positive electrode sheet and a battery. The positive electrode lithium supplement material provided comprises lithium ferrite and a coating layer, wherein the coating layer is coated on at least part of the surface of the lithium ferrite; the coating layer comprises a MOFs material and a potassium tetratitanate whisker. A preparation method of a positive electrode lithium supplement material is also provided, comprising the following steps: mixing an iron source, an organic ligand, a first solvent and a second solvent, reacting at a first temperature for a first time to obtain a first product; mixing the first product with a potassium tetratitanate whisker powder, reacting at a second temperature for a second time, washing and drying to obtain a second product; mixing the second product, a third solvent and lithium ferrite, and after ball milling, forming a coating layer comprising a MOFs material and a potassium tetratitanate whisker on the surface of the lithium ferrite to obtain a positive electrode lithium supplement material. The present invention can improve the structural stability of the positive electrode lithium supplement material, thereby facilitating the improvement of the cycle performance of the battery and reducing the gas production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a positive electrode lithium supplement material and a preparation method thereof, a positive electrode sheet and a battery. Background Art

[0002] In recent years, with the crisis of oil resources and the influence of environmental factors, countries have been competing to develop hybrid vehicles and electric vehicles, which has provided a good opportunity for the development of automotive power batteries. At present, the performance of power batteries has been improved in terms of specific capacity and cycle stability, but there are still some key issues that restrict the further development of electric vehicles.

[0003] During the first charge and discharge process of the battery, irreversible capacity loss limits the performance and application of many high-energy materials. Most of the irreversible capacity loss comes from the active lithium consumed by the formation of the solid electrolyte interface (SEI) on the surface of the negative electrode during the first charge process. The formation of the SEI film permanently consumes a large amount of active lithium from the positive electrode, thereby reducing the cycle performance and energy density of the lithium-ion battery. Supplementing lithium ions to the electrode active material can significantly increase the reversible capacity of the material and thus increase the energy density of the battery.

[0004] Currently, lithium ferrite (Li 5 FeO 4 ) has attracted people's attention due to its good compatibility with battery systems, low production cost, non-toxicity and high gram capacity (860 mAh / g). 5 FeO 4 ) has abundant raw materials, low price, environmental friendliness, excellent thermal stability and safety, and its gram capacity is more than three times that of the common positive electrode materials currently available, so it is often used as a positive electrode material lithium supplement. However, based on the stability and surface property research of lithium ferrite, it was found that the material has serious gas production and polarization in the process of decomposing and producing active lithium, which will eventually lead to problems such as battery cell cycle attenuation, increased internal resistance, and reduced power and battery safety.

[0005] Based on the above research, it is necessary to provide a modified lithium ferrite material to overcome the intrinsic defects of lithium ferrite from the material itself, and to fully consider the material properties of lithium ferrite and adopt a specific modification method to greatly improve the storage performance and cycle performance of the obtained material. Summary of the invention

[0006] In view of this, the present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a positive electrode lithium supplement material and a preparation method thereof, a positive electrode sheet and a battery, which can improve the gas production and polarization problems of the existing lithium supplement material lithium ferrite, and can improve the stability of the positive electrode lithium supplement material, thereby improving the cycle stability of the battery.

[0007] In order to solve the above technical problems, this application is implemented as follows:

[0008] According to the first aspect of the present application, an embodiment of the present application provides a positive electrode lithium supplement material, the positive electrode lithium supplement material comprises lithium ferrite and a coating layer, the coating layer is coated on at least a portion of the surface of the lithium ferrite;

[0009] The coating layer comprises MOFs material and potassium tetratitanate whiskers.

[0010] In addition, the positive electrode lithium supplement material according to the present application may also have the following additional technical features:

[0011] In some embodiments, the MOFs material includes an iron-based MOFs material.

[0012] In some embodiments, the iron-based MOFs material includes Fe 2 (dobdc).

[0013] In some embodiments, the potassium tetratitanate whiskers are doped in the MOFs material to form a conductive network in the coating layer.

[0014] In some embodiments, the coating layer has a thickness of 15 nm to 60 nm.

[0015] In some embodiments, the average particle size of the lithium ferrite is 6 μm to 9 μm.

[0016] In some embodiments, the average particle size of the positive electrode lithium supplement material is 10 μm to 15 μm.

[0017] In some embodiments, the average diameter of the potassium tetratitanate whiskers is 1 nm to 3 nm, and the length of the potassium tetratitanate whiskers is 20 nm to 100 nm.

[0018] In some embodiments, the mass proportion of the potassium tetratitanate whiskers in the positive electrode lithium supplement material is 0.5% to 15%.

[0019] In some of the embodiments, the mass proportion of the MOFs material in the positive electrode lithium supplement material is 1% to 15%.

[0020] According to the second aspect of the present application, an embodiment of the present application provides a method for preparing a positive electrode lithium supplement material, the method comprising the following steps:

[0021] Mixing an iron source, an organic ligand, a first solvent and a second solvent, and reacting at a first temperature for a first time to obtain a first product;

[0022] The first product is mixed with potassium tetratitanate whisker powder, reacted at a second temperature for a second time, and washed and dried to obtain a second product;

[0023] The second product, the third solvent and lithium ferrite are mixed, and after ball milling, a coating layer including MOFs material and potassium tetratitanate whiskers is formed on the surface of the lithium ferrite to obtain the positive electrode lithium supplement material.

[0024] In some embodiments, the step of obtaining the first product satisfies at least one of the following characteristics (1) to (6):

[0025] (1) The iron source includes at least one of ferric chloride, ferric nitrate or ferric sulfate;

[0026] (2) The organic ligand includes 2,5-dihydroxyterephthalic acid (H4DOBDC);

[0027] (3) the first solvent includes at least one of alcohols, ketones or ethers;

[0028] (4) The second solvent includes N,N-dimethylformamide;

[0029] (5) The molar ratio of the iron source to the organic ligand is 5:(1-3);

[0030] (6) The first temperature is 120°C to 160°C, and the first time is 15h to 25h.

[0031] In some embodiments, the step of obtaining the second product satisfies at least one of the following characteristics (1) to (4):

[0032] (1) In the positive electrode lithium supplement material, the mass content of the potassium tetratitanate whiskers is 0.5% to 15%;

[0033] (2) The second temperature is 90°C to 120°C, and the second time is 2h to 6h;

[0034] (3) The washing solvent includes at least one of methanol, ethanol, propanol or acetone, and the washing frequency is not less than 3 times;

[0035] (4) The drying temperature is 60°C to 80°C.

[0036] In some embodiments, the third solvent includes at least one of methanol, ethanol, propanol or acetone.

[0037] In some embodiments, the mass ratio of the second product to lithium ferrite is (1-3):8.

[0038] In some embodiments, the rotation speed of the ball mill is 500 to 2000 r / min, and the time of the ball mill is 0.5 h to 2 h.

[0039] According to the third aspect of the present application, an embodiment of the present application provides a positive electrode sheet, which includes a current collector and a positive electrode active material layer arranged on the surface of the current collector; the positive electrode active material layer includes the positive electrode lithium replenishing material as described above or the positive electrode lithium replenishing material prepared by the method described above, as well as a positive electrode active material, a conductive agent and a binder.

[0040] In some embodiments, the mass proportion of the positive electrode lithium supplement material in the positive electrode active material layer is 0.5% to 4%.

[0041] According to a fourth aspect of the present application, an embodiment of the present application provides a battery, which includes the positive electrode sheet and the negative electrode sheet.

[0042] The application of the technical solution of this application has at least the following beneficial effects:

[0043] In the embodiment of the present application, the positive electrode lithium supplement material provided is coated on the surface of lithium ferrite with a coating layer including MOFs material and potassium tetratitanate whiskers. The MOFs material can absorb oxygen released by the lithium ferrite material when releasing active lithium to a certain extent, thereby alleviating the gas production problem existing in the process of decomposition of the lithium ferrite material to produce active lithium. At the same time, the high conductivity and hydrophobicity of potassium tetratitanate whiskers are utilized to reduce the polarization of the MOFs / lithium ferrite material, alleviate the polarization problem, and improve the structural stability of the positive electrode lithium supplement material, thereby facilitating improving the cycle performance and power performance of the battery using the positive electrode lithium supplement material, and effectively reducing the storage gas production.

[0044] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 Shown is a schematic structural diagram of a positive electrode lithium supplement material provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0046] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.

[0047] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0048] Below, the embodiments of the positive electrode lithium replenishing material, the preparation method of the positive electrode lithium replenishing material, the positive electrode sheet, the battery, etc. of the present application are specifically disclosed with appropriate reference to the drawings in detail. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0049] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0050] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0051] As analyzed in the background technology of this application, by adding a certain amount of lithium ferrite (LiFePO4) to the traditional positive electrode material, 5 FeO 4) as a positive electrode lithium supplement, which is beneficial to improve the energy density and cycle performance of lithium batteries. However, based on the study of the stability and surface properties of lithium ferrite (lithium-rich lithium ferrite material), it was found that the material has certain intrinsic defects. For example, the material has gas production and polarization problems in the process of decomposing and producing active lithium, which affects its application effect and ultimately leads to problems such as reduced battery cycle performance, increased internal resistance, and reduced power performance. Therefore, it is necessary to fully consider the material properties of lithium ferrite and overcome the intrinsic defects of lithium ferrite from the material itself through modification to alleviate the above problems. In view of this, the present application provides a positive electrode lithium supplement material and a preparation method thereof, a positive electrode sheet and a battery. The present application is described in detail below.

[0052] [Positive electrode lithium supplement material]

[0053] In some embodiments, a positive electrode lithium supplement material is provided, which includes lithium ferrite and a coating layer, and the coating layer is coated on at least a portion of the surface of the lithium ferrite; wherein the coating layer includes MOFs material and potassium tetratitanate whiskers.

[0054] It should be noted that in the present application, the "coating" is not limited to direct coating, but also includes indirect coating. For example, the coating layer coats the lithium ferrite, and there may be no other structure between the coating layer and the outer surface of the lithium ferrite, or there may be one or more layers of other structures between the coating layer and the outer surface of the lithium ferrite. Preferably, there is no other structure between the coating layer and the outer surface of the lithium ferrite.

[0055] The coating layer is formed or coated on at least part of the surface of lithium ferrite, which can protect or improve the lithium ferrite, and can be used to alleviate the gas production and polarization problems of lithium ferrite materials, and improve the structural stability of positive electrode lithium supplement materials. The coating layer is formed or coated on at least part of the surface of lithium ferrite, which means that the coating layer can completely encapsulate the lithium ferrite in the coating layer, or the coating layer can only coat a part of the outer surface of the lithium ferrite; that is, the coating layer can completely coat the lithium ferrite, or it can coat part of the surface of the lithium ferrite, preferably completely coating.

[0056] The positive electrode lithium supplement material provided is a core-shell structure, wherein the core is made of lithium ferrite material, and the outer shell or shell layer, i.e., the coating layer, is mainly composed of MOFs material and potassium tetratitanate whiskers, which can play an excellent role in protecting or improving the lithium ferrite core material, especially in alleviating the gas production and polarization problems of lithium ferrite material. Specifically, the inventors of the present application have fully considered the intrinsic defects of lithium ferrite material and adopted a new MOFs material (such as Fe 2(dobdc) material) is coated to form a core-shell structure. The novel MOFs material absorbs oxygen released by the lithium ferrite material when releasing active lithium to a certain extent, which can alleviate the gas production problem existing in the process of lithium ferrite material decomposing to produce active lithium; at the same time, the MOFs / lithium ferrite material (the core of which is lithium ferrite and the shell of which includes MOFs material) is coated and modified, that is, potassium tetratitanate whiskers are added to the coating layer, and the high conductivity and hydrophobicity of potassium tetratitanate whiskers are utilized to reduce the polarization of the MOFs / lithium ferrite material, that is, due to Li 5 FeO 4 The material is sensitive to moisture. 5 FeO 4 The material will decompose prematurely when it comes into contact with water and cannot achieve the lithium replenishment effect. The addition of potassium tetratitanate whiskers with high conductivity and hydrophobicity can avoid Li 5 FeO 4 The material decomposes prematurely when it comes into contact with water, thereby alleviating the polarization problem of the material, thereby improving the structural stability of the modified positive electrode lithium replenishing material, making the modified positive electrode lithium replenishing material exhibit good electrochemical properties, which is beneficial to improving the cycle performance and power performance of the battery using the positive electrode lithium replenishing material, and effectively reducing storage gas production.

[0057] Compared with the existing ordinary lithium ferrite material, the modified lithium ferrite material provided by the present invention can improve the cycle performance. For example, in some specific embodiments, the cycle performance (0.5C / 0.5C 2.5-3.65V), the cycle retention rate of the 2000-cycle battery cell can be improved from about 89% to about 97.2%; the modified lithium ferrite material provided by the present invention can reduce the storage gas production. For example, in some specific embodiments, the storage gas production (45℃100%SOC (state of charge)), the 3-month gas production can be reduced from about 8.0wt% to about 1.6 wt%; the modified lithium ferrite material provided by the present invention can improve the power performance. For example, in some specific embodiments, the direct current internal resistance (DCR) performance (25℃50%SOC 2C 30s) can be reduced from about 1.1 mΩ to about 0.88 mΩ.

[0058] The inventors have found through in-depth research that when the modified positive electrode lithium replenishing material of the present application satisfies the above-mentioned design conditions and optionally satisfies one or more of the following conditions, the performance of the positive electrode lithium replenishing material can be further improved.

[0059] In some embodiments, the MOFs material includes an iron-based MOFs material. In the present application, the MOFs material is preferably an iron-based MOFs material, and more preferably, the MOFs material is a MOFs material having a bimetallic Fe-Fe structure, that is, an iron-based MOFs bimetallic adsorption material.

[0060] In some embodiments, the iron-based MOFs material includes Fe 2 (dobdc).

[0061] The above Fe 2 (dobdc) is MOFs-Fe material, which is a new type of porous material in metal organic framework (MOFs). It is composed of metal ions or metal clusters connected with organic ligands through coordination bonds. Among them, MOFs with unsaturated metal vacancies have good gas adsorption capacity. Fe 2 (dobdc) can absorb oxygen, Fe 2 The principle of oxygen absorption by (dobdc) is mainly divided into physical adsorption and chemical adsorption. Physical adsorption is due to its large specific surface area and porous structure, while chemical adsorption is due to the fact that the iron metal center can form a strong iron-oxygen bond with the oxygen atoms in the organic ligand. 2 When (dobdc) is exposed to an oxygen-rich environment, its unsaturated iron metal center attracts and captures oxygen molecules, thereby achieving the maximum six-coordinated form of Fe.

[0062] It should be noted that Fe 2 (dobdc) is a kind of MOFs material and is a new type of MOFs dual ligand adsorption material known in the prior art, namely MOFs-Fe 2 (dobdc), which can be obtained from commercial sources or prepared by methods known in the relevant field, and the present application does not limit its source.

[0063] The above adsorption material Fe 2 (dobdc) can be used to absorb gases such as oxygen. In this application, a new MOFs material Fe 2 The coating layer of (dobdc) is used to coat and modify lithium ferrite to form a core-shell structure. 2 The (dobdc) material absorbs the oxygen released by the lithium ferrite material when releasing active lithium to a certain extent, thereby alleviating the gas production in the process of lithium ferrite material decomposing to produce active lithium, and solving the gas production problem of traditional lithium ferrite material.

[0064] In some embodiments, potassium tetratitanate whiskers are doped into the MOFs material to form a conductive network in the coating layer.

[0065] In this application, the coating layer is mainly composed of MOFs-Fe 2 (dobdc) and potassium tetratitanate whiskers, wherein potassium tetratitanate whiskers can be doped in MOFs-Fe 2 In dobdc, a conductive network can be formed in the coating layer, and the high conductivity and hydrophobicity of potassium tetratitanate whiskers are utilized to reduce the Fe 2(dobdc) / Li 5 FeO 4 The polarization of the material improves its stability at the same time, thereby greatly improving the material's energy density, power performance and cycle performance.

[0066] In some embodiments, the coating layer has a thickness of 15 nm to 60 nm. As an example, the coating layer may have a thickness of 15 nm, 18 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, or any range between two thereof.

[0067] By controlling the coating thickness within the above range, it is helpful to make MOFs-Fe 2 The content of (dobdc) and potassium tetratitanate whiskers is within the appropriate range to form a complete lattice and grains, which can help the performance of the positive electrode lithium supplement material and improve the electrochemical performance of the battery. If the thickness of the coating layer is too thin, it will not be enough to exert the coating effect of the coating layer; if there is too much coating material and the thickness of the coating layer is too thick, it will increase the transmission distance of lithium ions and affect the power and cycle performance of the battery cell.

[0068] In some embodiments, the average particle size of lithium ferrite is 6 μm to 9 μm. As an example, the average particle size of lithium ferrite can be any one of 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, or a range between any two of them.

[0069] In some embodiments, the average particle size of the positive electrode lithium supplement material is 10 μm to 15 μm. As an example, the average particle size of the positive electrode lithium supplement material with a core-shell structure can be any one of 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 13 μm, 13.5 μm, 14 μm, and 15 μm, or a range between any two of them.

[0070] In some embodiments, the average diameter of the potassium tetratitanate whiskers is 1 nm to 3 nm; as an example, the average diameter of the potassium tetratitanate whiskers can be any point value of 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, or a range value between any two of them. Optionally, the length of the potassium tetratitanate whiskers is 20 nm to 100 nm; as an example, the length of the potassium tetratitanate whiskers can be any point value of 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, or a range value between any two of them.

[0071] Potassium tetratitanate whiskers are fibrous conductive materials, which function similarly to carbon nanotubes, but have much higher conductivity than carbon nanotubes. In the present application, by using the above-mentioned potassium tetratitanate whiskers, the conductivity of the positive electrode lithium supplement material can be improved, and the polarization of the lithium ferrite material can also be reduced.

[0072] In some embodiments, the mass proportion of potassium tetratitanate whiskers in the positive electrode lithium supplement material is 0.5% to 15%. As an example, the doping amount of potassium tetratitanate whiskers in the positive electrode lithium supplement material is 0.5wt% to 15wt%, for example, it can be any one of 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 8%, 10%, 12%, 14%, 15%, or any range between two of them.

[0073] In the present application, by controlling the doping amount of potassium tetratitanate whiskers within the above range, it is possible to help the performance of the positive electrode lithium supplement material and improve the electrochemical performance of the battery. If the amount of potassium tetratitanate whiskers added is too little, it is not enough to form a complete potassium tetratitanate whisker conductive network, thereby affecting the conductivity of the material; if the amount of potassium tetratitanate whiskers added is too much, agglomeration will form, resulting in a series of defects such as uneven coating and excessive specific surface area, thereby causing a reduction in the power performance of the battery cell.

[0074] In some embodiments, the mass proportion of MOFs materials in the positive electrode lithium supplement material is 1% to 15%. As an example, the mass proportion of MOFs materials in the positive electrode lithium supplement material can be any one of 1%, 1.5%, 2%, 2.5%, 3%, 4%, 5%, 6%, 8%, 10%, 12%, 14%, 15%, or a range between any two of them.

[0075] By controlling the addition amount of MOFs within the above range, the gas production problem of the material can be effectively improved and the electrochemical performance of the material can be enhanced.

[0076] [Preparation method of positive electrode lithium supplement material]

[0077] In some embodiments, a method for preparing a positive electrode lithium supplement material is provided, the method comprising the following steps:

[0078] Mixing an iron source, an organic ligand, a first solvent and a second solvent, and reacting at a first temperature for a first time to obtain a first product;

[0079] The first product is mixed with potassium tetratitanate whisker powder, reacted at a second temperature for a second time, and washed and dried to obtain a second product;

[0080] The second product, the third solvent and lithium ferrite are mixed, and after ball milling, a coating layer including MOFs material and potassium tetratitanate whiskers is formed on the surface of the lithium ferrite to obtain a positive electrode lithium supplement material.

[0081] The preparation method of the positive electrode lithium replenishing material provided by the present invention can first prepare MOFs material, then mix the prepared MOFs material with potassium tetratitanate whisker powder, and then mix it with lithium ferrite after the reaction, and modify the lithium ferrite by ball milling using the MOFs material and potassium tetratitanate whisker powder to form a positive electrode lithium replenishing material with a core-shell structure. The method is simple to operate, has strong feasibility, is economical and environmentally friendly, and is easy to realize industrialization.

[0082] It should be understood that all the features and advantages described above for the “positive electrode lithium replenishing material” are also applicable to the “method for preparing the positive electrode lithium replenishing material” and will not be described in detail here.

[0083] In some specific embodiments, the method for preparing the positive electrode lithium supplement material specifically includes the following steps (a) to (c):

[0084] (a) An iron source, an organic ligand, a first solvent and a second solvent are mixed and reacted at a first temperature for a first time to obtain a first product, wherein the first product is a MOFs material.

[0085] In step (a), the iron source includes, but is not limited to, any one or more combinations of ferric chloride, ferric nitrate or ferric sulfate.

[0086] The organic ligand may be 2,5-dihydroxyterephthalic acid (H4DOBDC), also known as H4 (dobdc).

[0087] In some embodiments, the molar ratio of the iron source to the organic ligand is 5:(1-3); as an example, the molar ratio of the iron source to the organic ligand is any one of 5:1, 5:2, 5:3 or a range between any two of them.

[0088] By controlling the molar ratio of the iron source to the organic ligand within the above-mentioned appropriate range, MOFs-Fe 2 (dobdc) material can make the gas production of the battery prepared by the positive electrode lithium supplement material smaller. This is because, under this ratio, Fe 2 The (dobdc) coating layer has the highest relative crystallinity, complete crystal form, and has more unsaturated Fe (II) active sites, which chemically adsorb oxygen. At the same time, under this preparation condition, that is, within the above molar ratio range, a larger specific surface area and porosity can be obtained, which also gives it a larger physical adsorption gas space, thereby improving the MOFs-Fe 2 (dobdc) The adsorption properties of the material can reduce the gas production of the battery.

[0089] In step (a), the first solvent may be a conventional solvent, such as a solvent that can be used to completely dissolve the reactants. For example, the first solvent includes, but is not limited to, any one or more combinations of alcohols, ketones or ethers. As an example, the first solvent may be an alcohol solvent such as methanol, ethanol, isopropanol, butanol, and of course, it may also be a conventional ketone, ether or other solvent.

[0090] The second solvent may be selected from N,N-dimethylformamide (DMF).

[0091] In some embodiments, in step (a), the first temperature is 120°C to 160°C, and the first time is 15h to 25h. As an example, the first temperature can be any point value of 120°C, 130°C, 140°C, 150°C, 160°C, or a range between any two of them; the first time can be any point value of 15h, 16h, 18h, 20h, 21h, 22h, 24h, 25h, or a range between any two of them.

[0092] In MOFs-Fe 2 In the preparation of (dobdc) materials, by controlling the reaction temperature and time within the above range, the battery cycle performance prepared by the prepared positive electrode lithium supplement material can be good. This performance improvement is mainly due to Fe 2 (dobdc) is sensitive to the synthesis temperature. As the temperature extends to both sides of the optimal temperature, the relative crystallinity also shows a corresponding trend. If the reaction temperature or reaction time is not within the above range provided by the present invention, the obtained modified Li 5 FeO 4 The performance of the battery prepared by the material will be reduced. For example, when the reaction time is short, the crystallinity of the composite material crystal is small, and a complete lattice and grain cannot be formed, and there are many defects, resulting in excessive consumption of electrolyte; when the reaction time is too long, the particles will grow to form larger grains, which will hinder the passage of lithium ions, thereby causing a reduction in the power performance of the lithium-ion battery.

[0093] Exemplarily, the above step (a) specifically includes: adding an iron source, an organic ligand 2,5-dihydroxyterephthalic acid (H4DOBDC) (the molar ratio of the iron source to the organic ligand is 5: (1-3)), and 5-15 mL of the first solvent to 45-80 mL of the second solvent DMF in sequence, stirring evenly to obtain a precursor solution; transferring the above precursor solution into a stainless steel hydrothermal autoclave with polytetrafluoroethylene, reacting under reaction conditions of 120-160° C. and 15-25 hours, transferring to a glove box after the reaction is completed, slowly cooling to room temperature to obtain a first product, and storing it for later use.

[0094] (b) mixing the first product obtained in step (a) with potassium tetratitanate whisker powder, reacting at a second temperature for a second time, washing and drying to obtain a second product.

[0095] In step (b), potassium tetratitanate whisker powder is added to the first product obtained in the above step (a), wherein the amount of potassium tetratitanate whisker powder added can be calculated according to the weight ratio of potassium tetratitanate whiskers to the final positive electrode lithium replenishing material, such as the amount of potassium tetratitanate whiskers accounting for 0.3% to 0.8% of the weight of the final positive electrode lithium replenishing material; or, the amount of potassium tetratitanate whiskers accounting for 0.5% to 15% of the weight of the final positive electrode lithium replenishing material; that is, the doping amount of potassium tetratitanate whiskers in the positive electrode lithium replenishing material is 0.5wt% to 15wt%.

[0096] By controlling the addition amount of potassium tetratitanate whisker powder within a reasonable range, it can help to improve the performance of the positive electrode lithium supplement material and enhance the electrochemical performance of the battery. If the addition amount of potassium tetratitanate whisker is too small, it is not enough to form a complete potassium tetratitanate whisker conductive network, thereby affecting the conductivity of the material. If the addition amount is too large, it will form agglomerates, resulting in a series of defects such as uneven coating and excessive specific surface area, thereby causing a reduction in the power performance of the battery cell.

[0097] In some embodiments, in step (b), the second temperature is 90°C to 120°C, and the second time is 2h to 6h. Preferably, the second temperature is 95°C to 105°C, and more preferably, the second temperature is 100°C. As an example, the second temperature can be any one of 90°C, 95°C, 100°C, 105°C, 110°C, and 120°C, or a range between any two of them; the second time can be any one of 2h, 3h, 4h, 5h, and 6h, or a range between any two of them.

[0098] In step (b), by controlling the reaction time and temperature within the second temperature and second time range, a coating material with excellent performance can be obtained. When the temperature or time is not within the above range, the obtained positive electrode lithium supplement material, i.e., modified Li 5 FeO 4 The performance of the battery prepared by the material will be reduced. This is because after sintering, the potassium tetratitanate whiskers need to be heated and stirred in water to make them disperse completely to the standard for use. This process is also called boiling and loosening process. When the boiling time is short, the whiskers cannot be completely loosened to form a network. When the boiling time is too long, the water molecules will destroy the whisker structure.

[0099] In some embodiments, in step (b), the washing solvent includes at least one of methanol, ethanol, propanol or acetone, and the number of washings is not less than 3 times, for example, the number of washings can be 3 to 5 times. Of course, in other embodiments, other washing solvents can also be used, and this application does not limit this.

[0100] In step (b), the drying temperature is 60° C. to 80° C. As an example, the drying temperature may be any one of 60° C., 65° C., 70° C., 75° C., and 80° C., or a range between any two of them.

[0101] Exemplarily, the above step (b) specifically includes: adding potassium tetratitanate whisker powder to the first product obtained in the above step (a), heating and stirring, reacting under reaction conditions of 90-120°C and 2-6h. After the reaction is completed, slowly cooling to room temperature, and washing with methanol or other washing solvents (such as any one of methanol, ethanol or acetone or a combination of at least two) for 3-5 times, drying at 60°C-80°C to obtain a second product, and the obtained product is stored for later use.

[0102] (c) The second product, the third solvent and lithium ferrite are mixed and ball-milled to form a coating layer including MOFs material and potassium tetratitanate whiskers on the surface of the lithium ferrite to obtain a modified Li 5 FeO 4 Material, that is, positive electrode lithium replenishing material is obtained.

[0103] In step (c), the second product obtained in step (b) is dispersed in a third solvent, lithium ferrite is added thereto, and the second product, the third solvent and the lithium ferrite are mixed; wherein the third solvent includes but is not limited to at least one of methanol, ethanol, propanol or acetone; of course, in other embodiments, the third solvent can also be other solvents that can be used to disperse the above-mentioned second product, and the present application does not limit this.

[0104] In some embodiments, the mass ratio of the second product to lithium ferrite is (1-3): 8. As an example, the mass ratio of the second product to lithium ferrite can be any one of 1:8, 2:8, 3:8 or a range between any two of them.

[0105] By controlling the mass ratio of the second product to lithium ferrite within the above reasonable range, the coating layer of the obtained positive electrode lithium supplement material can be within a suitable thickness range, which is beneficial to improving the electrochemical performance of the material. 5 FeO 4The performance of the battery prepared with the material will be reduced. This is because if there is too little coating material, the coating layer will be too thin to exert the coating effect; if there is too much coating material, the coating layer will be too thick, which will increase the transmission distance of lithium ions and affect the power and cycle performance of the battery cell.

[0106] In some embodiments, the ball milling speed is 500-2000 r / min, and the ball milling time is 0.5h-2h. As an example, the ball milling speed can be 500r / min, 600r / min, 800r / min, 1000r / min, 1500r / min, 2000r / min, etc., and the ball milling time can be 0.5h, 1h, 1.5h, 2h, etc.

[0107] [Positive electrode]

[0108] In some embodiments, the embodiments of the present application provide a positive electrode sheet, which includes a current collector and a positive electrode active material layer arranged on the surface of the current collector; the positive electrode active material layer includes the aforementioned positive electrode lithium replenishing material or the positive electrode lithium replenishing material prepared by the aforementioned method, as well as a positive electrode active material, a conductive agent and a binder.

[0109] The present application has no particular restrictions on the material of the current collector in the positive electrode sheet, as long as the purpose of the present application can be achieved, and it can be selected according to actual needs. For example, in some embodiments, the positive electrode current collector may include aluminum foil, aluminum alloy foil, etc. Of course, in other embodiments, a composite current collector (such as an aluminum-carbon composite current collector) may also be used.

[0110] The embodiments of the present application do not particularly limit the types of positive electrode active materials, conductive agents and binders in the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, in some embodiments, the positive electrode active material may include but is not limited to positive electrode materials such as lithium iron phosphate. The binder may include but is not limited to polyacrylate, polyimide, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene butadiene copolymer (styrene butadiene rubber), polyvinyl alcohol, polytetrafluoroethylene, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose or sodium hydroxymethyl cellulose. The conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, acetylene black, Ketjen black, graphene or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes.

[0111] The present application has no particular restriction on the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode active material layer. Those skilled in the art can select the ratio according to actual needs as long as the purpose of the present application can be achieved.

[0112] In some embodiments, the mass proportion of the positive electrode lithium supplement material in the positive electrode active material layer is 0.5% to 4%. As an example, the mass proportion of the positive electrode lithium supplement material in the positive electrode active material layer can be any one of 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or a range between any two of them.

[0113] The present application has no particular restrictions on the preparation method of the positive electrode sheet, and a preparation method known in the art can be selected as long as the purpose of the present application can be achieved. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: dispersing the positive electrode active material, the positive electrode lithium supplement material, the positive electrode conductive agent, and the positive electrode binder in N-methylpyrrolidone (NMP) solvent and mixing to form a uniform positive electrode slurry, coating the positive electrode slurry on the positive electrode collector, and drying, cold pressing, slitting, etc. to obtain a positive electrode sheet.

[0114] [Battery]

[0115] In some embodiments, the present application provides a battery, which includes the aforementioned positive electrode sheet and a negative electrode sheet.

[0116] The battery may be a secondary battery or a primary battery, preferably a secondary battery. For example, the battery may be a lithium ion secondary battery, a lithium primary battery, etc., but is not limited thereto. The battery structure of the present application includes but is not limited to a soft-pack lithium ion battery, a square hard-shell battery, or a cylindrical hard-shell battery, etc.

[0117] The battery includes the above-mentioned positive electrode lithium supplement material provided in the embodiment of the present application. Therefore, the battery, such as a lithium-ion secondary battery, also has the characteristics of excellent electrochemical performance.

[0118] It should be noted that, in the specific implementation manner, the present application is explained by taking a lithium-ion battery as an example of a secondary battery, but the battery of the present application is not limited to a lithium-ion battery.

[0119] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode material. As an example, the negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0120] In this embodiment, the specific materials and structures of the negative electrode current collector and the negative electrode active material layer in the negative electrode sheet are not limited, and the negative electrode sheet structure and components known in the art that can be used in secondary batteries can be selected.

[0121] In some embodiments, the battery further includes an electrolyte and a separator.

[0122] The electrolyte may be an electrolyte, and the electrolyte that can be used in the embodiments of the present application may be an electrolyte known in the prior art. The specific type and structure of the electrolyte may be an electrolyte type that can be used in a secondary battery and is well known in the art, such as an ester electrolyte or an ether electrolyte, etc., which is not limited and will not be described in detail here.

[0123] The present application has no particular restrictions on the type of isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected. As an example, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.

[0124] Example

[0125] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents, materials or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0126] Example 1

[0127] 1. Preparation of positive electrode lithium supplement materials

[0128] (a) 2.7 mmol of ferric chloride (FeCl 2 ), 1.08 mmol of organic ligand H4DOBDC (the molar ratio of iron source to organic ligand is 5:2), and 6 mL of methanol are added into 50 mL of DMF in sequence and stirred evenly to obtain a precursor solution; the precursor solution is transferred into a stainless steel hydrothermal autoclave with polytetrafluoroethylene, and the reaction is carried out at 140 ° C for 20 h. After the reaction is completed, it is transferred to a glove box and slowly cooled to room temperature to obtain the first product, which is stored for later use.

[0129] (b) Add potassium tetratitanate whisker powder (calculated as 0.5% of the final positive electrode lithium supplement material mass) to the first product obtained in the above step (a), heat and stir, and react at 100°C for 4 hours. After the reaction is completed, slowly cool to room temperature, wash with methanol three times, and dry at 60°C to obtain a second product, which is stored for later use. The length of the potassium tetratitanate whisker is 80nm.

[0130] (c) The second product obtained in step (b) is dispersed in anhydrous ethanol and Li 5 FeO 4The mass ratio of the second product to lithium ferrite (the average particle size of lithium ferrite is 7 μm) is 2:8. A planetary ball mill is used for ball milling. The speed of the ball mill is 900 or 1000 r / min. After ball milling for 1 hour, a modified lithium ferrite material is obtained, that is, a positive electrode lithium supplement material is obtained.

[0131] 2. Preparation of positive electrode

[0132] The prepared positive electrode lithium supplement material, positive electrode active material LFP (lithium iron phosphate), conductive agent acetylene black, and binder PVDF are mixed in a mass ratio of 2.5:94.5:1:2, and solvent NMP is added. The mixture is stirred under the action of a vacuum mixer until the system becomes uniform to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain a positive electrode sheet.

[0133] 3. Preparation of negative electrode sheet

[0134] The negative electrode active material graphite, the conductive agent SP, CMC, and the binder SBR are mixed in a mass ratio of 96.4:1:1.2:1.4, and the solvent deionized water is added, and stirred under the action of a vacuum mixer until the system is uniform to obtain a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain a negative electrode sheet.

[0135] 4. Electrolyte

[0136] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then a solute LiPF is added to the organic solvent. 6 Dissolve and mix evenly to obtain an electrolyte; wherein LiPF 6 The concentration is 1 mol / L.

[0137] 5. Battery Assembly

[0138] The positive electrode sheet, the separator (9μm PP separator) and the negative electrode sheet are stacked in sequence, then wound into a battery cell and loaded into an aluminum shell. After processes such as liquid injection, formation and capacity division, a lithium-ion battery is obtained.

[0139] Embodiment 2-5

[0140] Embodiment 2-5 is substantially the same as Embodiment 1, except that:

[0141] In <Preparation of positive electrode lithium supplement material>, in step (a), the molar ratio of the iron source to the organic ligand in Example 2 is 5:1;

[0142] The molar ratio of the iron source to the organic ligand in Example 3 is 5:3;

[0143] The molar ratio of the iron source to the organic ligand in Example 4 is 5:0.5;

[0144] The molar ratio of the iron source to the organic ligand in Example 5 is 5:4.

[0145] The rest are the same as in Example 1.

[0146] Embodiment 6-9

[0147] Embodiments 6-9 are substantially the same as Embodiment 1, except that:

[0148] In <Preparation of positive electrode lithium supplement material>, in step (a), the first temperature of Example 6 is 120°C;

[0149] The first temperature of Example 7 is 160°C;

[0150] The first temperature of Example 8 is 100° C.;

[0151] The first temperature of Example 9 is 180°C.

[0152] The rest are the same as in Example 1.

[0153] Examples 10-13

[0154] Examples 10-13 are substantially the same as Example 1, except that:

[0155] In <Preparation of positive electrode lithium supplement material>, in step (a), the first time of Example 10 is 15h;

[0156] The first time of Example 11 is 25h;

[0157] The first time of Example 12 is 10 hours;

[0158] The first time in Example 13 is 30 h.

[0159] The rest are the same as in Example 1.

[0160] Examples 14-17

[0161] Examples 14-17 are substantially the same as Example 1, except that:

[0162] In <Preparation of positive electrode lithium supplement material>, in step (b), the amount of potassium tetratitanate whisker powder added in Example 14 is calculated based on 5.0% of the mass of the final positive electrode lithium supplement material;

[0163] The amount of potassium tetratitanate whisker powder added in Example 15 is calculated based on 15% of the mass of the final positive electrode lithium supplement material;

[0164] The amount of potassium tetratitanate whisker powder added in Example 16 is calculated based on 0.1% of the mass of the final positive electrode lithium supplement material;

[0165] The amount of potassium tetratitanate whisker powder added in Example 17 is calculated based on 17% of the mass of the final positive electrode lithium supplement material.

[0166] The rest are the same as in Example 1.

[0167] Examples 18-21

[0168] Examples 18-21 are substantially the same as Example 1, except that:

[0169] In <Preparation of positive electrode lithium supplement material>, in step (b), the second time of Example 18 is 2h;

[0170] The second time of Example 19 is 6 hours;

[0171] The second time of Example 20 is 1 h;

[0172] The second time of Example 21 is 8h.

[0173] The rest are the same as in Example 1.

[0174] Examples 22-25

[0175] Examples 22-25 are substantially the same as Example 1, except that:

[0176] In <Preparation of positive electrode lithium supplement material>, in step (c), the mass ratio of the second product of Example 22 to lithium ferrite is 1:8;

[0177] The mass ratio of the second product of Example 23 to lithium ferrite is 3:8;

[0178] The mass ratio of the second product of Example 24 to lithium ferrite is 0.5:8;

[0179] The mass ratio of the second product of Example 25 to lithium ferrite is 5:8.

[0180] The rest are the same as in Example 1.

[0181] Examples 26-29

[0182] Examples 26-29 are substantially the same as Example 1, except that:

[0183] In <Preparation of positive electrode lithium supplement material>, in step (b), the length of the potassium tetratitanate whiskers of Example 26 is 20 nm;

[0184] The length of the potassium tetratitanate whiskers of Example 27 is 100 nm;

[0185] The length of the potassium tetratitanate whiskers of Example 28 is 15 nm;

[0186] The length of the potassium tetratitanate whiskers of Example 29 is 120 nm.

[0187] The rest are the same as in Example 1.

[0188] Examples 30-33

[0189] Examples 30-33 are substantially the same as Example 1, except that:

[0190] In <Preparation of positive electrode lithium supplement material>, in step (c), the average particle size of the lithium ferrite in Example 30 is 6 μm;

[0191] The average particle size of lithium ferrite in Example 31 is 9 μm;

[0192] The average particle size of lithium ferrite in Example 32 is 4 μm;

[0193] The average particle size of the lithium ferrite in Example 33 is 12 μm.

[0194] The rest are the same as in Example 1.

[0195] Comparative Example 1

[0196] Comparative Example 1 is substantially the same as Example 1, except that:

[0197] In <Preparation of positive electrode lithium supplement material>, step (a) is omitted, that is, the preparation of MOFs material is not performed, and the prepared positive electrode lithium supplement material only includes potassium tetratitanate whiskers and lithium ferrite.

[0198] The rest are the same as in Example 1.

[0199] Comparative Example 2

[0200] Comparative Example 2 is substantially the same as Example 1, except that:

[0201] In <Preparation of positive electrode lithium supplement material>, potassium tetratitanate whisker powder is not added in step (b), that is, the prepared positive electrode lithium supplement material only includes MOFs material and lithium ferrite.

[0202] The rest are the same as in Example 1.

[0203] Comparative Example 3

[0204] Comparative Example 3 is substantially the same as Example 1, except that:

[0205] In <Preparation of positive electrode lithium supplement material>, ball milling was not performed in step (c).

[0206] The rest are the same as in Example 1.

[0207] Performance Testing

[0208] The performance tests were conducted on the lithium-ion batteries prepared in the above-mentioned embodiments and comparative examples, wherein the electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester, and the gas adsorption was measured using an Intelligent Gravimetric Analyser (IGA001, Hyde Analytical Instruments). Specifically, the following tests were conducted:

[0209] (1) Cycle performance test: The lithium-ion battery was placed at 25°C for 30 minutes, charged at a constant current of 0.5C to 3.65V, then charged at a constant voltage of 0.05C, and then discharged at a constant current of 0.5C to 2.5V. The discharge capacity at this time was recorded as the discharge capacity of the first cycle. The battery was placed at rest for 10 minutes, and the capacity of the lithium-ion battery at the 2000th cycle was recorded.

[0210] The capacity retention rate at the 2000th cycle = the discharge capacity at the 2000th cycle / the discharge capacity at the 1st cycle.

[0211] (2) Gas production test: Intelligent Gravimetric Analyser (IGA001, Hyde Analytical Instruments) was used. The sample was activated under vacuum and heating at 433 K for 12 hours. When the sample weight no longer changed, it was considered that the sample was fully activated. Then the temperature was slowly lowered to the desired test temperature. Before the gas production test, the sample was kept under vacuum for 30 minutes. During the test, the adsorption equilibrium point corresponding to each pressure point was kept stable for 30 minutes.

[0212] (3) DC internal resistance (DCR) test: The lithium-ion battery is left at 25°C for 30 minutes, discharged at 1C constant current to 2.5V, left at 10 minutes, charged at 1C constant current and constant voltage to 3.65V, left at 10 minutes, discharged at 1C constant current to 50% SOC, left at 10 minutes, discharged at 2C constant current for 30 seconds to calculate the DCR.

[0213] The test results are shown in Table 1.

[0214] Table 1

[0215]

[0216] It can be seen from the data in Table 1 that by comparing Examples 1 to 33 with Comparative Examples 1 to 3, the positive electrode lithium supplement material obtained by the preparation method described in the embodiment of the present invention, i.e., the modified Li 5 FeO 4 The battery prepared by the material not only has low DC resistance, but also has long cycle life and can reduce the gas production of the battery. This shows that the positive electrode lithium supplement material provided by the present invention can improve the cycle performance and power performance of the battery and reduce the storage gas production.

[0217] Specifically, by comparing Examples 1 to 5, it can be seen that compared with Examples 4 to 5, Examples 1 to 3 have a more suitable raw material ratio, that is, a suitable iron source and organic ligand ratio, and the positive electrode lithium supplement material, that is, the modified Li 5 FeO 4 The gas production of the battery prepared by the material is small. This is because under this ratio, Fe 2 The (dobdc) coating layer has the highest relative crystallinity, complete crystal form, and more unsaturated Fe (II) active sites, which can chemically adsorb oxygen. At the same time, under the preparation conditions, the material can have a larger specific surface area and porosity and a larger physical adsorption gas space.

[0218] By comparing Examples 1, 6 to 9, it can be seen that compared with Examples 8 to 9, Examples 1, 6 to 7 have a more suitable Fe 2 (dobdc) reaction temperature, the battery cycle performance prepared by the positive electrode lithium supplement material is good. This performance improvement is mainly due to Fe 2 (dobdc) is sensitive to the synthesis temperature, and as the temperature extends to both sides of the optimal temperature, the relative crystallinity also shows a corresponding trend.

[0219] By comparing Examples 1 and 10 to 13, it can be seen that compared with Examples 12 to 13, Examples 1 and 10 to 11 have a more suitable Fe 2 When the reaction time is not within the preferred parameter range provided by the present invention, the battery performance of the obtained positive electrode lithium supplement material will be reduced. This is because when the reaction time is short, the crystallinity of the composite material crystal is small, and a complete lattice and grains cannot be formed, and there are many defects, resulting in excessive consumption of electrolyte; when the reaction time is too long, the particles will grow to form larger grains, hindering the passage of lithium ions, thereby causing a reduction in the power performance of the lithium ion battery.

[0220] By comparing Examples 1 and 14 to 17, it can be seen that, compared with Examples 16 to 17, Examples 1 and 14 to 15 add a more reasonable amount of potassium tetratitanate whiskers, which can help to improve the performance of the positive electrode lithium supplement material and enhance the electrochemical performance of the battery. When the amount of potassium tetratitanate whiskers added is too little, it is not enough to form a complete potassium tetratitanate whisker conductive network, thereby affecting the conductivity of the material. When the amount of potassium tetratitanate whiskers added is too much, agglomeration will be formed, resulting in a series of defects such as uneven coating and excessive specific surface area, thereby causing a reduction in the power performance of the battery cell.

[0221] By comparing Examples 1 and 18 to 21, it can be seen that compared with Examples 20 to 21, Examples 1 and 18 to 19 have better electrical performance of the battery prepared by the positive electrode lithium supplement material under the more suitable second time condition. When the boiling and loosening time of potassium tetratitanate whiskers is not within the preferred parameter range provided by the present invention, the performance of the battery prepared by the obtained positive electrode lithium supplement material will be reduced. After sintering, the potassium tetratitanate whiskers need to be heated and stirred in water to make them dispersed completely to the standard that can be used. This process is also called boiling and loosening process. When the boiling time is short, the whiskers cannot be completely loosened to form a network. When the boiling time is too long, the water molecules will destroy the whisker structure.

[0222] By comparing Examples 1, 22 to 25, it can be seen that, compared with Examples 24 to 25, Examples 1, 22 to 23 have better electrical performance of the battery prepared by the positive electrode lithium supplement material within a more suitable mass ratio range of the second product to lithium ferrite. When the ratio of the coating material to the substrate, that is, the ratio of the coating layer material to the lithium ferrite, is not within the preferred parameter range provided by the present invention, the performance of the battery prepared by the obtained positive electrode lithium supplement material will be reduced. If the coating material is too little, the coating layer will be too thin to exert the coating effect of the coating layer. If the coating material is too much, the coating layer will be too thick, which will increase the transmission distance of lithium ions and affect the power and cycle performance of the battery cell.

[0223] By comparing Examples 1, 26 to 29, it can be seen that compared with Examples 28 to 29, Examples 1, 26 to 27 have better electrical performance of the battery prepared by the positive electrode lithium supplement material within a more suitable potassium tetratitanate whisker length range. When the potassium tetratitanate whisker length is not within the preferred parameter range provided by the present invention, the performance of the battery prepared by the obtained positive electrode lithium supplement material will be reduced. If the whisker length is too short, the coating layer is not enough to form a sufficient conductive network. If the potassium tetratitanate whisker length is too long, it will form agglomerations, affecting the power and cycle performance of the battery cell.

[0224] By comparing Examples 1, 30 to 33, it can be seen that compared with Examples 32 to 33, Examples 1, 30 to 31 have better electrical performance of the battery prepared by the positive electrode lithium supplement material in a more suitable potassium ferrite particle size range. When the potassium ferrite particle size range is not within the preferred parameter range provided by the present invention, the performance of the battery prepared by the obtained positive electrode lithium supplement material will be reduced. If the material particle size is too small, agglomeration will be formed. If the material particle size is too large, the lithium ion transmission distance will be increased, affecting the power and cycle performance of the battery cell.

[0225] By comparing Example 1 with Comparative Examples 1 to 2, it can be seen that without coating, the material performance cannot be improved. By comparing Example 1 with Comparative Example 3, it can be seen that without ball milling, the coating layer cannot effectively perform its function.

[0226] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0227] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.

[0228] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0229] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0230] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A positive electrode lithium supplement material, characterized in that: The positive electrode lithium supplement material comprises lithium ferrite and a coating layer, wherein the coating layer is coated on at least a portion of the surface of the lithium ferrite; The coating layer includes MOFs material and potassium tetratitanate whiskers; The MOFs material includes an iron-based MOFs material, wherein the iron-based MOFs material includes Fe2(dobdc); The potassium tetratitanate whiskers are doped in the MOFs material to form a conductive network in the coating layer; The mass proportion of the potassium tetratitanate whiskers in the positive electrode lithium supplement material is 0.5% to 15%; The mass proportion of the MOFs material in the positive electrode lithium supplement material is 1% to 15%.

2. The positive electrode lithium supplement material according to claim 1, characterized in that: The coating layer has a thickness of 15 nm to 60 nm.

3. The positive electrode lithium supplement material according to claim 1 or 2, characterized in that: The average particle size of the lithium ferrite is 6 μm to 9 μm; And / or, the average particle size of the positive electrode lithium supplement material is 10 μm to 15 μm.

4. The positive electrode lithium supplement material according to claim 1 or 2, characterized in that: The average diameter of the potassium tetratitanate whisker is 1nm-3nm, and the length of the potassium tetratitanate whisker is 20nm-100nm.

5. A method for preparing a positive electrode lithium supplement material, characterized in that: The following steps are involved: An iron source, an organic ligand, a first solvent and a second solvent are mixed and reacted at a first temperature for a first time to obtain a first product; wherein the iron source comprises at least one of ferric chloride, ferric nitrate or ferric sulfate; the organic ligand comprises 2,5-dihydroxyterephthalic acid (H4DOBDC); and the molar ratio of the iron source to the organic ligand is 5:(1-3); The first product is mixed with potassium tetratitanate whisker powder, reacted at a second temperature for a second time, and washed and dried to obtain a second product; The second product, the third solvent and lithium ferrite are mixed, wherein the mass ratio of the second product to the lithium ferrite is (1-3):

8. After ball milling, a coating layer including MOFs material and potassium tetratitanate whiskers is formed on the surface of the lithium ferrite to obtain the positive electrode lithium supplement material.

6. The method for preparing the positive electrode lithium supplement material according to claim 5, characterized in that: The step of obtaining the first product satisfies at least one of the following characteristics (1) to (3): (1) The first solvent includes at least one of alcohols, ketones or ethers; (2) the second solvent comprises N,N-dimethylformamide; (3) The first temperature is 120°C to 160°C, and the first time is 15h to 25h.

7. The method for preparing a positive electrode lithium supplement material according to claim 5, characterized in that: The step of obtaining the second product satisfies at least one of the following characteristics (1) to (4): (1) In the positive electrode lithium supplement material, the mass content of the potassium tetratitanate whiskers is 0.5% to 15%; (2) The second temperature is 90°C to 120°C, and the second time is 2h to 6h; (3) The washing solvent includes at least one of methanol, ethanol, propanol or acetone, and the washing frequency is not less than 3 times; (4) The drying temperature is 60°C to 80°C.

8. The method for preparing a positive electrode lithium supplement material according to any one of claims 5 to 7, characterized in that: The third solvent comprises at least one of methanol, ethanol, propanol or acetone; And / or, the rotation speed of the ball mill is 500-2000 r / min, and the time of the ball mill is 0.5h-2h.

9. A positive electrode sheet, characterized in that: It includes a current collector and a positive electrode active material layer arranged on the surface of the current collector; The positive electrode active material layer comprises the positive electrode lithium replenishing material according to any one of claims 1 to 4 or the positive electrode lithium replenishing material prepared by the method according to any one of claims 5 to 8, as well as a positive electrode active material, a conductive agent and a binder; The mass proportion of the positive electrode lithium supplement material in the positive electrode active material layer is 0.5% to 4%.

10. A battery, characterized in that: It includes the positive electrode sheet and the negative electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • Positive lithium supplementing material, preparation method thereof, positive plate and secondary battery

    CN115249792A

  • Composite positive electrode material and preparation method thereof, positive electrode plate and secondary battery

    CN117276546A

  • Positive electrode lithium supplementing material and preparation method thereof, positive electrode plate and secondary battery

    CN117577848A

  • Iron-based lithium supplementing material for positive electrode, and preparation method therefor and use thereof

    WO2024012481A1