Platinum / palladium-based catalyst for CO oxidation resistant to heavy metal poisoning, preparation method and application thereof

By uniformly loading the Pt-Pd/WO3-Cr2O3 catalyst on the TiO2 carrier and processing it in NaOH or KOH medium, the problem of poisoning and deactivation of the precious metal catalyst caused by heavy metals is solved, and efficient CO oxidation performance and resistance to heavy metal poisoning are achieved.

CN118304885BActive Publication Date: 2024-10-18ZHEJIANG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410448530.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-10-18
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

The activity of existing CO oxidation catalysts decreases rapidly in the presence of heavy metals (such as Se and As), causing the problem of poisoning and deactivation of precious metal catalysts that has not been effectively solved.

Method used

Using TiO2 as a carrier, the Pt-Pd/WO3-Cr2O3 catalyst is supported by wet impregnation and treated in NaOH or KOH medium to enhance the redox ability of the catalyst, reduce the interaction between heavy metals and precious metals, and improve the ability to resist heavy metal poisoning.

Benefits of technology

In the range of 180-220°C, the catalyst's CO removal efficiency is greater than 92%, and it remains efficient in the presence of 0.2% SeO2 or As2O3, significantly improving its resistance to heavy metal poisoning and CO oxidation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004791838860000091
    Figure BDA0004791838860000091
  • Figure BDA0004791838860000101
    Figure BDA0004791838860000101
  • Figure BDA0004791838860000111
    Figure BDA0004791838860000111
Patent Text Reader

Abstract

The present invention belongs to the field of environmental catalysis technology, relates to an atmospheric pollutant, especially the field of CO purification technology, and particularly relates to a heavy metal poisoning resistant CO oxidation platinum / palladium-based catalyst, a preparation method and its application. The catalyst comprises a carrier and an active component loaded on the carrier, the catalyst also comprises a co-catalyst, and the catalyst comprises the following components in mass percentage: 0.05-0.2% active component, 4-15% co-catalyst, and the balance is carrier TiO 2 , active components, co-catalysts and carriers TiO 2 The sum of the mass percentages is 100%; the active component is selected from a single component Pt or Pd, or a Pt-Pd dual component; the co-catalyst includes WO 3 3‑10%, Cr 2 O 3 0.5-3% and 0.5-2% of either NaOH or KOH. The catalyst has good resistance to heavy metal (Se, As, etc.) poisoning and better CO oxidation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental catalysis technology, relates to an atmospheric pollutant, especially CO purification technology, and particularly relates to a heavy metal poisoning-resistant CO oxidation platinum / palladium-based catalyst, a preparation method and an application thereof. Background Art

[0002] With the progress of society and the development of industry, environmental pollution issues have increasingly attracted people's attention. Carbon monoxide (CO) is one of the main pollutants in the atmosphere, mainly from tail gas emissions from incomplete combustion of fossil fuels such as coal, oil and natural gas, and chemical production processes. CO is a flammable, explosive and highly toxic gas. Excessive emissions will not only cause great harm to the ecological environment, but also pose a serious threat to the human body. Therefore, studying efficient and environmentally friendly CO waste gas removal technology and effectively reducing CO emissions are of great significance to protecting the environment and human health.

[0003] The CO catalytic oxidation method is to catalytically convert CO into non-toxic CO2 under the action of a catalyst. The method has the advantages of high removal efficiency, low cost, deep removal, wide application range, and no secondary pollution. In the CO catalytic oxidation reaction, noble metal (Pt, Pd, etc.) catalysts have high CO oxidation activity and good stability, but in actual industrial flue gas, SO2, H2O and heavy metals (Se, As, etc.) are often contained, which affect the activity of the catalyst, resulting in a rapid decrease in the activity of the noble metal catalyst, affecting the actual use effect of the catalyst. CN114669286A provides a platinum-based catalyst for CO oxidation and its preparation method and application. The platinum-based catalyst uses TiO2-SiO2 composite oxide as a carrier, Pt as an active component, and adopts a co-hydrolysis method. By adjusting the molar ratio of TiO2 and SiO2, the amount of noble metal Pt is reduced, the synergistic effect between the carrier and the active component is fully exerted, and the size of the active component is increased, so that it has a high CO catalytic oxidation efficiency while improving sulfur resistance. CN114643065A discloses a noble metal catalyst for catalytic oxidation of CO and a preparation method thereof, wherein the noble metal catalyst uses a one-step mechanical ball milling method to load one or more of the noble metals Pt, Ag, Pd, Rh, Ir, Ru, Os or Au on the surface of anatase TiO2, and adds one or more of the auxiliary agents Co, Cr, Zr, Sn, Mo, W, Fe, Ce, Ni, Nb, etc., so that the catalyst can achieve complete conversion of CO at a relatively low temperature and has good sulfur and water resistance. The water resistance and sulfur resistance of the existing CO oxidation catalysts have been greatly improved, but the poisoning and deactivation of the noble metal (Pt, Pd, etc.) catalyst caused by heavy metals (Se, As, etc.) has not been effectively solved. Summary of the invention

[0004] The object of the present invention is to provide a heavy metal poisoning resistant CO oxidation platinum / palladium-based catalyst, which has good heavy metal poisoning resistance and better CO oxidation performance.

[0005] The second object of the present invention is to provide a method for preparing the heavy metal poisoning-resistant CO oxidation platinum / palladium-based catalyst.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] A heavy metal poisoning resistant CO oxidation catalyst comprises a carrier and an active component loaded on the carrier, and the catalyst also comprises a co-catalyst. The catalyst comprises the following components in mass percentage: 0.05-0.2% of the active component, 4-15% of the co-catalyst, and the balance is the carrier TiO2, and the sum of the mass percentages of the active component, the co-catalyst and the carrier TiO2 is 100%; wherein the active component is selected from single-component Pt or Pd, or Pt-Pd double-component; the co-catalyst comprises 3-10% of WO3, 0.5-3% of Cr2O3, and 0.5-2% of one of NaOH or KOH.

[0008] In the preparation method of the heavy metal poisoning resistant CO oxidation catalyst of the present invention, a uniformly loaded Pt-Pd / WO3-Cr2O3-TiO2 catalyst is obtained by a method of wet impregnation loading followed by rotary evaporation treatment, and a heavy metal (Se, As, etc.) poisoning resistant CO oxidation catalyst is obtained by an impregnation loading method of NaOH or KOH. The WO3-Cr2O3 in the catalyst can interact with the precious metals Pt and Pd, thereby increasing the redox ability of the catalyst and promoting the catalyst activity, while reducing the interaction between the heavy metal oxides and the precious metals Pt and Pd. NaOH or KOH provides more alkaline sites, preferentially reacts with the heavy metal oxides, and reduces the toxicity of the heavy metal oxides, so that the catalyst has better heavy metal poisoning resistance and better CO oxidation performance.

[0009] Preferably, the TiO2 is nano-anatase TiO2 with an average pore diameter of 10-20 nm and a total pore volume of >0.3 ml / g.

[0010] Preferably, when the active component is a Pt-Pd dual component, the mass ratio of Pt to Pd is 1:5-1:10.

[0011] Preferably, the catalyst comprises the following components in mass percentage: active component Pd or Pt-Pd dual component 0.1-0.2%, carrier TiO2 85.9-89.9%, WO3 7-10%, Cr2O3 2-3% and one of NaOH or KOH 1-2%.

[0012] A method for preparing a heavy metal poisoning resistant CO oxidation catalyst according to the present invention comprises the following steps:

[0013] S1. Prepare an impregnation solution containing ammonium metatungstate and chromium nitrate, immerse the dried carrier in the impregnation solution and stir for 60-120 minutes, perform rotary evaporation for 10-60 minutes, and then dry at 105-120° C. for 12-24 hours, and then calcine at 450-550° C. for 3-5 hours, and then fully grind to obtain WO3-Cr2O3-TiO2 powder;

[0014] S2, preparing a precursor solution containing an active component, stirring and dissolving it at 40-60° C. to obtain a precursor solution;

[0015] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution of S2 for wet impregnation loading for 30-60 min, ultrasonically oscillating, rotary evaporating the obtained solution for 10-60 min, then drying at 105-120°C for 12-24 h, and then calcining at 400-550°C for 3-5 h;

[0016] S4. The material obtained in S3 is placed in a NaOH or KOH solution, stirred for 30-60 minutes, and then subjected to rotary evaporation for 10-60 minutes, and then dried at 105-120° C. for 12-24 hours to obtain a CO oxidation catalyst resistant to heavy metal poisoning.

[0017] Preferably, the drying condition of the carrier after drying in S1 is drying at a temperature of 105-120° C. for 12-24 hours.

[0018] Preferably, in the impregnation solution, chromium nitrate is added in the form of chromium nitrate oxalic acid solution, and the mass concentration of oxalic acid in the chromium nitrate oxalic acid solution is 1%-10%.

[0019] Preferably, the precursor solution containing the active component is a solution obtained by adding one or both of platinum salt or palladium salt to water or dilute nitric acid; the concentration of the dilute nitric acid is 0.5-5%; the platinum salt is chloroplatinic acid, platinum nitrate or dinitrosodiammineplatinum, and the palladium salt is palladium chloride or palladium nitrate.

[0020] Preferably, the ultrasonic oscillation time in S3 is 10-30 min. A suitable time can make the Pt and Pd loading more uniform.

[0021] An application of the CO oxidation platinum / palladium-based catalyst according to claim 1, characterized in that the CO oxidation platinum / palladium-based catalyst is used for catalytic oxidation treatment of industrial flue gas containing CO.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. In the catalyst prepared by the method of the present invention, WO3-Cr2O3 and the noble metal have a synergistic effect, which increases the redox ability of the catalyst, promotes the catalyst activity, and reduces the interaction between selenium oxide and arsenic oxide and the noble metal. NaOH or KOH provides more alkaline sites, preferentially reacts with heavy metal oxides, and reduces the toxicity of heavy metal oxides. The heavy metal poisoning-resistant CO oxidation platinum / palladium-based catalyst prepared by the present invention has a CO removal efficiency of more than 92% in the range of 180-220°C. When loaded with 0.2% mass fraction of SeO2 or As2O3, in the same range, its CO removal efficiency is more than 84.5%, showing good resistance to heavy metal poisoning and better CO oxidation performance.

[0024] 2. The raw materials in the preparation method of the present invention are easily available, the process is simple, energy-saving, and suitable for industrial application. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described in detail below through specific embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any form of modification and / or change made to the present invention will fall within the protection scope of the present invention.

[0026] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0027] The carrier used in the following examples is TiO2, nano-grade anatase TiO2, commercially available, with an average pore diameter of 10-20 nm and a total pore volume of >0.3 ml / g.

[0028] Example 1

[0029] A method for preparing a heavy metal poisoning-resistant platinum-based CO oxidation catalyst, the specific steps are as follows:

[0030] S1. A solution prepared by stirring ammonium metatungstate at 50°C and dissolving it in water and a solution prepared by stirring chromium nitrate at 50°C and dissolving it in 5% oxalic acid are mixed to obtain an impregnation solution, and a TiO2 carrier dried at 105°C for 12 hours is impregnated therein, stirred for 60 minutes, subjected to rotary evaporation for 10 minutes, and then dried at 105°C for 12 hours, and then calcined at 450°C for 3 hours, and then fully ground to obtain WO3-Cr2O3-TiO2 powder;

[0031] S2, adding chloroplatinic acid into deionized water, stirring and dissolving at 40° C. to obtain a precursor solution;

[0032] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution for wet impregnation loading for 30 minutes, ultrasonically vibrating for 10 minutes, rotary evaporating the obtained solution for 10 minutes, and then drying at 105°C for 12 hours, and then calcining at 400°C for 3 hours to obtain a Pt / WO3-Cr2O3-TiO2 catalyst;

[0033] S4, the Pt / WO3-Cr2O3-TiO2 catalyst obtained in S3 is placed in a NaOH solution and stirred evenly for 30 minutes, then subjected to rotary evaporation for 10 minutes, and then dried in an oven at 105°C for 12 hours to obtain a heavy metal poisoning resistant CO oxidation catalyst. The catalyst composition is as follows by mass percentage: carrier TiO2 87.9%, active component Pt 0.1%, promoter WO 38%, promoter Cr2O 33%, and promoter NaOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0034] Example 2

[0035] A method for preparing a heavy metal poisoning-resistant CO oxidation palladium-based catalyst, the specific steps are as follows:

[0036] S1. A solution prepared by stirring ammonium metatungstate at 60°C and dissolving it in water and a solution prepared by stirring chromium nitrate at 60°C and dissolving it in 5% oxalic acid are mixed to obtain an impregnation solution, and a TiO2 carrier dried at 110°C for 18 hours is impregnated therein, stirred for 90 minutes, subjected to rotary evaporation for 30 minutes, and then dried at 110°C for 12 hours, and then calcined at 500°C for 4 hours, and then fully ground to obtain WO3-Cr2O3-TiO2 powder;

[0037] S2, adding palladium nitrate into 0.5% dilute nitric acid solution, stirring and dissolving at 50° C. to obtain a precursor solution;

[0038] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution for wet impregnation loading for 30 minutes, ultrasonically vibrating for 15 minutes, rotary evaporating the obtained solution for 30 minutes, and then drying at 110°C for 18 hours, and then calcining at 500°C for 4 hours to obtain a Pd / WO3-Cr2O3-TiO2 catalyst;

[0039] S4, the Pd / WO3-Cr2O3-TiO2 catalyst obtained in S3 is placed in a NaOH solution and stirred evenly for 45 minutes, then subjected to rotary evaporation for 30 minutes, and then dried in an oven at 110°C for 18 hours to obtain a heavy metal poisoning resistant CO oxidation catalyst. The catalyst composition is as follows by mass percentage: carrier TiO2 87.95%, active component Pd 0.05%, promoter WO 38%, promoter Cr2O 33%, and promoter NaOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0040] Example 3

[0041] A method for preparing a heavy metal poisoning-resistant CO oxidation palladium-based catalyst, the specific steps are as follows:

[0042] S1. A solution prepared by stirring ammonium metatungstate at 60°C and dissolving it in water and a solution prepared by stirring chromium nitrate at 60°C and dissolving it in 5% oxalic acid are mixed to obtain an impregnation solution, and a TiO2 carrier dried at 110°C for 18 hours is impregnated therein, stirred for 90 minutes, subjected to rotary evaporation for 30 minutes, and then dried at 110°C for 12 hours, and then calcined at 500°C for 4 hours, and then fully ground to obtain WO3-Cr2O3-TiO2 powder;

[0043] S2, adding palladium nitrate into 0.5% dilute nitric acid solution, stirring and dissolving at 50° C. to obtain a precursor solution;

[0044] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution for wet impregnation loading for 30 minutes, ultrasonically vibrating for 15 minutes, rotary evaporating the obtained solution for 30 minutes, and then drying at 110°C for 18 hours, and then calcining at 500°C for 4 hours to obtain a Pd / WO3-Cr2O3-TiO2 catalyst;

[0045] S4, the Pd / WO3-Cr2O3-TiO2 catalyst obtained in S3 is placed in a NaOH solution and stirred evenly for 45 minutes, then subjected to rotary evaporation for 30 minutes, and then dried in an oven at 110°C for 18 hours to obtain a heavy metal poisoning resistant CO oxidation catalyst. The catalyst composition is as follows by mass percentage: carrier TiO2 87.9%, active component Pd 0.1%, promoter WO 38%, promoter Cr2O 33%, and promoter NaOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0046] Example 4

[0047] A method for preparing a heavy metal poisoning-resistant CO oxidation palladium-based catalyst, the specific steps are as follows:

[0048] S1. A solution prepared by stirring ammonium metatungstate at 60°C and dissolving it in water and a solution prepared by stirring chromium nitrate at 60°C and dissolving it in 5% oxalic acid are mixed to obtain an impregnation solution, and a TiO2 carrier dried at 110°C for 18 hours is impregnated therein, stirred for 90 minutes, subjected to rotary evaporation for 30 minutes, and then dried at 110°C for 12 hours, and then calcined at 500°C for 4 hours, and then fully ground to obtain WO3-Cr2O3-TiO2 powder;

[0049] S2, adding palladium nitrate into 0.5% dilute nitric acid solution, stirring and dissolving at 50° C. to obtain a precursor solution;

[0050] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution for wet impregnation loading for 30 minutes, ultrasonically vibrating for 15 minutes, rotary evaporating the obtained solution for 30 minutes, and then drying at 110°C for 18 hours, and then calcining at 500°C for 4 hours to obtain a Pd / WO3-Cr2O3-TiO2 catalyst;

[0051] S4, the Pd / WO3-Cr2O3-TiO2 catalyst obtained in S3 is placed in a NaOH solution and stirred evenly for 45 minutes, then subjected to rotary evaporation for 30 minutes, and then dried in an oven at 110°C for 18 hours to obtain a heavy metal poisoning resistant CO oxidation catalyst. The catalyst composition is as follows by mass percentage: carrier TiO2 86.8%, active component Pd 0.2%, promoter WO 38%, promoter Cr2O 33%, and promoter NaOH 2%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0052] Example 5

[0053] A method for preparing a heavy metal poisoning-resistant platinum-palladium-based CO oxidation catalyst, the specific steps are as follows:

[0054] S1. A solution prepared by stirring ammonium metatungstate at 60°C and dissolving it in water and a solution prepared by stirring chromium nitrate at 60°C and dissolving it in 5% oxalic acid are mixed to obtain an impregnation solution, and a TiO2 carrier dried at 110°C for 18 hours is impregnated therein, stirred for 90 minutes, subjected to rotary evaporation for 30 minutes, and then dried at 110°C for 12 hours, and then calcined at 500°C for 4 hours, and then fully ground to obtain WO3-Cr2O3-TiO2 powder;

[0055] S2, adding platinum nitrate and palladium chloride into a 0.5% dilute nitric acid solution, stirring and dissolving at 50° C. to obtain a precursor solution;

[0056] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution for wet impregnation loading for 30 minutes, ultrasonically vibrating for 15 minutes, rotary evaporating the obtained solution for 30 minutes, and then drying at 110°C for 18 hours, and then calcining at 500°C for 4 hours to obtain a Pt-Pd / WO3-Cr2O3-TiO2 catalyst;

[0057] S4, the Pt-Pd / WO3-Cr2O3-TiO2 catalyst obtained in S3 is placed in a KOH solution and stirred evenly for 45 minutes, then subjected to rotary evaporation for 30 minutes, and then dried in an oven at 110°C for 18 hours to obtain a heavy metal poisoning resistant CO oxidation catalyst. The catalyst composition is as follows by mass percentage: carrier TiO2 89.9%, active component Pt 0.0167%, active component Pd 0.0833%, promoter WO 37%, promoter Cr2O 32%, promoter KOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0058] Example 6

[0059] A method for preparing a heavy metal poisoning-resistant platinum-palladium-based CO oxidation catalyst, the specific steps are as follows:

[0060] S1. A solution prepared by stirring ammonium metatungstate at 60°C and dissolving it in water and a solution prepared by stirring chromium nitrate at 60°C and dissolving it in 5% oxalic acid are mixed to obtain an impregnation solution, and a TiO2 carrier dried at 110°C for 18 hours is impregnated therein, stirred for 90 minutes, subjected to rotary evaporation for 30 minutes, and then dried at 110°C for 12 hours, and then calcined at 500°C for 4 hours, and then fully ground to obtain WO3-Cr2O3-TiO2 powder;

[0061] S2, adding dinitrodiammine platinum and palladium chloride into a 0.5% dilute nitric acid solution, stirring and dissolving at 50° C. to obtain a precursor solution;

[0062] S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution for wet impregnation loading for 30 minutes, ultrasonically vibrating for 15 minutes, rotary evaporating the obtained solution for 30 minutes, and then drying at 110°C for 18 hours, and then calcining at 500°C for 4 hours to obtain a Pt-Pd / WO3-Cr2O3-TiO2 catalyst;

[0063] S4, the Pt-Pd / WO3-Cr2O3-TiO2 catalyst obtained in S3 is placed in a KOH solution and stirred evenly for 45 minutes, then subjected to rotary evaporation for 30 minutes, and then dried in an oven at 110°C for 18 hours to obtain a heavy metal poisoning resistant CO oxidation catalyst. The catalyst composition is as follows by mass percentage: carrier TiO2 89.9%, active component Pt 0.0091%, active component Pd 0.091%, promoter WO3 10%, promoter Cr2O3 3%, promoter KOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0064] Comparative Example 1

[0065] Steps S1 and S4 in Example 3 are removed, and other conditions remain unchanged.

[0066] The CO oxidation catalyst obtained in this comparative example has the following composition by mass percentage: carrier TiO2 99.9%, active component Pd 0.1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0067] Compared with Example 3, this comparative example does not load the co-catalysts WO3, Cr2O3 and NaOH. The purpose is to investigate the differences in the catalytic CO oxidation activity and the resistance to heavy metal poisoning of the catalyst in the absence of the synergistic effect of WO3 and Cr2O3 and the action of NaOH.

[0068] Comparative Example 2

[0069] Step S1 in Example 3 is removed, and other conditions remain unchanged.

[0070] The CO oxidation catalyst obtained in this comparative example has the following composition by mass percentage: carrier TiO2 98.9%, active component Pd 0.1%, promoter NaOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0071] Compared with Example 3, this comparative example does not load the co-catalyst WO3 and Cr2O3, the purpose of which is to investigate the differences in the catalytic CO oxidation activity and the resistance to heavy metal poisoning of the catalyst in the absence of the synergistic effect of WO3 and Cr2O3.

[0072] Comparative Example 3

[0073] In step S1 of Example 3, chromium nitrate and oxalic acid are not added, and other conditions remain unchanged.

[0074] The CO oxidation catalyst obtained in this comparative example has the following composition by mass percentage: carrier TiO2 90.9%, active component Pd 0.1%, promoter WO38%, promoter NaOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0075] Compared with Example 3, this comparative example does not load the co-catalyst Cr2O3, the purpose of which is to investigate the differences in the catalytic CO oxidation activity and the resistance to heavy metal poisoning of the catalyst in the absence of Cr2O3.

[0076] Comparative Example 4

[0077] In step S1 of Example 3, ammonium metatungstate is not added, and other conditions remain unchanged.

[0078] The CO oxidation catalyst obtained in this comparative example has the following composition by mass percentage: carrier TiO2 95.9%, active component Pd 0.1%, promoter Cr2O33%, promoter NaOH 1%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0079] Compared with Example 3, this comparative example does not load the co-catalyst WO3, the purpose of which is to investigate the differences in the catalytic oxidation of CO activity and the resistance to heavy metal poisoning of the catalyst in the absence of WO3.

[0080] Comparative Example 5

[0081] Step S4 in Example 3 is removed, and other conditions remain unchanged.

[0082] The CO oxidation catalyst obtained in this comparative example has the following composition by mass percentage: carrier TiO2 88.9%, active component Pd 0.1%, promoter WO 38%, promoter Cr2O 33%. The prepared catalyst is crushed and sieved to obtain catalyst particles with a particle size between 60 and 40 meshes.

[0083] Compared with Example 3, this comparative example does not load the co-catalyst NaOH, the purpose of which is to investigate the differences in the catalytic oxidation of CO activity and the resistance to heavy metal poisoning of the catalyst in the absence of NaOH.

[0084] Summary and Analysis of Examples and Comparative Examples

[0085] The catalyst compositions in the various embodiments and comparative examples are summarized as shown in Table 1.

[0086] Table 1 Summary of catalyst compositions in Examples and Comparative Examples

[0087] <![CDATA[TiO2(%)]]> Pt(%) Pd(%) <![CDATA[WO3(%)]]> <![CDATA[Cr2O3(%)]]> NaOH / KOH(%) Example 1 87.9 0.1 / 8 3 1 Example 2 87.95 / 0.05 8 3 1 Example 3 87.9 / 0.1 8 3 1 Example 4 86.8 / 0.2 8 3 2 Example 5 89.9 0.0167 0.0833 7 2 1 Example 6 85.8999 0.0091 0.091 10 3 1 Comparative Example 1 99.9 / 0.1 / / / Comparative Example 2 98.9 / 0.1 / / 1 Comparative Example 3 90.9 / 0.1 8 / 1 Comparative Example 4 95.9 / 0.1 / 3 1 Comparative Example 5 88.9 / 0.1 8 3 /

[0088] 1. CO removal test

[0089] In order to verify the catalytic CO oxidation performance of the catalysts prepared in the above examples, performance tests were performed on the CO oxidation catalysts prepared in Examples 1-6 and Comparative Examples 1-5.

[0090] 0.1 g of the catalyst particles prepared in each example was taken and placed in a catalyst activity evaluation device. The activity evaluation was carried out in a fixed bed reactor with an inner diameter of 8 mm. CO / N2 and air were mixed after being controlled by a mass flow meter. Deionized water was injected into the heating pipeline by adjusting the injection volume of a micro-injection pump to vaporize water to achieve the addition of water vapor. A simulated flue gas was obtained, the composition of which was 5000 ppm CO, 50 ppm SO2, and 10% H2O. Air was the balance gas, and the air velocity was 300000 ml×g -1 ×h -1 The catalyst activity was tested by MGA6 Plus. The CO removal efficiency of different catalysts is shown in Table 2.

[0091] Table 2 CO removal efficiency

[0092]

[0093] The following conclusions can be drawn from Table 2:

[0094] (1) The platinum / palladium-based catalysts for CO oxidation of Examples 1-6 have high CO removal efficiency and good activity. The Pd catalysts loaded with the same content have a higher CO removal efficiency than the Pt catalysts. When the Pt content in the two-component Pt-Pd catalyst is low, the CO removal efficiency is close to that of the Pd catalyst. The higher the Pd content in the catalyst, the higher the CO removal efficiency.

[0095] (2) By comparing Example 3 with Comparative Examples 1 and 2, it can be seen that under the same conditions, the catalyst loaded with WO3-Cr2O3 has a higher CO removal efficiency and exhibits better activity.

[0096] (3) Comparing Example 3 with Comparative Examples 3 and 4, it can be seen that under the same conditions, the CO removal efficiency of the catalyst loaded with WO3 or Cr2O3 alone is not as high as that of the catalyst loaded with WO3-Cr2O3 at the same time.

[0097] (4) By comparing Example 3 with Comparative Example 5, it can be seen that the CO removal efficiency of the catalyst impregnated with NaOH or KOH is basically the same as that of the catalyst not impregnated with NaOH or KOH, and does not affect the activity of the heavy metal poisoning resistant CO oxidation catalyst.

[0098] 2. Test on CO removal efficiency of various catalysts after selenium poisoning

[0099] In order to verify the anti-heavy metal selenium and arsenic poisoning characteristics of the CO oxidation catalyst prepared in the above embodiments, the catalysts in the above embodiments and comparative examples were subjected to simulated selenium and arsenic poisoning, respectively. Specifically, the CO oxidation catalyst was placed in a fixed bed reactor, and the selenium-containing and arsenic-containing solutions were injected into the preheater by a peristaltic pump, and gas-phase SeO2 and As2O3 were formed after heating. Using air as a carrier gas, gas-phase SeO2 and As2O3 were brought into the reactor and deposited on the catalyst. By controlling the concentration of arsenic-containing and selenium-containing solutions, the flow rate of the peristaltic pump, the temperature of the preheater and other parameters, the loading amounts of SeO2 and As2O3 on the catalyst were accurately achieved to be 0.2wt%, respectively. Then, the catalysts after simulating selenium and arsenic poisoning were tested for CO removal performance, and the test conditions were the same as above. The CO removal efficiency of different catalysts is shown in Tables 3 and 4.

[0100] Table 3 CO removal efficiency of each catalyst after selenium poisoning

[0101]

[0102] The following conclusions can be drawn from Table 3:

[0103] (1) After the CO oxidation platinum / palladium-based catalysts of Examples 1-6 were poisoned with 0.2 wt% SeO2, the CO removal efficiency of each catalyst decreased, but the CO removal efficiency of the Pd catalyst loaded with the same content was still higher than that of the Pt catalyst. The higher the Pd content in the catalyst, the higher the CO removal efficiency.

[0104] (2) By comparing Example 3 with Comparative Examples 1 and 2, it can be seen that under the same SeO2 poisoning conditions, the catalyst without WO3-Cr2O3 and NaOH loading has a greater decrease in CO removal efficiency, while the catalyst loaded with WO3-Cr2O3 and NaOH has a higher CO removal efficiency and exhibits better activity.

[0105] (3) By comparing Example 3 with Comparative Examples 3 and 4, it can be seen that under the same SeO2 poisoning condition, the CO removal efficiency of the catalyst loaded with WO3 or Cr2O3 alone is not as high as that of the catalyst doped with WO3-Cr2O3 at the same time, and the decline is more obvious.

[0106] (4) By comparing Example 3 with Comparative Example 5, it can be seen that under the same SeO2 poisoning conditions, the catalyst impregnated with NaOH or KOH has a higher CO removal efficiency than the unimpregnated catalyst, showing a higher resistance to heavy metal SeO2 poisoning.

[0107] Table 4 CO removal efficiency of each catalyst after arsenic poisoning

[0108]

[0109] The following conclusions can be drawn from Table 4:

[0110] (1) After the CO oxidation platinum / palladium-based catalysts of Examples 1-6 were poisoned with 0.2 wt% As2O3, the CO removal efficiency of each catalyst decreased, but the CO removal efficiency of the Pd catalyst with the same loading content was still higher than that of the Pt catalyst. The higher the Pd content in the catalyst, the higher the CO removal efficiency.

[0111] (2) By comparing Example 3 with Comparative Examples 1 and 2, it can be seen that under the same As2O3 poisoning conditions, the catalyst without WO3-Cr2O3 and NaOH loading has a greater decrease in CO removal efficiency, while the catalyst loaded with WO3-Cr2O3 and NaOH has a higher CO removal efficiency and exhibits better activity.

[0112] (3) Comparing Example 3 with Comparative Examples 3 and 4, it can be seen that under the same As2O3 poisoning condition, the CO removal efficiency of the catalyst loaded with WO3 or Cr2O3 alone is not as high as that of the catalyst doped with WO3-Cr2O3 at the same time, and the decline is more obvious.

[0113] (4) By comparing Example 3 with Comparative Example 5, it can be seen that under the same As2O3 poisoning conditions, the catalyst impregnated with NaOH or KOH has a higher CO removal efficiency than the unimpregnated catalyst, showing a higher resistance to heavy metal As2O3 poisoning.

[0114] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0115] The above is a detailed introduction to a heavy metal poisoning resistant CO oxidation platinum / palladium-based catalyst, preparation method and application provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A heavy metal poisoning resistant CO oxidation catalyst, the catalyst comprising a carrier and an active Component, characterized in that: The catalyst also includes a co-catalyst, and the catalyst includes the following components in percentage by mass: Active ingredient 0.05-0.2%, Promoter 4-15%, The balance is carrier TiO2, and the sum of the mass percentages of active components, co-catalysts and carrier TiO2 is 100%; Wherein, the active component is selected from single component Pt or Pd, or Pt-Pd dual component; The promoter includes WO3 3-10%, Cr2O3 0.5-3%, and one of NaOH or KOH 0.5-2%.

2. The heavy metal poisoning resistant CO oxidation catalyst according to claim 1, characterized in that: The TiO2 is nano-anatase TiO2 with an average pore diameter of 10-20 nm and a total pore volume of >0.3 ml / g.

3. The heavy metal poisoning resistant CO oxidation catalyst according to claim 1, characterized in that: When the active component is a Pt-Pd dual component, the mass ratio of Pt to Pd is 1:5-1:

10.

4. The heavy metal poisoning resistant CO oxidation catalyst according to claim 1, characterized in that The catalyst comprises the following components in percentage by mass: 0.1-0.2% of active component Pd or Pt-Pd dual component, 85.9-89.9% of carrier TiO2, 7-10% of WO3, 2-3% of Cr2O3 and 1-2% of one of NaOH or KOH.

5. A method for preparing a heavy metal poisoning resistant CO oxidation catalyst according to claim 1, characterized in that The method comprises the following steps: S1. Prepare an impregnation solution containing ammonium metatungstate and chromium nitrate, immerse the dried carrier in the impregnation solution and stir for 60-120 minutes, perform rotary evaporation for 10-60 minutes, and then dry at 105-120° C. for 12-24 hours, and then calcine at 450-550° C. for 3-5 hours, and then fully grind to obtain WO3-Cr2O3-TiO2 powder; S2, preparing a precursor solution containing an active component, stirring and dissolving it at 40-60° C. to obtain a precursor solution; S3, placing the WO3-Cr2O3-TiO2 powder obtained in S1 in the precursor solution of S2 for wet impregnation loading for 30-60 min, ultrasonically oscillating, rotary evaporating the obtained solution for 10-60 min, then drying at 105-120°C for 12-24 h, and then calcining at 400-550°C for 3-5 h; S4. The material obtained in S3 is placed in a NaOH or KOH solution, stirred for 30-60 minutes, and then subjected to rotary evaporation for 10-60 minutes, and then dried at 105-120° C. for 12-24 hours to obtain a CO oxidation catalyst resistant to heavy metal poisoning.

6. The preparation method according to claim 5, characterized in that: The drying condition of the carrier after drying in S1 is drying at a temperature of 105-120° C. for 12-24 hours.

7. The preparation method according to claim 5, characterized in that: In the impregnation solution, chromium nitrate is added in the form of chromium nitrate oxalic acid solution, and the mass concentration of oxalic acid in the chromium nitrate oxalic acid solution is 1%-10%.

8. The preparation method according to claim 5, characterized in that: The precursor solution containing active components is a solution obtained by adding one or both of platinum salt or palladium salt into water or dilute nitric acid; the concentration of the dilute nitric acid is 0.5-5%; the platinum salt is chloroplatinic acid, platinum nitrate or dinitrosodiammineplatinum, and the palladium salt is palladium chloride or palladium nitrate.

9. The preparation method according to claim 5, characterized in that: The time of ultrasonic oscillation in S3 is 10-30 minutes.

10. Use of the CO oxidation catalyst according to claim 1, characterized in that: The CO oxidation catalyst is used for catalytic oxidation treatment of CO-containing industrial flue gas.

Citation Information

Patent Citations

  • Precious metal catalyst for catalytic oxidation of CO and preparation method thereof

    CN114643065A

  • Platinum-based catalyst for CO oxidation and preparation method and application thereof

    CN114669286A

  • Catalyst for synergistic control of oxynitride and mercury and method for preparing same

    CN105263617A

  • Pt-based catalyst for CO purification as well as preparation method and application of the Pt-based catalyst

    CN111185167A

  • Non-noble metal composite oxide catalyst as well as preparation method and application thereof

    CN114618512A