A method for checking the density of diode plastic packaging and controlling the process
By combining the dichotomy method with helium mass spectrometry leak detection technology and diffusion-type standard leak detectors, the problems of low detection efficiency with the naked eye and high detection costs with scanning electron microscopes are solved, and efficient and intuitive diode density detection and production process quality are achieved. Control.
Patent Information
- Application Number
- CN202410421272.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-04-09
Smart Images

Figure CN118310684B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic device detection, and in particular relates to a method for checking the compactness of diode plastic packaging and controlling the process. Background Art
[0002] With the development demand of new quality productivity, product stability and ultra-high cost-effective product requirements; the application of semiconductor diodes in automobiles, aerospace and special industries is becoming more and more extensive, especially for transient suppression diodes, ESD electrostatic diodes, Schottky diodes and plastic-sealed diodes. In order to ensure the quality and stability of the products, plastic sealing density inspection is required before leaving the factory.
[0003] At present, the traditional practice in the industry is to use artificial naked eyes for observation and detection, and the second is to use scanning electron microscope SEM. For the first method of using artificial naked eyes for observation and detection, the main problem is that naked eye detection is inefficient, has poor accuracy, and is time-consuming and laborious. For the second method of using scanning electron microscope SEM, it mainly uses ultrasonic scanning mode, focuses the ultrasonic wave emitted by the ultrasonic transducer, emits it to the surface of the sample, and then penetrates into the sample. The ultrasonic wave will generate a reflected wave signal on each interface. The sample needs to be placed in water, resulting in low scanning efficiency. Generally, it takes two hours to scan once, and the accessories are expensive. The samples completed during the experiment are basically scrapped, which wastes materials and leads to very high costs. With the rapid development of various container industries in China, coupled with the rapid development of packaging and sealing technology; there are more and more mass spectrometer leak detector manufacturers; the price of the instrument is relatively low, and it is self-controllable; the mass spectrometer leak detector is used for the detection of semiconductor diodes. It is a non-destructive and efficient method, and it is an easy-to-master solution and technical route. Therefore, in response to the above problems, this technical solution provides a method for diode plastic sealing density inspection and process control, which has important practical significance. Summary of the invention
[0004] The present invention provides a method for inspecting and controlling the compactness of a diode plastic package, which solves the problems of large errors and low efficiency in the existing manual inspection using the naked eye, and high equipment and material costs and the inability to achieve quantitative testing caused by inspection using a scanning electron microscope (SEM).
[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:
[0006] The present invention provides a method for checking the density of diode plastic packaging and controlling the process, which is used to optimize the process and use helium mass spectrometry leak detection technology to control the density of the product. Specifically, the method checks the density of the product workpiece after it has undergone die bonding and wire bonding, welding and cleaning, injection molding and packaging, and 3D visual inspection, and includes the following steps:
[0007] S1. Helium detection: The product workpieces that have completed the above steps are sampled according to the AQL strict sampling method. According to the size of the product workpiece, they are placed in the corresponding container of the corresponding helium leak detector. The mass spectrometer leak detector is sufficient to read a leak less than or equal to 10 -4 (Pa.m 3 ) / s helium detection rate, the number of samples per unit container is controlled to be n;
[0008] Specific tests include the following:
[0009] S11, placing the product workpiece into the cavity of the pressurized container and closing the cavity;
[0010] S12, evacuate the chamber to below 0.1 mbar, and then fill it with 5-6 bar of helium with a helium concentration of 99%;
[0011] S13, maintain pressure for 30-60 minutes, and release the pressure in the cavity to normal pressure;
[0012] S14, opening the cavity and taking out the product workpiece;
[0013] S15. Use dry and water-free compressed air to clean the surface of the product with helium;
[0014] S16, placing the product workpiece into the vacuum test chamber, and closing the chamber;
[0015] S17, press the leak test button to start the vacuum test;
[0016] S18. Fill the test chamber with air until it reaches atmospheric pressure, open the test chamber, take out the test product, and use a diffusion-type standard leak detector that has been calibrated by the standard at least once per shift to check the effectiveness of the instrument. The leak rate should be more than 5.0x10 - 9 mbarl / s, it is judged as unqualified, and below this leakage rate it is judged as qualified;
[0017] S2. Use the dichotomy method to judge unqualified product workpieces, specifically:
[0018] Divide the total number of product workpieces n into two equal parts of n / 2, and perform the process step S1 on the two equal parts to determine the defective conditions of the two equal parts of sample product workpieces; if one or two groups of the sample product workpieces after being divided into two equal parts are unqualified, divide the group of unqualified products into two equal parts again, perform the process step S1 again, and determine the defective conditions of the sample product workpieces after being divided into two equal parts twice; if one or two groups of the sample product workpieces after being divided into two equal parts twice are still unqualified, divide the group of unqualified products into two equal parts again and perform the process step S1 again; if there are still unqualified conditions in the subsequent groups after being divided into two equal parts, continue to divide into two equal parts, and after dividing into two equal parts at least five times, use the step S1 to determine the defective conditions of the sample product workpieces after each division; the complexity of the repetition is the standard for judging efficiency and product quality;
[0019] When n / 2 k , which means that the total number n can be completely judged after k equal parts; among them, when k>4, k=log2 n ; That is, the k value is greater than 4. After the first bisection, the k values of the left and right groups are greater than 3. That is, after more than four bisections, it can be judged that the process flow of the overall product workpiece needs to be readjusted;
[0020] The product workpieces of unqualified components are rejected, and the product workpieces of qualified components are transferred to the next step;
[0021] S3. Through the automatic test line TMTT of SMD diode products, the leakage current and withstand voltage parameters of qualified components are tested and silk-screened for easy packaging.
[0022] Furthermore, the dry water-free compressed air uses compressed air with a refrigeration capacity greater than 85PH provided by a compressor.
[0023] Furthermore, after each bisection, components with the same number or a difference of one in the bisection are regarded as bisection components of the same level.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The use of a diffusion-type standard leak detector for inspection can be based on numerical quantitative inspection. Compared with the traditional density inspection that relies on visual inspection of the appearance, ultrasonic inspection that relies on wavelength reflection to form an image, and also relies on picture judgment, it is more intuitive, faster, and more efficient;
[0026] (2) Since the product workpiece is not damaged by the use of pressurized helium filling and a diffusion-type standard leak detector for inspection, the waste of materials during the inspection process is greatly reduced, and there is no need for a high-end scanning electron microscope (SEM), which reduces the cost of purchasing instruments for inspection.
[0027] (3) Higher efficiency: Previously, a scanning electron microscope (SEM) could only detect 50 PCS at a time. However, the mass spectrometer can flexibly design the detection capacity, and can detect 500-1000 PCS or even more at a time. In addition, the steps of the present invention provide real-time quality control of the production process.
[0028] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0030] Figure 1 This is a step diagram of a method for checking the plastic package density and controlling the process of a diode according to the present invention. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] See also Figure 1 As shown, a method for checking the density of plastic packaging of diodes and controlling the process of the present invention is used to optimize the process and use helium mass spectrometry leak detection technology to control the density of products, specifically, to check the density of product workpieces that have undergone die bonding and wire bonding, welding and cleaning, injection molding and packaging, and 3D visual inspection in sequence;
[0033] For the die bonding of diode wafers, the wafer is taken out from the blue film wafer, solder is applied to the pad by spot soldering or scraping solder, and the wafer is placed on the solder of the device by the die bonding machine; for devices with wire bonding process, the wafer and the pad are first fixed by eutectic or conductive glue, and then wire bonding is arranged;
[0034] Welding and cleaning work: the workpiece after the above fixing steps is placed in a nitrogen welding furnace for welding. After welding, an ultrasonic cleaning is performed;
[0035] Injection molding, packaging, and rib cutting process: the cleaned workpiece will pass the IPQC process inspection, and the packaging process will focus on controlling the waking time of the injection molding glue. Injection molding and packaging are carried out according to normal requirements. After the packaging is completed, it will be placed for 6 hours and the rib cutting process will be arranged;
[0036] 3D visual inspection: all the workpieces completed in S3 above are inspected on 6 sides according to the appearance requirements to ensure the integrity of the workpieces and the absence of obvious cracks or other appearance defects;
[0037] The method for checking the density of diode plastic packaging and controlling the process of the present technical solution includes the following steps:
[0038] S1. Helium detection: The product workpieces that have completed the above steps are sampled according to the AQL strict sampling method. According to the size of the product workpiece, they are placed in the corresponding container of the corresponding helium leak detector. The mass spectrometer leak detector is sufficient to read a leak less than or equal to 10 -4 (Pa.m 3 ) / s helium detection rate, the number of samples per unit container is controlled to be n;
[0039] Specific tests include the following:
[0040] S11, placing the product workpiece into the cavity of the pressurized container and closing the cavity;
[0041] S12, evacuate the chamber to below 0.1 mbar, and then fill it with 5-6 bar of helium with a helium concentration of 99%;
[0042] S13, maintain pressure for 30-60 minutes, and release the pressure in the cavity to normal pressure;
[0043] S14, opening the cavity and taking out the product workpiece;
[0044] S15. Use dry and water-free compressed air to clean the surface of the product with helium; the dry and water-free compressed air uses compressed air with a refrigeration capacity greater than 85PH provided by a compressor;
[0045] S16, placing the product workpiece into the vacuum test chamber, and closing the chamber;
[0046] S17, press the leak test button to start the vacuum test;
[0047] S18. Fill the test chamber with air until it reaches atmospheric pressure, open the test chamber, take out the test product, and use a diffusion-type standard leak detector that has been calibrated by the standard at least once per shift to check the effectiveness of the instrument. The leak rate should be more than 5.0x10- 9 mbarl / s, it is judged as unqualified, and it is qualified if the leakage rate is lower than this.
[0048] S2. Use the dichotomy method to judge unqualified product workpieces, specifically:
[0049] Divide the total number of product workpieces n into two equal parts of n / 2, and perform the process step S1 on the two equal parts to determine the defective conditions of the two equal parts of sample product workpieces; if one or two groups of the sample product workpieces after being divided into two equal parts are unqualified, divide the group of unqualified products into two equal parts again, perform the process step S1 again, and determine the defective conditions of the sample product workpieces after being divided into two equal parts twice; if one or two groups of the sample product workpieces after being divided into two equal parts twice are still unqualified, divide the group of unqualified products into two equal parts again and perform the process step S1 again; if there are still unqualified conditions in the subsequent groups after being divided into two equal parts, continue to divide into two equal parts, and after dividing into two equal parts at least five times, use the step S1 to determine the defective conditions of the sample product workpieces after each division; the complexity of the repetition is the standard for judging efficiency and product quality;
[0050] When n / 2 k , which means that the total number n can be completely judged after k equal parts; among them, when k>4, k=log2 n ; That is, the k value is greater than 4. After the first bisection, the k values of the left and right groups are greater than 3. That is, after more than four bisections, it can be judged that the process flow of the overall product workpiece needs to be readjusted;
[0051] The product workpieces of unqualified components are rejected, and the product workpieces of qualified components are transferred to the next step;
[0052] S3. Through the automatic test line TMTT of SMD diode products, the leakage current and withstand voltage parameters of qualified components are tested and silk-screened for easy packaging.
[0053] After each bisection, the components in the bisection with the same quantity or a difference of one are regarded as bisection components of the same level.
[0054] As in this specific embodiment:
[0055] For example, 200 transient suppression diodes, ESD electrostatic diodes, and Schottky diodes are inspected using the diode plastic package density inspection and process control method of this technical solution. The dichotomy is as follows:
[0056] One-time binary division: For example, 200 transient suppression diodes are divided into two equal parts of 100 diodes each. This specific embodiment is only used for specific explanation. The specific value can be selected as 500-1000. This embodiment adopts the value of 200 only for the sake of calculation. A diffusion-type standard leak detector such as the SFJ-16M+ model is used to detect the leak rate of each group after the one-time binary division. Since the diodes are not up to standard during the plastic sealing process, helium will remain in the corresponding gaps or holes, which will cause unqualified product workpieces to be measured. However, the time cost of measuring one by one is too high, so a binary division method is used for rapid inspection;
[0057] If two groups of 100 samples are divided into two equal groups, the leakage rate of each group is measured using a diffusion type standard leak detector, and the overall leakage rate of each group does not exceed 5.0x10 -9 mbarl / s, the whole is qualified and no secondary binary action is required;
[0058] If the overall leakage rate of any of the two second-class groups does not exceed 5.0x10 -9 mbarl / s, the corresponding group is divided into two equal parts, and each group is divided into two equal parts of 50. The diffusion type standard leak detector is used to measure the leakage rate of each group after the second division. If the overall leakage rate of one group does not exceed 5.0x10 -9 mbarl / s, then this group is qualified and does not need to perform three binary operations; the overall leakage rate of the other group exceeds 5.0x10 -9 mbarl / s, the group is unqualified and needs to be divided three times; if the overall leakage rate of the two groups exceeds 5.0x10 -9 mbarl / s, then both groups need to perform three two-point movements respectively;
[0059] After three times of bisection, each group is divided into two equal parts of 25. Use a diffusion type standard leak detector to measure the leakage rate of each group after three times of bisection. If the overall leakage rate of one group does not exceed 5.0x10 -9 mbarl / s, then this group is qualified and does not need to perform four binary operations; the overall leakage rate of the other group exceeds 5.0x10 -9 mbarl / s, the group is unqualified and needs to be divided four times; if the overall leakage rate of the two groups exceeds 5.0x10 -9 mbarl / s, then both groups need to perform four two-point movements respectively;
[0060] After four bisections, each group is divided into 12 or 13 equal parts. Two halves with a difference of one are considered as halves of the same level. Use a diffusion-type standard leak detector to measure the leak rate of each group after four bisections. If the overall leak rate of one group does not exceed 5.0x10-9 mbarl / s, then this group is qualified and does not need to perform five binary operations; the overall leakage rate of the other group exceeds 5.0x10 -9 mbarl / s, the group is unqualified and needs to be split five times; if the overall leakage rate of both groups exceeds 5.0x10 -9 mbarl / s, then both groups need to perform five two-point movements respectively;
[0061] After five splits, each group is divided into 6 or 6 or 7 equal parts. Two equal parts differ by one and are considered as equal parts of the same level. Use a diffusion type standard leak detector to measure the leak rate of each group after five splits. If the overall leak rate of one group does not exceed 5.0x10 -9 mbarl / s, then this group is qualified; the other group’s overall leakage rate is more than 5.0x10 -9 mbarl / s, the group is unqualified; if the overall leakage rate of both groups exceeds 5.0x10 - 9 mbarl / s, the group is directly regarded as unqualified; at this time, k is 5, which is greater than 4, that is, the k value is greater than 4. After the first bisection, the k values of the left and right groups are greater than 3, that is, after more than four bisections, it can be judged that the process flow of the overall product workpiece needs to be readjusted. That is, after 5 bisections, each group is still unqualified, then the overall process is unqualified and needs to be readjusted.
[0062] This technical solution has the following advantages over the prior art:
[0063] (1) The use of a diffusion-type standard leak detector for inspection can be based on numerical quantitative inspection. Compared with the traditional density inspection that relies on visual inspection of the appearance, ultrasonic inspection that relies on wavelength reflection to form an image, and also relies on picture judgment, it is more intuitive, faster, and more efficient;
[0064] (2) Since the product workpiece is not damaged by the use of pressurized helium filling and a diffusion-type standard leak detector for inspection, the waste of materials during the inspection process is greatly reduced, and there is no need for a high-end scanning electron microscope (SEM), which reduces the cost of purchasing instruments for inspection.
[0065] (3) Higher efficiency: Previously, a scanning electron microscope (SEM) could only detect 50 PCS at a time. However, the mass spectrometer can flexibly design the detection capacity, and can detect 500-1000 PCS or even more at a time. In addition, the steps of the present invention provide real-time quality control of the production process.
[0066] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for checking the density of diode plastic packaging and controlling the process, which is used to optimize the process and use helium mass spectrometry leak detection technology to control the density of the product, specifically, to check the density of the product workpiece after die bonding and wire bonding, welding and cleaning, injection molding and packaging, and 3D visual inspection, and is characterized in that: The steps include: S1. Helium detection: Sample the product workpiece according to the AQL strict sampling method, put it into the corresponding container of the corresponding helium leak detector according to the size of the product workpiece, and use the mass spectrometer leak detector to read less than or equal to 10 -4 (Pa.m 3 ) / s helium detection rate, the number of samples per unit container is controlled to be n; Specific tests include the following: S11, placing the product workpiece into the cavity of the pressurized container and closing the cavity; S12, evacuate the chamber to below 0.1mbar, and then fill it with 5-6bar of helium, with a helium concentration of 99%; S13, maintain pressure for 30-60 minutes, and release the pressure in the cavity to normal pressure; S14, opening the cavity and taking out the product workpiece; S15. Use dry and water-free compressed air to clean the surface of the product with helium; S16, placing the product workpiece into the vacuum test chamber, and closing the chamber; S17, press the leak test button to start the vacuum test; S18. Fill the test chamber with air until it reaches atmospheric pressure, open the test chamber, take out the test product, and use a diffusion-type standard leak detector that has been calibrated by the standard at least once per shift to check the effectiveness of the instrument. The leak rate should be more than 5.0x10 -9 mbarl / s, it is judged as unqualified, and it is qualified if the leakage rate is lower than this. S2. Use the dichotomy method to judge unqualified product workpieces, specifically: Divide the total number of product workpieces n into two equal parts of n / 2, and perform the inspection of the process steps of S1 on the two equal parts to determine the defective conditions of the sample product workpieces in the two equal parts; if one or two groups of the sample product workpieces after being divided into two equal parts are unqualified, divide the group of unqualified products divided into two equal parts again, and perform the process steps of S1 again, and determine the defective conditions of the sample product workpieces after being divided into two equal parts twice; if one or two groups of the sample product workpieces after being divided into two equal parts twice are still unqualified, divide the group of unqualified products divided into two equal parts again and perform the process steps of S1 again; if there are still unqualified conditions in the subsequent groups after being divided into two equal parts, continue to divide into two equal parts, and after at least five times of dividing into two equal parts, use the steps of S1 to determine the defective conditions of the sample product workpieces after each division into two equal parts; the complexity of the repetition is the standard for judging efficiency and product quality; When n / 2 k , which means that the total number n can be completely judged after k times of bisection; among them, when k>4, k=log2 n ; That is, the k value is greater than 4. After the first bisection, the k values of the left and right groups are greater than 3. That is, after more than four bisections, it can be judged that the process flow of the overall product workpiece needs to be readjusted; The product workpieces of unqualified components are rejected, and the product workpieces of qualified components are transferred to the next step; S3. Through the automatic test line TMTT of SMD diode products, the leakage current and withstand voltage parameters of qualified components are tested and silk-screened for easy packaging.
2. A method for checking the plastic package compactness of a diode and controlling the process according to claim 1, characterized in that: The dry water-free compressed air adopts compressed air with a refrigeration capacity greater than 85PH provided by a compressor.
3. The method for checking the plastic package compactness and controlling the process of a diode according to claim 1, characterized in that: After each bisection, components with the same number or a difference of one in the bisection are regarded as bisection components of the same level.