A corrosion-resistant aluminum alloy material and its preparation process

By introducing Sc, Zr, Ti and other elements into the Al-Zn-Mg-Cu series aluminum alloy, and using homogenization annealing, hot extrusion and solid solution heat treatment, combined with the compounding of corrosion-resistant coatings, traditional aluminum alloy materials have been solved. The problem of insufficient corrosion resistance in extreme environments improves the corrosion resistance and service life of the material.

CN118308619BActive Publication Date: 2024-10-22CHANGZHOU INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410421009.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-10-22
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

Traditional corrosion-resistant aluminum alloy materials show insufficient corrosion resistance in high temperature, high humidity and acid-base corrosive environments, and are prone to corrosion and oxidation, affecting the performance and life of the material, and alloying may reduce the strength and toughness of the material.

Method used

A preparation process is adopted, including the introduction of Sc, Zr, Ti and other elements into the Al-Zn-Mg-Cu series aluminum alloy, and through homogenization annealing, hot extrusion, solid solution heat treatment and aging treatment, combined with bisphenol A ring Corrosion-resistant coating compounded with oxyacrylate and polyester acrylate to enhance the adhesion and corrosion resistance of the coating.

Benefits of technology

It effectively improves the corrosion resistance, strength and toughness of aluminum alloy materials, extends its service life, and inhibits metal oxidation through the phosphate radicals and double bonds in the anti-corrosion compound, significantly improving the degree of coating solidification and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of aluminum alloy materials, specifically to a corrosion-resistant aluminum alloy material and a preparation process thereof. The aluminum alloy material includes the following chemical compositions by mass percentage: Si: 0.05-0.15%, Fe: 0.1-0.2%, Cu: 1.2-1.5%, Mn: 0.7-0.9%, Mg: 2.5-3.8%, Zn: 10.2-12.4%, Ti: 0.02-0.04%, Zr: 0.08-0.15%, Sc: 0.2-0.4%, and the balance is Al. The present invention obtains an aluminum alloy material through processes such as melting, refining, casting, and heat treatment, and applies a corrosion-resistant coating on its surface. After ultraviolet curing treatment, not only the durability and anti-flaking properties of the coating are improved; at the same time, the corrosion resistance of the material is enhanced, and the service life of the aluminum alloy material is effectively extended.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a corrosion-resistant aluminum alloy material and a preparation process thereof. Background Art

[0002] Corrosion-resistant aluminum alloy materials are widely used in aerospace, automobile manufacturing, construction and other fields. Traditional corrosion-resistant aluminum alloy materials mainly include aluminum-magnesium alloy, aluminum-zinc alloy, etc. The traditional preparation process includes extrusion, rolling, heat treatment and other steps to obtain aluminum alloy materials with good corrosion resistance.

[0003] However, with the continuous development of industrial technology, there are still some specific problems with existing corrosion-resistant aluminum alloys. In order to improve the corrosion resistance of aluminum alloys, alloying elements are usually added, but this may lead to a contradiction between strength and toughness. Alloying may reduce the plasticity and toughness of the material, thereby affecting its reliability in practical applications. In addition, in some extreme environments, such as high temperature, high humidity, acid and alkali corrosion, traditional corrosion-resistant aluminum alloys may show insufficient corrosion resistance, prone to corrosion and oxidation, which in turn affects the performance and life of the material.

[0004] Therefore, we propose a corrosion-resistant aluminum alloy material and a preparation process thereof. Summary of the invention

[0005] The object of the present invention is to provide a corrosion-resistant aluminum alloy material and a preparation process thereof to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A preparation process of a corrosion-resistant aluminum alloy material comprises the following steps:

[0008] Step S1: putting an aluminum ingot into a melting furnace, heating it to 720-750°C, keeping it warm for 40-50 minutes, and obtaining aluminum liquid; adding Al-Si master alloy, Al-Zr master alloy, Al-Sc master alloy, Al-Cu master alloy, Al-Mn master alloy, Al-Ti-B master alloy and Fe, stirring evenly, heating to 750-800°C, keeping it warm for 1-2 hours, cooling to 740-750°C, adding Mg and Zn, stirring evenly, and obtaining alloy liquid; then adding a refining agent for refining, degassing and deslagging, and obtaining a refined liquid; casting to obtain an aluminum alloy ingot;

[0009] Step S2: subjecting the aluminum alloy ingot obtained in step S1 to homogenization annealing, hot extrusion, solution heat treatment and aging treatment to obtain an aluminum alloy material;

[0010] Step S3: grinding, polishing, cleaning and drying the surface of the aluminum alloy material obtained in step S2 in sequence, and then coating it with corrosion-resistant coating, and irradiating it with ultraviolet light to obtain a corrosion-resistant aluminum alloy material.

[0011] Furthermore, the aluminum alloy material includes the following chemical components in mass percentage: Si: 0.05-0.15%, Fe: 0.1-0.2%, Cu: 1.2-1.5%, Mn: 0.7-0.9%, Mg: 2.5-3.8%, Zn: 10.2-12.4%, Ti: 0.02-0.04%, Zr: 0.08-0.15%, Sc: 0.2-0.4%, and the balance is Al.

[0012] Furthermore, in step S1, the refining agent is hexachloroethane, and its dosage is 0.2-0.4% of the mass of the alloy liquid.

[0013] Furthermore, in step S1, the casting temperature is 720-740°C.

[0014] Furthermore, the homogenization annealing process conditions in step S2 are: first, keep warm at 420-440° C. for 4-8 hours, then keep warm at 460-480° C. for 6-12 hours, and air cool.

[0015] Furthermore, the hot extrusion process conditions in step S2 are: preheating temperature 450-480° C., holding time 2-3 h, extrusion ratio (10-15): 1, and extrusion speed 2-10 cm / s.

[0016] Furthermore, the process conditions of the solution heat treatment in step S2 are: first, keep warm at 440-450°C for 1-2h, then keep warm at 470-490°C for 1-2h, and then quench in water.

[0017] Furthermore, the aging treatment process conditions in step S2 are: aging temperature 120-150° C., and insulation time 10-20 h.

[0018] Furthermore, the preparation method of the corrosion-resistant coating in step S3 is as follows:

[0019] Bisphenol A epoxy acrylate, polyester acrylate and active diluent are mixed evenly, and anti-corrosion compound, photoinitiator, leveling agent, adhesion promoter and defoaming agent are added and mixed evenly to obtain corrosion-resistant coating.

[0020] Furthermore, the corrosion-resistant coating includes the following components by weight: 20-30 parts of bisphenol A epoxy acrylate, 40-50 parts of polyester acrylate, 15-30 parts of active diluent, 5-15 parts of anti-corrosion compound, 2-5 parts of photoinitiator, 0.5-1.0 parts of leveling agent, 0.8-1.2 parts of adhesion promoter, and 0.5-2.0 parts of defoaming agent.

[0021] Furthermore, the active diluent is tetrahydrofurfuryl acrylate.

[0022] Furthermore, the preparation method of the antiseptic compound is as follows:

[0023] Step (1): 4-allylcatechol, epichlorohydrin and benzyltriethylammonium chloride are mixed uniformly, heated to 70-80° C., reacted for 3-5 hours, cooled to 55-65° C., sodium hydroxide is added, and the reaction is continued for 4-5 hours. After washing and drying, an epoxidized monomer is obtained;

[0024] Step (2): Evenly mix lactic acid and epoxidized monomer, add triphenylphosphine and p-hydroxyanisole, mix evenly, heat to 95-105° C., react for 8-10 hours, cool to 40-50° C., add pyrophosphoric acid, mix evenly, react for 22-24 hours, extract and rotary evaporate to obtain phosphate monomer;

[0025] Step (3): Evenly mix the phosphate monomer and acetone, add polyaniline and mix evenly, and obtain an anticorrosive composite after filtering, washing and drying.

[0026] In the above technical scheme, 4-allylcatechol and epichlorohydrin react under the catalysis of benzyltriethylammonium chloride to obtain epoxidized 4-allylcatechol, that is, epoxidized monomer; then lactic acid and epoxidized monomer undergo a ring-opening reaction to introduce double bonds, and then pyrophosphoric acid is introduced to phosphorylate it to obtain a phosphate monomer containing double bonds; finally, the phosphate monomer is doped with polyaniline to obtain an anti-corrosion composite; it can not only enhance the adhesion between the coating and the substrate, and improve the durability and anti-flaking properties of the coating; it can also enhance the corrosion resistance of the coating, thereby extending the service life of the aluminum alloy material.

[0027] Furthermore, in the step (1), the mass ratio of 4-allylcatechol to epichlorohydrin and benzyltriethylammonium chloride is 1:(4-5):(0.02-0.04).

[0028] Furthermore, in step (1), the mass of sodium hydroxide is 0.25-0.30 times the mass of 4-allylcatechol.

[0029] Furthermore, in the step (2), the mass ratio of lactic acid to epoxidized monomer is 1:(0.8-1.0).

[0030] Furthermore, in step (2), the mass of triphenylphosphine is 1-3% of the mass of lactic acid.

[0031] Furthermore, in the step (2), the mass of p-hydroxyanisole is 0.5-2.0% of the mass of lactic acid.

[0032] Furthermore, in step (2), the mass of pyrophosphate is 7-8 times the mass of lactic acid.

[0033] Furthermore, in the step (3), the mass ratio of the phosphate monomer to acetone is 1:(1-3).

[0034] Furthermore, in step (3), the mass of the polyaniline is 0.5-1.0 times the mass of the phosphate monomer.

[0035] Furthermore, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0036] Furthermore, the UV irradiation process conditions are: irradiation with 360-410nm ultraviolet rays for 1-10min, irradiation intensity of 20-30mW / cm 2 .

[0037] Furthermore, the thickness of the corrosion-resistant coating is 60-120 μm.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1. A corrosion-resistant aluminum alloy material and a preparation process thereof of the present invention can effectively improve the corrosion resistance, strength and toughness of the aluminum alloy material by introducing elements such as Sc, Zr, Ti, etc. into the Al-Zn-Mg-Cu aluminum alloy and adopting homogenization annealing, hot extrusion, solution heat treatment and aging treatment processes, so that the aluminum alloy material has better performance and service life in practical applications.

[0040] 2. A corrosion-resistant aluminum alloy material and a preparation process thereof of the present invention are obtained by compounding bisphenol A epoxy acrylate and polyester acrylate, and combining them with the action of an anti-corrosion composite and a variety of additives to obtain a corrosion-resistant coating, which can effectively protect the aluminum alloy material and has lower environmental pollution; wherein the anti-corrosion composite contains phosphate and double bonds, which can not only effectively improve the corrosion resistance of the coating, enhance the adhesion of the coating, and inhibit metal oxidation, but also improve the degree of curing of the coating, thereby protecting the aluminum alloy material and extending its service life. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] In this embodiment, the aluminum ingots are: A00 aluminum ingots, with an aluminum content of ≥99.7%, sourced from Shanghai Xincheng Aluminum Co., Ltd.; Al-Si master alloy: grade Al-Si50, sourced from Wuxi Taicheng Metal Materials Products Co., Ltd.; Al-Zr master alloy: grade Al-Zr5, sourced from Suzhou Rongqian Rare Metal Products Co., Ltd.; Al-Sc master alloy: grade Al-Sc2, sourced from Suzhou Zhengde Rare Earth Materials Co., Ltd.; Al-Cu master alloy: grade Al-Cu50, sourced from Wuxi Taicheng Metal Materials Products Co., Ltd.; Al-Mn master alloy: grade Al-20Mn, Sourced from Wuxi Taicheng Metal Materials Products Co., Ltd.; Al-Ti-B master alloy: brand AlTi5B1, sourced from Shenzhen Ruihongjia Metal Materials Co., Ltd.; Fe: iron powder, 200 mesh, iron content ≥99%, sourced from Laiwu Aoxing Powder Materials Co., Ltd.; Mg: brand Mg99.98, sourced from Suzhou Rongqian Rare Metal Products Co., Ltd.; Zn: brand Zn99.95, sourced from Tianjin Zhongtonglian Metal Materials Co., Ltd.; bisphenol A epoxy acrylate: model HL-103A85, sourced from Wenzhou Hengli New Materials Co., Ltd.; polyester acrylate: model AgiSyn 730, sourced from Shanghai Guangyi Chemical Co., Ltd.; leveling agent: model BYK-333, sourced from Huizhou Aike New Materials Co., Ltd.; adhesion promoter: model PM-2, sourced from Nanjing Quanxi New Materials Co., Ltd.; defoaming agent: model AKN-3386, sourced from Foshan Qianyou Chemical Co., Ltd.

[0043] In the following examples and comparative examples, 1 part is equal to 10 g.

[0044] Embodiment 1: A process for preparing a corrosion-resistant aluminum alloy material, comprising the following process:

[0045] Step S1: putting an aluminum ingot into a melting furnace, heating it to 720°C, keeping it warm for 40 minutes, and obtaining aluminum liquid; adding Al-Si master alloy, Al-Zr master alloy, Al-Sc master alloy, Al-Cu master alloy, Al-Mn master alloy, Al-Ti-B master alloy and Fe, stirring evenly, heating to 750°C, keeping it warm for 1 hour, cooling to 740°C, adding Mg and Zn, stirring evenly, and obtaining alloy liquid; then adding a refining agent for refining (hexachloroethane, the amount of which is 0.2% of the mass of the alloy liquid), degassing and removing slag, and obtaining a refined liquid; casting to obtain an aluminum alloy ingot, the casting temperature is 720°C;

[0046] Step S2: subjecting the aluminum alloy ingot obtained in step S1 to homogenization annealing (first keeping at 420°C for 4h, then keeping at 460°C for 6h, air cooling), hot extrusion (preheating temperature 450°C, keeping time 2h, extrusion ratio 10:1, extrusion speed 2cm / s), solution heat treatment (first keeping at 440°C for 1h, then keeping at 470°C for 1h, water quenching) and aging treatment (aging temperature 120°C, keeping time 10h) to obtain an aluminum alloy material;

[0047] The aluminum alloy material includes the following chemical compositions in mass percentage: Si: 0.05%, Fe: 0.1%, Cu: 1.2%, Mn: 0.7%, Mg: 2.5%, Zn: 10.2%, Ti: 0.02%, Zr: 0.08%, Sc: 0.2%, and the balance is Al;

[0048] Step S3: The surface of the aluminum alloy material obtained in step S2 is sequentially ground, polished, cleaned and dried, and then coated with corrosion-resistant coating, and then irradiated with ultraviolet light (irradiated with 360nm ultraviolet light for 1min, irradiation intensity 30mW / cm 2 ), to obtain a corrosion-resistant aluminum alloy material;

[0049] The preparation method of the corrosion-resistant coating in step S3 is as follows:

[0050] 20 parts of bisphenol A epoxy acrylate, 40 parts of polyester acrylate and 15 parts of active diluent are mixed evenly, and 5 parts of anticorrosive compound, 2 parts of photoinitiator, 0.5 parts of leveling agent, 0.8 parts of adhesion promoter and 0.5 parts of defoamer are added and mixed evenly to obtain a corrosion-resistant coating;

[0051] The preparation method of the anticorrosive compound is as follows:

[0052] Step (1): 5 parts of 4-allylcatechol, 20 parts of epichlorohydrin and 0.1 parts of benzyltriethylammonium chloride are mixed uniformly, heated to 70° C., reacted for 3 hours, cooled to 55° C., 1.25 parts of sodium hydroxide are added, and the reaction is continued for 4 hours. After washing and drying, an epoxidized monomer is obtained;

[0053] Step (2): 5 parts of lactic acid and 4 parts of epoxidized monomer are mixed evenly, 0.05 parts of triphenylphosphine and 0.025 parts of p-hydroxyanisole are added and mixed evenly, the temperature is raised to 95° C., the mixture is reacted for 8 hours, the temperature is lowered to 40° C., 35 parts of pyrophosphoric acid are added and mixed evenly, the mixture is reacted for 22 hours, and the mixture is extracted and rotary evaporated to obtain a phosphate monomer;

[0054] Step (3): 5 parts of phosphate monomer and 5 parts of acetone are mixed evenly, and 2.5 parts of polyaniline are added and mixed evenly, and after filtering, washing and drying, an anticorrosive composite is obtained.

[0055] Embodiment 2: A process for preparing a corrosion-resistant aluminum alloy material, comprising the following process:

[0056] Step S1: putting an aluminum ingot into a melting furnace, heating it to 730°C, keeping it warm for 45 minutes, and obtaining aluminum liquid; adding Al-Si master alloy, Al-Zr master alloy, Al-Sc master alloy, Al-Cu master alloy, Al-Mn master alloy, Al-Ti-B master alloy and Fe, stirring evenly, heating to 780°C, keeping it warm for 1.5 hours, cooling to 745°C, adding Mg and Zn, stirring evenly, and obtaining alloy liquid; then adding a refining agent for refining (hexachloroethane, the amount of which is 0.3% of the mass of the alloy liquid), degassing and removing slag, and obtaining a refined liquid; casting to obtain an aluminum alloy ingot, the casting temperature is 730°C;

[0057] Step S2: subjecting the aluminum alloy ingot obtained in step S1 to homogenization annealing (first keeping at 430°C for 6 hours, then keeping at 470°C for 8 hours, air cooling), hot extrusion (preheating temperature 470°C, keeping time 2.5 hours, extrusion ratio 12:1, extrusion speed 6 cm / s), solution heat treatment (first keeping at 445°C for 1.5 hours, then keeping at 480°C for 1.5 hours, water quenching) and aging treatment (aging temperature 130°C, keeping time 15 hours) to obtain an aluminum alloy material;

[0058] The aluminum alloy material includes the following chemical compositions in mass percentage: Si: 0.10%, Fe: 0.15%, Cu: 1.3%, Mn: 0.8%, Mg: 3.6%, Zn: 11.2%, Ti: 0.03%, Zr: 0.10%, Sc: 0.3%, and the balance is Al;

[0059] Step S3: The surface of the aluminum alloy material obtained in step S2 is sequentially ground, polished, cleaned and dried, and then coated with corrosion-resistant coating. After being irradiated with ultraviolet light (irradiated with 380nm ultraviolet light for 5min, with an irradiation intensity of 25mW / cm 2 ), to obtain a corrosion-resistant aluminum alloy material;

[0060] The preparation method of the corrosion-resistant coating in step S3 is as follows:

[0061] 25 parts of bisphenol A epoxy acrylate, 45 parts of polyester acrylate and 18 parts of active diluent are mixed evenly, and 12 parts of anticorrosive compound, 3 parts of photoinitiator, 0.8 parts of leveling agent, 1 part of adhesion promoter and 1 part of defoamer are added and mixed evenly to obtain a corrosion-resistant coating;

[0062] The preparation method of the anticorrosive compound is as follows:

[0063] Step (1): 12 parts of 4-allylcatechol, 54 parts of epichlorohydrin and 0.36 parts of benzyltriethylammonium chloride were mixed uniformly, heated to 75° C., reacted for 4 hours, cooled to 60° C., 3.36 parts of sodium hydroxide were added, and the reaction was continued for 4.5 hours. After washing and drying, an epoxidized monomer was obtained;

[0064] Step (2): 12 parts of lactic acid and 10.8 parts of epoxidized monomer are mixed evenly, 0.24 parts of triphenylphosphine and 0.12 parts of p-hydroxyanisole are added and mixed evenly, the temperature is raised to 100° C., the reaction is performed for 9 hours, the temperature is lowered to 45° C., 90 parts of pyrophosphoric acid are added and mixed evenly, the reaction is performed for 23 hours, and the phosphate ester monomer is obtained by extraction and rotary evaporation;

[0065] Step (3): 12 parts of phosphate monomer and 24 parts of acetone are mixed evenly, and 9.6 parts of polyaniline are added and mixed evenly, and after filtering, washing and drying, an anticorrosive composite is obtained.

[0066] Embodiment 3: A process for preparing a corrosion-resistant aluminum alloy material, comprising the following process:

[0067] Step S1: putting an aluminum ingot into a melting furnace, heating it to 750°C, keeping it warm for 50 minutes, and obtaining aluminum liquid; adding Al-Si master alloy, Al-Zr master alloy, Al-Sc master alloy, Al-Cu master alloy, Al-Mn master alloy, Al-Ti-B master alloy and Fe, stirring evenly, heating to 800°C, keeping it warm for 2 hours, cooling to 750°C, adding Mg and Zn, stirring evenly, and obtaining alloy liquid; then adding a refining agent for refining (hexachloroethane, the amount of which is 0.4% of the mass of the alloy liquid), degassing and removing slag, and obtaining a refined liquid; casting to obtain an aluminum alloy ingot, the casting temperature is 740°C;

[0068] Step S2: subjecting the aluminum alloy ingot obtained in step S1 to homogenization annealing (first keeping at 440°C for 8h, then keeping at 480°C for 12h, air cooling), hot extrusion (preheating temperature 480°C, keeping time 3h, extrusion ratio 15:1, extrusion speed 10cm / s), solution heat treatment (first keeping at 450°C for 2h, then keeping at 490°C for 2h, water quenching) and aging treatment (aging temperature 150°C, keeping time 20h) to obtain an aluminum alloy material;

[0069] The aluminum alloy material includes the following chemical compositions in mass percentage: Si: 0.15%, Fe: 0.2%, Cu: 1.5%, Mn: 0.9%, Mg: 3.8%, Zn: 12.4%, Ti: 0.04%, Zr: 0.15%, Sc: 0.4%, and the balance is Al;

[0070] Step S3: The surface of the aluminum alloy material obtained in step S2 is sequentially ground, polished, cleaned and dried, and then coated with corrosion-resistant coating. After ultraviolet irradiation (irradiation with 410nm ultraviolet light for 10min, irradiation intensity of 20mW / cm 2 ), to obtain a corrosion-resistant aluminum alloy material;

[0071] The preparation method of the corrosion-resistant coating in step S3 is as follows:

[0072] 30 parts of bisphenol A epoxy acrylate, 50 parts of polyester acrylate and 30 parts of active diluent are mixed evenly, and 15 parts of anticorrosive compound, 5 parts of photoinitiator, 1.0 part of leveling agent, 1.2 parts of adhesion promoter and 2.0 parts of defoamer are added and mixed evenly to obtain a corrosion-resistant coating;

[0073] The preparation method of the anticorrosive compound is as follows:

[0074] Step (1): 15 parts of 4-allylcatechol, 60 parts of epichlorohydrin and 0.6 parts of benzyltriethylammonium chloride are mixed uniformly, heated to 80° C., reacted for 5 hours, cooled to 65° C., 4.5 parts of sodium hydroxide are added, and the reaction is continued for 5 hours. After washing and drying, an epoxidized monomer is obtained;

[0075] Step (2): 15 parts of lactic acid and 15 parts of epoxidized monomer are mixed evenly, 0.45 parts of triphenylphosphine and 0.3 parts of p-hydroxyanisole are added and mixed evenly, the mixture is heated to 105° C., reacted for 10 hours, cooled to 50° C., 120 parts of pyrophosphoric acid are added and mixed evenly, reacted for 24 hours, extracted and rotary evaporated to obtain a phosphate monomer;

[0076] Step (3): 15 parts of phosphate monomer and 45 parts of acetone are mixed evenly, and 15 parts of polyaniline are added and mixed evenly, and after filtering, washing and drying, an anticorrosive composite is obtained.

[0077] Comparative Example 1: The aluminum alloy material includes the following chemical components in mass percentage: Si: 0.05%, Fe: 0.1%, Cu: 1.2%, Mn: 0.7%, Mg: 1%, Zn: 2%, Ti: 0.01%, Zr: 0.01%, Sc: 0.05%, and the balance is Al; other steps and processes are the same as in Example 1.

[0078] Comparative Example 2: The corrosion-resistant coating includes the following components by weight: 20 parts of bisphenol A epoxy acrylate, 40 parts of polyester acrylate, 15 parts of active diluent, 1 part of anti-corrosion compound, 2 parts of photoinitiator, 0.5 parts of leveling agent, 0.8 parts of adhesion promoter, and 0.5 parts of defoaming agent; other steps and processes are the same as those in Example 1.

[0079] Comparative Example 3: A process for preparing a corrosion-resistant aluminum alloy material, comprising the following processes:

[0080] Compared with Example 2, in Comparative Example 3, the corrosion-resistant coating in step S3 is replaced with an aqueous acrylic resin emulsion of the same quality (model E0503, sourced from Shenzhen Yoshida Chemical Co., Ltd.); the other steps are the same as those in Example 2.

[0081] Comparative Example 4: A process for preparing a corrosion-resistant aluminum alloy material, comprising the following processes:

[0082] The preparation method of the anticorrosive compound is as follows:

[0083] Step (1): 12 parts of 4-allylcatechol, 54 parts of epichlorohydrin and 0.36 parts of benzyltriethylammonium chloride were mixed uniformly, heated to 75° C., reacted for 4 hours, cooled to 60° C., 3.36 parts of sodium hydroxide were added, and the reaction was continued for 4.5 hours. After washing and drying, an epoxidized monomer was obtained;

[0084] Step (2): 12 parts of lactic acid and 2.4 parts of epoxidized monomer are mixed evenly, 0.24 parts of triphenylphosphine and 0.12 parts of p-hydroxyanisole are added and mixed evenly, the temperature is raised to 100° C., the reaction is performed for 9 hours, the temperature is lowered to 45° C., 90 parts of pyrophosphoric acid are added and mixed evenly, the reaction is performed for 23 hours, and the phosphate ester monomer is obtained by extraction and rotary evaporation;

[0085] Step (3): 12 parts of phosphate monomer and 24 parts of acetone are mixed evenly, and 9.6 parts of polyaniline are added and mixed evenly, and after filtering, washing and drying, an anticorrosive composite is obtained;

[0086] Compared with Example 2, the mass ratio of lactic acid to epoxidized monomer in Comparative Example 4 is 1:0.2; the other steps are the same as those in Example 2.

[0087] Experiment: The corrosion-resistant aluminum alloy materials obtained in Examples 1-3 and Comparative Examples 1-4 were used to prepare samples, and their properties were tested and the test results were recorded:

[0088] Adhesion is measured according to GB / T 5210-2006 "Adhesion test for paints and varnishes by pull-off method". Experimental steps: Use a tensile testing machine to apply tensile stress in a direction perpendicular to the plane of the specimen. The stress increases steadily at a rate not exceeding 1 MPa / s. The destruction of the test combination should be completed within 90 seconds from the application of stress. Record the tensile force value that destroys the test combination.

[0089] The corrosion resistance was determined according to GB / T 1771-2007 “Determination of neutral salt spray resistance of paints and varnishes”. The experimental steps were as follows: scratch the coating with a corrosion scratcher. The scratch width was 0.3-1.0 mm. The scratch was 25 mm away from each side of the coating sample. The sample was placed in a salt spray chamber. The test solution was a 5% by mass NaCl solution. After 48 hours, the sample was observed to see if there was blistering, corrosion, etc. Three coatings were measured in parallel.

[0090] Hardness test: Cut a 10mm×10mm×5mm sample and use a HV-1000 microhardness tester with a test load of 250kgf and a loading force holding time of 20s. Perform point tests on different parts (with an interval of at least 3mm) 5 times at random and take the average value.

[0091] Test Results

[0092] Adhesion / MPa Corrosion morphology Hardness / HV Example 1 3.68 No obvious changes on the surface 312 Example 2 3.75 No obvious changes on the surface 317 Example 3 3.72 No obvious changes on the surface 315 Comparative Example 1 3.58 No obvious changes on the surface 286 Comparative Example 2 2.90 Slight corrosion 308 Comparative Example 3 2.53 Generate bubbles 295 Comparative Example 4 3.49 Slight corrosion 310

[0093] According to the data in the above table, we can clearly draw the following conclusions:

[0094] 1. Compared with Examples 1-3, the hardness of the product obtained in Comparative Example 1 decreases, indicating that the performance of the aluminum alloy material prepared by the present invention is affected by its component ratio. By selecting the component ratio within the range, a material with excellent performance can be prepared.

[0095] 2. Compared with Examples 1-3, the products obtained in Comparative Examples 2 and 3 showed a decrease in adhesion and corrosion resistance, indicating that the performance of the corrosion-resistant coating prepared by the present invention is affected by its component ratio. By selecting the component ratio within the said range, the prepared coating has excellent adhesion and corrosion resistance; compared with the water-based acrylic resin emulsion, the corrosion-resistant coating prepared by the present invention has better performance.

[0096] 3. Compared with Examples 1-3, the adhesion and corrosion resistance of the product obtained in Comparative Example 4 are both reduced. It can be seen that the performance of the anti-corrosion composite prepared by the present invention is affected by the ratio of each reagent in its preparation process. By selecting a mass ratio within the said range, the prepared anti-corrosion composite has excellent corrosion resistance, thereby extending the service life of the flange.

[0097] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0098] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A preparation process of a corrosion-resistant aluminum alloy material, Features: The steps include: Step S1: putting an aluminum ingot into a melting furnace, heating it to 720-750°C, keeping it warm for 40-50 minutes, and obtaining aluminum liquid; adding Al-Si master alloy, Al-Zr master alloy, Al-Sc master alloy, Al-Cu master alloy, Al-Mn master alloy, Al-Ti-B master alloy and Fe, stirring evenly, heating to 750-800°C, keeping it warm for 1-2 hours, cooling to 740-750°C, adding Mg and Zn, stirring evenly, and obtaining alloy liquid; then adding a refining agent for refining, degassing and deslagging, and obtaining a refined liquid; casting to obtain an aluminum alloy ingot; Step S2: subjecting the aluminum alloy ingot obtained in step S1 to homogenization annealing, hot extrusion, solution heat treatment and aging treatment to obtain an aluminum alloy material; Step S3: grinding, polishing, cleaning and drying the surface of the aluminum alloy material obtained in step S2 in sequence, coating the surface with corrosion-resistant coating, and irradiating the surface with ultraviolet light to obtain a corrosion-resistant aluminum alloy material; The aluminum alloy material includes the following chemical components in mass percentage: Si: 0.05-0.15%, Fe: 0.1-0.2%, Cu: 1.2-1.5%, Mn: 0.7-0.9%, Mg: 2.5-3.8%, Zn: 10.2-12.4%, Ti: 0.02-0.04%, Zr: 0.08-0.15%, Sc: 0.2-0.4%, and the balance is Al; The preparation method of the corrosion-resistant coating in step S3 is as follows: Bisphenol A epoxy acrylate, polyester acrylate and reactive diluent are mixed evenly, and anti-corrosion compound, photoinitiator, leveling agent, adhesion promoter and defoamer are added and mixed evenly to obtain corrosion-resistant coating; The corrosion-resistant coating comprises the following components by weight: 20-30 parts of bisphenol A epoxy acrylate, 40-50 parts of polyester acrylate, 15-30 parts of reactive diluent, 5-15 parts of anticorrosive compound, 2-5 parts of photoinitiator, 0.5-1.0 parts of leveling agent, 0.8-1.2 parts of adhesion promoter, and 0.5-2.0 parts of defoaming agent; The preparation method of the anticorrosive compound is as follows: Step (1): 4-allylcatechol, epichlorohydrin and benzyltriethylammonium chloride are mixed uniformly, heated to 70-80°C, reacted for 3-5h, cooled to 55-65°C, sodium hydroxide is added, and the reaction is continued for 4-5h. After washing and drying, an epoxidized monomer is obtained; Step (2): Evenly mix lactic acid and epoxidation monomer, add triphenylphosphine and p-hydroxyanisole, mix evenly, heat to 95-105°C, react for 8-10h, cool to 40-50°C, add pyrophosphoric acid, mix evenly, react for 22-24h, extract and rotary evaporate to obtain phosphate monomer; Step (3): uniformly mixing the phosphate monomer and acetone, adding polyaniline and mixing uniformly, filtering, washing and drying to obtain an anticorrosive composite; In the step (1), the mass ratio of 4-allylcatechol to epichlorohydrin and benzyltriethylammonium chloride is 1:(4-5):(0.02-0.04); In the step (2), the mass ratio of lactic acid to epoxidized monomer is 1:(0.8-1.0).

2. A process for preparing a corrosion-resistant aluminum alloy material according to claim 1, Features: The homogenization annealing process conditions in step S2 are: first, keep at 420-440° C. for 4-8 hours, then keep at 460-480° C. for 6-12 hours, and air cool.

3. A process for preparing a corrosion-resistant aluminum alloy material according to claim 1, Features: The process conditions of the solution heat treatment in step S2 are: first, keep warm at 440-450°C for 1-2 hours, then keep warm at 470-490°C for 1-2 hours, and then quench in water.