A method for preparing a self-crosslinking waterproofing agent for denim fabrics

Through the preparation method of self-crosslinking waterproofing agent, the reaction of polyurethane prepolymer and blocked isocyanate with hydroxyl epoxy POSS, combined with stearyl methacrylate and water-soluble functional monomers, solves the problem of existing fluorine-free waterproofing agents. The problem of insufficient environmental protection and washability in textile materials has been achieved by improving the waterproof performance of efficient and environmentally friendly products.

CN118307722BActive Publication Date: 2024-10-22韶关市北纺智造科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410416668.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-10-22
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

The application of existing fluorine-free waterproofing agents in textile materials has problems such as poor environmental protection, insufficient water resistance, and high complexity of use. In particular, it is difficult to improve the waterproof performance of denim fabrics to meet market demand.

Method used

A method for preparing a self-crosslinking waterproofing agent is adopted, through the reaction of polyurethane prepolymer and blocked isocyanate with hydroxyl epoxy POSS, combined with stearyl methacrylate, butyl acrylate and water-soluble functional monomer DMC, and the use of initiator The agent initiates a reaction to form a self-crosslinking waterproofing agent that does not require the addition of an external cross-linking agent.

Benefits of technology

It achieves environmental protection, washability and simple waterproof performance improvement, improves the combination of fiber and waterproof agent, enhances the waterproof effect, and does not require the addition of an external emulsifier for emulsion polymerization, and has good stability and high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307722B_ABST
    Figure CN118307722B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a self-crosslinking waterproofing agent for denim fabrics, comprising the following steps: S1, reacting the NCO at one end of a polyurethane prepolymer with the OH in hydroxyethyl acrylate to obtain a single-end-capped product, and then end-capping the NCO at the other end of the single-end-capped product with a hydroxyl epoxy POSS to obtain a blocked isocyanate; S2, adding blocked isocyanate to octadecyl methacrylate melted into a liquid at 80°C, and then dropping monomers butyl acrylate, hydroxypropyl methacrylate and paraffin therein respectively, stirring evenly and heating to 90°C, and then adding deionized water of the same temperature to obtain a mixed solution; dissolving a water-soluble functional monomer DMC in the remaining deionized water to obtain a functional monomer solution, dissolving an initiator in the functional monomer solution and dropping it in batches into the mixed solution to initiate a reaction, and cooling and bottling after the reaction is complete to obtain a self-crosslinking waterproofing agent. The waterproofing agent prepared by the present invention is environmentally friendly and washable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of textile materials, and in particular to a self-crosslinking waterproofing agent and a preparation method thereof. Background Art

[0002] Denim fabrics are known for their rugged, strong, bold and exaggerated appearance, and are deeply loved by young people. With the continuous changes in market demand, denim fabrics are also more delicate and colorful. The application of denim fabrics in the design of bags and shoes enhances the artistic charm and cultural connotation of the design, reflecting the current fashion style and aesthetic needs of people for bags and shoes. It can be foreseen that the application design of denim fabrics will have better market value in the future bags and shoes market. With the technological progress of modern dyeing and finishing processes, functional finishing of textile fabrics is an important means to increase the added value of textiles. Waterproof finishing of denim fabrics can give denim bags and shoes good waterproof properties, increase the added value of denim bags and shoes, thereby meeting the increasingly diversified needs of consumers and creating economic benefits for enterprises.

[0003] Traditional fluorine-based waterproofing agents have excellent waterproofing properties and are inexpensive and good quality. They once dominated the waterproofing agent market. However, with long-term use, people gradually discovered that this type of waterproofing agent is not environmentally friendly, difficult to degrade, and has strong bioaccumulation. The most serious thing is that it can cause cancer. With the global attention to environmental pollution control and the improvement of quality requirements for related products, many countries in the world have adopted policies to restrict the use of fluorine elements to reduce pollution to the environment. Therefore, it has become a general trend to develop high-quality fluorine-free waterproofing agents. At present, there are two main types of fluorine-free waterproofing agents: alkane long-chain water repellents and silicone water repellents. Alkane long-chain water repellents include common paraffin-metal salts, hydroxymethyl, pyridine, etc. and silicone water repellents. Paraffin-metal salt water repellents are easy to use and inexpensive, but they are not resistant to washing and dry cleaning, feel hard and have a sour taste. They can only be used in industrial fabrics that are not often washed, such as low-end applications such as covering cloth and curtains. The simplest hydroxymethyl waterproofing agent is hydroxymethyl stearamide, which was developed by ICI of the United Kingdom and is traded under the name VelanNW. Hydroxylmethyl waterproofing agents are aqueous dispersions, which are not stable enough for storage and are not widely used. Pyridine quaternary ammonium salt waterproofing agents can provide long-lasting waterproofing properties, but toxic gases (hydrogen chloride and pyridine) will be released during the finishing process, so they are not environmentally friendly products and have been eliminated. Silicone waterproofing agents have a decent waterproofing effect and are suitable for cotton fabrics that require a soft touch; at the same time, because they are two components, they are more troublesome to use, have poor stability, and are easy to demulsify, so they are not suitable for high-speed waterproofing processing of chemical fiber fabrics. In addition, most of the fluorine-free waterproofing agents on the market are linear polymer materials with poor water washing performance, and cross-linking agents are often required to improve the durability of the waterproof finishing effect. Therefore, there is an urgent need for a method for preparing an environmentally friendly, washable self-cross-linking waterproofing agent. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a method for preparing a self-crosslinking waterproofing agent for denim fabrics.

[0005] The purpose of the present invention is achieved by the following technical solutions:

[0006] A method for preparing a self-crosslinking waterproof agent for denim fabrics, comprising the following steps: S1, preparing a self-crosslinking waterproof agent having a structural formula The -NCO at one end of the polyurethane prepolymer reacts with the -OH in hydroxyethyl acrylate to obtain a single-terminated product, and then the -NCO at the other end of the single-terminated product is capped with a hydroxyl epoxy POSS to obtain a blocked isocyanate;

[0007] S2. Add blocked isocyanate to octadecyl methacrylate melted into liquid at 80°C, then drop monomers butyl acrylate, hydroxypropyl methacrylate and paraffin respectively, stir evenly and heat to 90°C, then add deionized water of the same temperature to obtain a mixed solution; dissolve the water-soluble functional monomer DMC in the remaining deionized water to obtain a functional monomer solution, dissolve the initiator in the functional monomer solution and drop it into the mixed solution in batches to initiate the reaction, cool and bottle after the reaction is complete to obtain a self-crosslinking waterproofing agent.

[0008] Preferably, the mass ratio of octadecyl methacrylate, blocked isocyanate, hydroxypropyl methacrylate, butyl acrylate, water-soluble functional monomer DMC, paraffin, initiator and deionized water is (21-25): (2-5): 2:3:3:1:0.5:100.

[0009] Preferably, the initiator is V50.

[0010] Preferably, the structural formula is The PO / EO copolyether is added with isophorone dicyanate under nitrogen protection at 70°C, and a drop of catalyst dibutyltin dilaurate is added, the temperature is gradually raised to 75°C, and the polyurethane prepolymer is obtained after reacting for 2 hours. In the structural formula of the PO / EO copolyether, X1=1-3, X2=1-3, Y=5-15; the mass ratio of PO / EO copolyether to isophorone diisocyanate is 200:(80.6-88.9).

[0011] Preferably, the hydroxyl-containing epoxy POSS is obtained by stirring epoxy POSS and dimethylamine at a constant temperature of 70° C. for 5 hours, and each 0.1 mol of epoxy POSS corresponds to 13.5 g of dimethylamine.

[0012] Preferably, the epoxy POSS is one of glycidyloxypropyl cage-type polysilsesquioxane and octa-epoxycyclohexylethyl cage-type polysilsesquioxane.

[0013] Preferably, the mass ratio of PO / EO copolyether, isophorone diisocyanate, hydroxyethyl acrylate and hydroxyl epoxy POSS is 200: (80.6-88.9): 11.6: (60.3-100.5)

[0014] Preferably, the initiator is dissolved in the functional monomer solution and then added dropwise to the mixed solution in five equal portions, with each portion being added for 1 hour.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The waterproofing agent prepared by the invention is more environmentally friendly and easier to prepare than the traditional acrylic waterproofing agent; after being blocked by a specific epoxy POSS with a hydroxyl group, it will be unblocked at a certain temperature, and the exposed -NCO after unblocking will react and combine with the group of the denim fabric fiber, so that the waterproofing agent prepared by the invention does not need to be additionally added with a cross-linking agent during use, and part of the epoxy group can react with the hydroxyl group on the denim fabric fiber, thereby being fixed on the fiber, thereby improving the waterproofing effect of the waterproofing agent, and improving the washability of the waterproofing agent.

[0017] 2. Octadecanyl methacrylate is insoluble in water. Its molecule has an octadecyl hydrophobic group. When mixed with water, it will eventually separate and float on the upper layer of the water phase. This characteristic determines the application of octadecyl methacrylate in water phase polymerization. The place of free radical polymerization is the water phase. If it is not pulled into the water phase, octadecyl methacrylate will not participate in the polymerization. To solve this problem, an emulsifier is needed. Blocked isocyanate contains PO / EO polyether segments by connecting hydroxyl epoxy POSS and hydroxyethyl acrylate. It has a certain emulsification property, so emulsion polymerization can be carried out without the addition of an emulsifier. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the particle size column distribution diagram of the emulsion in Example 1. DETAILED DESCRIPTION

[0019] In order to make the technical problems solved by the present invention, the technical solutions adopted and the technical effects achieved clearer, the technical solutions of the embodiments of the present invention will be further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0020] Example 1

[0021] (1) Preparation of hydroxyl-containing epoxy POSS

[0022] Take a 500ml clean and dry four-necked flask, add 133.8g of glycidyloxypropyl cage-type polysilsesquioxane, and add 13.5g of dimethylamine dropwise under stirring. After the addition is complete, continue stirring, heat to 70°C, and react at a constant temperature for 5h to obtain the product. The reaction formula is as follows:

[0023]

[0024] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0025] Take a 1000ml clean and dry four-necked flask, add 200g PO / EO copolyether, evacuate the PO / EO copolyether at 110℃ to remove the moisture in the reactant for 1h. After evacuation, adjust the temperature of the oil bath to 70℃ and cool it down. After cooling, add 88.9g of isophorone dicyanate (IPDI) under nitrogen protection. At the same time, add a drop of catalyst dibutyltin dilaurate, gradually adjust the temperature of the oil bath, control the reaction temperature at 75℃, and the reaction time is 2 hours to obtain a polyurethane prepolymer. The reaction formula is as follows:

[0026]

[0027] In the structural formula of PO / EO copolyether, X1=1-3, X2=1-3, Y=5-15. After the reaction is completed, 11.6g of hydroxyethyl acrylate is added to react the -NCO at one end of the polyurethane prepolymer with the hydroxyl group in the hydroxyethyl acrylate, and the reaction is continued at 80°C for 2h. After the heat preservation is completed, 60.3g of hydroxyl epoxy POSS is added to cap the single-terminated product, and the heat preservation is carried out at 80°C for 30min to finally obtain the blocked isocyanate. The reaction formula is as follows:

[0028]

[0029] (3) Preparation of self-crosslinking waterproofing agent

[0030] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour before being cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 1:

[0031] Table 1 Synthesis formula of self-crosslinking waterproofing agent 1

[0032]

[0033] Example 2

[0034] (1) Preparation of hydroxyl-epoxy POSS

[0035] Take a 500ml clean and dry four-necked flask, add 141.8g of octaepoxycyclohexylethyl caged polysilsesquioxane, and add 13.5g of dimethylamine dropwise under stirring. After the addition is complete, continue stirring, heat to 70°C, and react at a constant temperature for 5h to obtain the product. The reaction formula is as follows:

[0036]

[0037] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0038] Take a 1000ml clean and dry four-necked flask, add 200g PO / EO copolyether, in the structural formula of PO / EO copolyether, X1=1-3, X2=1-3, Y=5-15, evacuate the PO / EO copolyether at 110℃ to remove the water in the reactant for 1h. After evacuation, adjust the temperature of the oil bath to 70℃ and cool it down. After cooling, add 80.6g of isophorone dicyanate (IPDI) under nitrogen protection. At the same time, add a drop of catalyst dibutyltin dilaurate, gradually adjust the temperature of the oil bath, control the reaction temperature at about 75℃, and the reaction time is 2 hours. After the reaction is completed, add 11.6g of hydroxyethyl acrylate to react the -NCO at one end of the polyurethane prepolymer with the hydroxyl group in hydroxyethyl acrylate, and keep the temperature at 80℃ to continue the reaction for 2h. After the heat preservation was completed, 60.3 g of hydroxyl epoxy POSS was added to cap the single-terminated product, and the product was heat-sealed at 80° C. for 30 minutes to obtain blocked isocyanate.

[0039] (2) Preparation of self-crosslinking waterproofing agent

[0040] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour before being cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 2:

[0041] Table 2 Synthesis formula of self-crosslinking waterproofing agent 2

[0042]

[0043] Example 3

[0044] (1) Epoxy POSS with hydroxyl groups

[0045] The same operation as in Example 1 was carried out under the same conditions.

[0046] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0047] Take a 1000ml clean and dry four-necked flask, add 200g PO / EO copolyether, in the structural formula of PO / EO copolyether, X1=1-3, X2=1-3, Y=5-15, evacuate the PO / EO copolyether at 110℃ to remove the water in the reactant for 1h. After evacuation, adjust the temperature of the oil bath to 70℃ and cool it down. After cooling, add 80.6g of isophorone dicyanate (IPDI) under nitrogen protection. At the same time, add a drop of catalyst dibutyltin dilaurate, gradually adjust the temperature of the oil bath, control the reaction temperature at about 75℃, and the reaction time is 2 hours. After the reaction is completed, add 11.6g of hydroxyethyl acrylate to react the -NCO at one end of the polyurethane prepolymer with the hydroxyl group in hydroxyethyl acrylate, and keep the temperature at 80℃ to continue the reaction for 2h. After the heat preservation was completed, 82.1 g of hydroxyl epoxy POSS was added to cap the single-terminated product, and the product was heat-sealed at 80° C. for 30 minutes to obtain blocked isocyanate.

[0048] (3) Preparation of self-crosslinking fluorine-free waterproofing agent

[0049] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour before being cooled and bottled. A self-crosslinking fluorine-free waterproofing agent is obtained. The specific formula is shown in Table 3:

[0050] Table 3 Synthesis formula of self-crosslinking waterproofing agent 3

[0051]

[0052] Example 4

[0053] (1) Preparation of hydroxyl-epoxy POSS

[0054] The same operation as in Example 1 was carried out under the same conditions.

[0055] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0056] Take a 1000ml clean and dry four-necked flask, add 200g PO / EO copolyether, in the structural formula of PO / EO copolyether, X1=1-3, X2=1-3, Y=5-15, evacuate the PO / EO copolyether at 110℃ to remove the water in the reactant for 1h. After evacuation, adjust the temperature of the oil bath to 70℃ and cool it down. After cooling, add 80.6g of isophorone dicyanate (IPDI) under nitrogen protection. At the same time, add a drop of catalyst dibutyltin dilaurate, gradually adjust the temperature of the oil bath, control the reaction temperature at about 75℃, and the reaction time is 2 hours. After the reaction is completed, add 11.6g of hydroxyethyl acrylate to react the -NCO at one end of the polyurethane prepolymer with the hydroxyl group in hydroxyethyl acrylate, and keep the temperature at 80℃ to continue the reaction for 2h. After the heat preservation was completed, 100.5 g of hydroxyl epoxy POSS was added to cap the single-terminated product, and the product was heat-sealed at 80° C. for 30 minutes to obtain blocked isocyanate.

[0057] (3) Preparation of self-crosslinking waterproofing agent

[0058] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 4:

[0059] Table 4 Synthesis formula of self-crosslinking waterproofing agent 4

[0060]

[0061] Example 5

[0062] (1) Preparation of hydroxyl-epoxy POSS

[0063] The same operation as in Example 1 was carried out under the same conditions.

[0064] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0065] The same operation as in Example 1 was carried out under the same conditions to obtain blocked isocyanate.

[0066] (3) Preparation of self-crosslinking waterproofing agent

[0067] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate monomer, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 80r / min, turn on the heating button at the same time, and heat it to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip it in five times, and each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 5:

[0068] Table 5 Synthesis formula of self-crosslinking waterproofing agent 5

[0069]

[0070] Example 6

[0071] (1) Preparation of hydroxyl-epoxy POSS

[0072] The same operation as in Example 1 was carried out under the same conditions.

[0073] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0074] The same operation as in Example 1 was carried out under the same conditions to obtain blocked isocyanate.

[0075] (3) Preparation of self-crosslinking waterproofing agent

[0076] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate monomer, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 6:

[0077] Table 6 Synthesis formula of self-crosslinking waterproofing agent

[0078]

[0079] Example 7

[0080] (1) Preparation of hydroxyl-epoxy POSS

[0081] The same operation as in Example 1 was carried out under the same conditions.

[0082] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0083] The same operation as in Example 1 was carried out under the same conditions to obtain a blocked isocyanate monomer.

[0084] (3) Preparation of self-crosslinking waterproofing agent

[0085] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate monomer, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 7:

[0086] Table 7 Synthesis formula of self-crosslinking fluorine-free waterproofing agent 7

[0087]

[0088] Example 8

[0089] (1) Preparation of hydroxyl-epoxy POSS

[0090] The same operation as in Example 1 was carried out under the same conditions.

[0091] (2) Preparation of blocked isocyanates based on PO / EO block copolyethers

[0092] The same operation as in Example 1 was carried out under the same conditions to obtain a blocked isocyanate monomer.

[0093] (3) Preparation of self-crosslinking waterproofing agent

[0094] After melting the waxy solid macromonomer SMA into a liquid in an oven at 80°C, add the blocked isocyanate monomer, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. A self-crosslinking waterproofing agent is obtained. The specific formula is shown in Table 8:

[0095] Table 8 Synthesis formula of self-crosslinking fluorine-free waterproofing agent 8

[0096]

[0097] Comparative Example 1

[0098] After melting the waxy solid macromonomer SMA into liquid in an oven at 80°C, add it to a four-necked flask together with Tween and Span. At the same time, add 1831 solid octadecyltrimethylammonium chloride to the reactor (four-necked flask), and then use a dropper to add oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Then repeat the dropping step 4 times (i.e. dropwise addition in five times, each dropwise addition lasts about 1 hour). The total dropwise addition time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. The external crosslinking agent waterproofing agent is obtained. It is recorded as a comparative sample. The specific formula is shown in Table 9:

[0099] Table 9 Synthetic formula of waterproofing agent 9

[0100]

[0101] Comparative Example 2

[0102] (1) Preparation of hydroxyl-epoxy POSS

[0103] The same operation as in Example 1 was carried out under the same conditions.

[0104] (2) Preparation of waterproofing agent

[0105] After melting the waxy solid macromonomer SMA into liquid in an oven at 80°C, add the modified POSS, and then use a dropper to add the oily functional monomers butyl acrylate (Ba), hydroxypropyl methacrylate (HPMA), and paraffin. Assemble the instrument, plug in the power supply, start stirring, adjust the stirring speed to 280r / min, turn on the heating button at the same time, and heat to about 90°C. After stirring for 30 minutes, slowly add 60ml of heated deionized water (pre-heat the deionized water to about 90°C with a thermoelectric heating jacket). After keeping the reaction warm for 30 minutes, weigh the water-soluble functional monomer DMC and dissolve it in 40ml of deionized water to obtain the functional monomer solution. Then dissolve 1 / 5 of the initiator V50 in the 1 / 5 functional monomer solution and add it dropwise to the reactor with a constant flow pump. Appropriately adjust the constant flow pump rate so that it drips in about 1 hour. Repeat the dripping step 4 times (that is, drip in five times, each dripping time is about 1 hour). The total dripping time is about 5 hours, and then the mixture is kept warm for 1 hour and then cooled and bottled. The waterproofing agent is obtained. The specific formula is shown in Table 10:

[0106] Table 10 Synthetic formula of waterproofing agent 10

[0107]

[0108] Performance test of waterproofing agent

[0109] 1) Waterproof finishing process

[0110] First, the sample fabric selected for the waterproof finishing process is a cotton fabric with strong water absorption. The polyacrylic acid emulsion is diluted 100 times, with a gram weight of 110g / L. The two-immersion and two-rolling process is adopted, and the soaking is 60s. The rolling rate is 100%, and then the soaked cotton fabric is placed in an oven for drying. The appropriate temperature is set to 90℃ and the appropriate time is 10min. After the drying is completed, it is baked again. The appropriate temperature is 145℃ and the appropriate time is 3min. The simple process is as follows:

[0111] Cotton fabric → two dips and two rolls (polyacrylic acid fluorine-free waterproofing agent 110g / L, diluted 100 times, soaking for 60s, rolling rate 100%) → drying (90℃, 10min) → baking (145℃, 3min).

[0112] 2) Emulsion particle size test

[0113] The sample solid content was diluted to 1%, shaken for 10 minutes, and the particle size of the acrylic emulsion was tested at room temperature using a laser particle size analyzer. Figure 1 As shown:

[0114] Depend on Figure 1 It can be seen that the particle sizes of the acrylic emulsion obtained in Example 1 are mostly distributed around 100 nm.

[0115] Table 11 Test of emulsion particle size

[0116]

[0117] It can be seen from Table 11 that the particle size of the waterproofing agent prepared by this technology is basically below 100nm. After testing, it has good stability, the emulsion system is stable, it is not easy to demulsify in acid or alkaline environment, has good high temperature resistance, and the emulsion has a long storage time.

[0118] 3) Contact angle test

[0119] Open the contact angle meter and contact angle measurement software, select the sessile drop method, create a new file, calibrate the needle, select the Young-Laplace equation, manual baseline and other parameters. Fix the treated nonwoven fabric on the cover glass with double-sided tape, and then place it flat on the test platform, click record and drip, and end the recording after the water drop drops down. In the recorded video, capture and save the stable image after the water drop contacts the cloth. The angle in the image is the contact angle between the water drop and the cloth. Reduce the test error, and then select two other different positions to continue the test, calculate the average of the three data, and complete the test.

[0120] Table 12 Waterproof performance of fluorine-free waterproofing agent

[0121]

[0122] It can be seen from Table 12 that the self-crosslinking fluorine-free waterproofing agent emulsion prepared in Example 1 has the best waterproof performance, and the maximum contact angle is 143.2°. Compared with the self-crosslinking fluorine-free waterproofing agent prepared by glycidyl ether oxypropyl cage-type polysilsesquioxane in Example 1 and Examples 3-8, the waterproof finishing effect of the self-crosslinking fluorine-free waterproofing agent prepared by octaepoxycyclohexylethyl cage-type polysilsesquioxane in Example 2 is slightly worse, but it is also better than the waterproof finishing effect of the traditional external crosslinking agent. Continue to increase the content of the blocked isocyanate monomer, the relative content of SMA decreases, and the hydrophobicity of the film after finishing decreases, resulting in a smaller contact angle. When dried at 90°C, the effect of changing the amount of blocked isocyanate on the contact angle is very small because the blocked isocyanate deblocking temperature is about 105°C. Compared with the waterproofing agent with a traditional external crosslinking agent, the waterproof finishing effect of the self-crosslinking agent waterproofing agent prepared by the present invention is significantly better than the waterproof finishing effect of the external crosslinking agent.

[0123] 4) Fabric washability test

[0124] According to GB / T 8629-2017 standard, the water resistance test of self-crosslinking fluorine-free waterproofing agent was carried out.

[0125] Table 13 Self-crosslinking fluorine-free waterproofing agent washing resistance test

[0126]

[0127] It can be seen from Table 13 that five water washings have an effect on the static contact angles of self-crosslinked fluorine-free waterproofing and externally crosslinked fluorine-free waterproofing. Compared with the waterproofing effect and water washing resistance of the externally added crosslinking agent in Example 1-8 and Comparative Example 1, the self-crosslinking waterproofing agent prepared by this technology is significantly better than the traditional waterproofing agent that requires an externally added crosslinking agent. The contact angle of the waterproof finishing of Example 1 after 5 water washings increased from 145.1° to 140.6°, the contact angle of the waterproof finishing of Comparative Example 1 after 5 water washings increased from 123.8° to 120.6°, the contact angle of the waterproof finishing of Example 1 after 10 water washings increased from 145.1° to 134.7°, and the contact angle of the waterproof finishing of Comparative Example 1 after 10 water washings increased from 123.8° to 110.8°. The waterproofing effect and water washing resistance of Example 1 are better than the waterproof finishing effect of the externally added crosslinking agent in the comparative example. The modified POSS in comparative example 2 does not have access to -NCO groups, and the prepared waterproofing agent cannot be self-crosslinked during the finishing process, so the water-washing resistance of the waterproofing agent prepared by Example 10 is poor, and the contact angle drops from 143.5° to 97.9° after washing 10 times. The fluorine-free waterproofing agent of the present invention will unblock and expose the -NCO group therein at 105°C, and then the -NCO group will react and combine with the group in the fiber, and there will be a part of epoxy groups on the POSS obtained after unblocking, and these epoxy groups have the opportunity to react with the hydroxyl groups on the cellulose fiber, thereby fixing the POSS on the fiber, thereby increasing the surface roughness, and improving the waterproofing effect of the waterproofing agent. In use, without the need for an additional crosslinking agent, the washing resistance of the fluorine-free waterproofing agent can be improved, so the self-crosslinking waterproofing agent prepared by the present invention has more excellent process performance.

[0128] The above-mentioned embodiments are only some preferred embodiments of the present invention, and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for preparing a self-crosslinking waterproofing agent for denim fabrics, characterized in that: The following steps are involved: S1, the structural formula is The -NCO at one end of the polyurethane prepolymer reacts with the -OH in hydroxyethyl acrylate to obtain a single-terminated product, and then the -NCO at the other end of the single-terminated product is terminated with a hydroxyl epoxy POSS to obtain a blocked isocyanate; S2. Add the blocked isocyanate to octadecyl methacrylate melted into a liquid at 80°C, then drop monomers butyl acrylate, hydroxypropyl methacrylate and paraffin respectively thereto, stir evenly and heat to 90°C, then add deionized water of the same temperature to obtain a mixed solution; dissolve the water-soluble functional monomer DMC in the remaining deionized water to obtain a functional monomer solution, dissolve the initiator in the functional monomer solution and drop it into the mixed solution in batches to initiate a reaction, cool and bottle after the reaction is complete to obtain a self-crosslinking waterproofing agent; the mass ratio of the octadecyl methacrylate, blocked isocyanate, hydroxypropyl methacrylate, butyl acrylate, water-soluble functional monomer DMC, paraffin, initiator and deionized water is (21-25): (2-5): 2:3:3:1:0.5:100; the initiator is V50; the structural formula is The PO / EO copolyether is placed under nitrogen protection at 70°C, isophorone dicyanate is added, and a drop of catalyst dibutyltin dilaurate is added, the temperature is gradually raised to 75°C, and the polyurethane prepolymer is obtained after reacting for 2 hours. In the structural formula of the PO / EO copolyether, X1=1-3, X2=1-3, and Y=5-15; the mass ratio of the PO / EO copolyether to the isophorone diisocyanate is 200:(80.6-88.9).

2. The method for preparing a self-crosslinking waterproofing agent for denim fabric according to claim 1, characterized in that: The hydroxyl-containing epoxy POSS is obtained by stirring epoxy POSS and dimethylamine at a constant temperature of 70° C. for 5 hours, and each 0.1 mol of the epoxy POSS corresponds to 13.5 g of the dimethylamine.

3. The method for preparing a self-crosslinking waterproofing agent for denim fabric according to claim 2, characterized in that: The epoxy POSS is one of glycidyloxypropyl cage-type polysilsesquioxane and octa-epoxycyclohexylethyl cage-type polysilsesquioxane.

4. The method for preparing a self-crosslinking waterproofing agent for denim fabric according to claim 3, characterized in that: The mass ratio of the PO / EO copolyether, isophorone diisocyanate, hydroxyethyl acrylate and hydroxyl-containing epoxy POSS is 200: (80.6-88.9): 11.6: (60.3-100.5).

5. The method for preparing the self-crosslinking waterproofing agent for denim fabric according to claim 1, characterized in that After the initiator is dissolved in the functional monomer solution, it is divided into five equal portions and added dropwise to the mixed solution, and the addition time of each portion is 1 hour.

Citation Information

Patent Citations

  • Fluoride-free waterproof agent with stereo silane structure and preparation method of fluoride-free waterproof agent

    CN106810650A

  • POSS modified polyacrylate fluoride-free waterproof agent and preparation method thereof

    CN111410712A

  • Vinyl-terminated prepolymers having low viscosity and good water solubility

    WO2016193302A1