Method for manufacturing germanium laser and germanium laser

By using hydrogen ion implantation and bonding processes in silicon-based monolithic integrated lasers to transfer germanium material to the SOI substrate, the crystal quality problem caused by low thermal conductivity during the germanium epitaxial growth process is solved, and the performance and performance of the laser are improved. Yield.

CN118336506BActive Publication Date: 2024-10-18SUZHOU WATECH ELECTRONICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410743073.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-18
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

In silicon-based monolithic integrated lasers, epitaxial growth of germanium causes uneven heat distribution due to the low thermal conductivity of the SOI substrate, affecting crystal quality and laser yield.

Method used

By forming the first silicon germanium layer, the germanium layer and the second silicon germanium layer on the donor original chip, injecting hydrogen ions, and using the bonding process to transfer them to the acceptor original chip, a germanium laser is formed, which avoids high temperature treatment and improves the Crystal quality.

Benefits of technology

It improves the crystal quality and yield of germanium lasers, reduces process difficulty, improves production efficiency, and makes the original chip easier to split and peel through stress differences.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118336506B_ABST
    Figure CN118336506B_ABST
Patent Text Reader

Abstract

The embodiment of the present application provides a method for manufacturing a germanium laser and a germanium laser, wherein the manufacturing method includes: forming a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer on the surface of a donor original sheet in sequence; injecting hydrogen ions above the donor original sheet; forming an oxide layer on the surface of an acceptor original sheet; placing the donor original sheet upside down on the acceptor original sheet, so that the silicon layer in the donor original sheet contacts the oxide layer in the acceptor original sheet, and bonding them using a bonding process; splitting the bonded donor original sheet and the acceptor original sheet so that the germanium layer, the second silicon germanium layer and the silicon layer in the donor original sheet remain on the acceptor original sheet; forming a laser in the germanium layer on the acceptor original sheet; forming an optical waveguide on the surface of the silicon layer on the acceptor original sheet; coupling the optical waveguide with the laser. The method for manufacturing a germanium laser and the germanium laser provided in the embodiment of the present application can improve the problem of low crystal quality caused by poor thermal conductivity of silicon dioxide in traditional solutions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an optical device manufacturing process, and in particular to a manufacturing method of a germanium laser and a germanium laser. Background Art

[0002] The invention of the transistor was a landmark event in the 20th century, pushing the development of human civilization to an unprecedented level. Microelectronic devices based on silicon materials have gradually achieved advantages such as low power consumption, low cost, and easy integration in the past few decades of development, quickly occupying most of the electronics market and becoming the cornerstone of the information revolution. However, the further reduction in the size of microelectronic devices has highlighted problems such as the channel effect of silicon materials. At the same time, metal interconnection delays and increased energy consumption are also the main reasons hindering the rapid development of very large integrated circuits.

[0003] Compared with electrons, photons have many advantages as information carriers: no interference between photons, zero rest mass of photons, and multi-channel compatibility. Due to the unique properties of photons, micro-photonic devices will have greater bandwidth and higher speed than microelectronic devices. And because the current mature integrated circuit technology is based on the silicon process platform, the limited solutions for optoelectronic integration are based on mature silicon integration technology.

[0004] When forming a complete silicon photonic chip, various passive optical devices and active optical devices need to be integrated on a unified silicon substrate. At present, there is still no integrated solution for the light source, one of the most basic devices for silicon photonic integration. Several possible solutions include external light sources and hybrid integrated on-chip light sources, erbium-doped silicon monolithic integration, integration of silicon germanium lasers, and III-V laser bonding integration and direct silicon growth.

[0005] Among them, silicon germanium lasers use heavy doping and material strain to modulate the energy band of germanium, causing it to emit light through direct bandgap electron transitions, and are compatible with CMOS processes, making them a promising technology. Specifically, silicon-based monolithic integrated lasers require epitaxial growth of direct bandgap materials such as germanium and III-V on silicon or insulators. Due to the differences in material systems and material heights, it is extremely challenging to achieve efficient optical field coupling between lasers and silicon photonic chips, which is one of the important challenges currently facing the practical application of silicon-based monolithic integrated lasers.

[0006] Growing germanium on silicon usually requires quite high temperatures because germanium has a high melting point. Generally speaking, to grow germanium on silicon, the silicon substrate needs to be heated to above about 700 degrees Celsius so that the germanium can be deposited on the silicon and form a thin film. This process is usually carried out in a special vapor deposition reaction chamber, and the deposition and growth of germanium is achieved by controlling the composition and temperature of the reaction gas.

[0007] In addition, SOI (Silicon-On-Insulator) is a semiconductor device manufacturing technology that introduces an insulating layer (usually silicon dioxide) on the silicon chip to isolate the crystalline silicon layer from the substrate. This technology has a wide range of applications in silicon optics, covering multiple fields such as waveguide devices, optical modulators, integrated optoelectronics, and photonic crystal devices, providing an important platform for the manufacture and integration of optical devices. There is an insulating layer of silicon dioxide in the middle of SOI, and its thermal conductivity is usually 1.3-1.4 W / (m·K), which is much smaller than the thermal conductivity of silicon, 100 - 150 W / (m·K). The poor thermal conductivity of the SOI substrate will lead to uneven heat distribution, resulting in uneven growth of the epitaxial layer, affecting the crystal quality of epitaxial germanium growth, and causing crystal defects. Summary of the invention

[0008] In order to solve one of the above technical defects, a method for manufacturing a germanium laser and a germanium laser are provided in an embodiment of the present application.

[0009] According to a first aspect of an embodiment of the present application, a method for manufacturing a germanium laser is provided.

[0010] Forming a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer in sequence on the surface of the donor original wafer;

[0011] Implanting hydrogen ions on top of the donor sheet;

[0012] Forming an oxide layer on the surface of the acceptor original wafer;

[0013] The donor original sheet is placed upside down on the acceptor original sheet, so that the silicon layer in the donor original sheet contacts the oxide layer in the acceptor original sheet, and a bonding process is used to perform bonding;

[0014] The bonded donor wafer and acceptor wafer are subjected to a splitting process, so that the first silicon germanium layer and the germanium layer in the donor wafer are separated, and the germanium layer, the second silicon germanium layer and the silicon layer in the donor wafer remain on the acceptor wafer;

[0015] A laser is formed in a germanium layer on an acceptor substrate;

[0016] An optical waveguide is formed on the surface of the silicon layer on the acceptor substrate;

[0017] Couple the optical waveguide to the laser.

[0018] According to a second aspect of an embodiment of the present application, a germanium laser is provided, comprising:

[0019] substrate;

[0020] an oxide layer located above the substrate;

[0021] The silicon layer, the second silicon germanium layer and the germanium layer are sequentially located on the oxide layer from bottom to top; the first silicon germanium layer, the germanium layer, the second silicon germanium layer and the silicon layer are sequentially formed on the substrate of the donor original wafer and formed on the oxide layer through a bonding process, and then the silicon layer, the second silicon germanium layer and the germanium layer are left on the oxide layer through a splitting process; a laser is formed in the germanium layer;

[0022] The optical waveguide is formed on the surface of the silicon layer and is spaced apart from the side surfaces of the second silicon germanium layer and the germanium layer.

[0023] The technical solution provided by the embodiment of the present application sequentially forms a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer on the surface of a donor wafer; injects hydrogen ions above the donor wafer; forms an oxide layer on the surface of an acceptor wafer; turns the donor wafer upside down on the acceptor wafer so that the silicon layer in the donor wafer contacts the oxide layer in the acceptor wafer, and performs a bonding process on them; performs a splitting process on the bonded donor wafer and the acceptor wafer so that the first silicon germanium layer in the donor wafer is separated from the germanium layer, and the germanium layer, the second silicon germanium layer and the silicon layer in the donor wafer remain on the acceptor wafer; forms a laser in the germanium layer on the acceptor wafer; forms an optical waveguide on the surface of the silicon layer on the acceptor wafer; and couples the optical waveguide with the laser. This solution embeds the SOI process into the process of germanium epitaxial growth, forms germanium on the donor wafer, and then transfers the germanium material to the acceptor wafer by hydrogen injection, bonding, and splitting. This process does not require applying a high temperature of more than 600°C to the acceptor wafer, thus improving the problem of low crystal quality caused by poor thermal conductivity of silicon dioxide in traditional solutions. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0025] Figure 1 A flow chart of a method for manufacturing a germanium laser provided in an embodiment of the present application;

[0026] Figure 2 A schematic diagram of the structure of forming a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer on a donor substrate in the method for manufacturing a germanium laser provided in an embodiment of the present application;

[0027] Figure 3 A schematic diagram of the structure of injecting hydrogen ions onto a donor wafer in the germanium laser manufacturing method provided in an embodiment of the present application;

[0028] Figure 4 A schematic diagram of a structure in which an oxide layer is formed on the surface of an acceptor substrate in a method for manufacturing a germanium laser provided in an embodiment of the present application;

[0029] Figure 5 A schematic diagram of the structure of bonding the donor wafer and the acceptor wafer in the method for manufacturing a germanium laser provided in an embodiment of the present application;

[0030] Figure 6 A schematic diagram of the structure of splitting the donor wafer and the acceptor wafer in the method for manufacturing a germanium laser provided in an embodiment of the present application;

[0031] Figure 7 A schematic diagram of the structure of forming a mask plate on the surface of an acceptor wafer in the method for manufacturing a germanium laser provided in an embodiment of the present application;

[0032] Figure 8 A schematic diagram of a structure for defining and forming a laser region to be formed in the germanium laser manufacturing method provided in an embodiment of the present application;

[0033] Fig. 9 A schematic diagram of the structure of forming an optical waveguide material layer on the surface of the silicon layer of the acceptor substrate in the germanium laser manufacturing method provided in an embodiment of the present application;

[0034] Fig.10 A schematic diagram of the structure of forming an optical waveguide in the method for manufacturing a germanium laser provided in an embodiment of the present application.

[0035] Reference numerals:

[0036] 11-donor substrate; 12-first silicon germanium layer; 13-germanium layer; 14-second silicon germanium layer; 15-silicon layer;

[0037] 21-substrate of the acceptor original sheet; 22-oxide layer; 23-optical waveguide;

[0038] 31- Photoresist. DETAILED DESCRIPTION

[0039] In order to make the technical solutions and advantages in the embodiments of the present application more clearly understood, the exemplary embodiments of the present application are further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than an exhaustive list of all the embodiments. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.

[0040] This embodiment provides a method for manufacturing a germanium laser, which can improve the problem of low crystal quality caused by poor thermal conductivity of silicon dioxide in traditional solutions.

[0041] like Figure 1 As shown, the manufacturing method of the germanium laser provided in this embodiment includes:

[0042] Step 101: forming a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer in sequence on the surface of a donor original wafer.

[0043] A wafer is selected as a donor wafer for providing germanium material. The donor wafer can be a silicon substrate, a silicon carbide substrate, or other semiconductor material substrates. This embodiment is described by taking a silicon substrate as an example.

[0044] like Figure 2 As shown, a first silicon germanium layer 12 is first formed on the surface of the substrate 11 of the donor original sheet, and then a germanium layer 13 is formed on the surface of the first silicon germanium layer 12 , and then a second silicon germanium layer 14 is formed on the surface of the germanium layer 13 , and finally a silicon layer 15 is formed on the surface of the second silicon germanium layer 14 .

[0045] The process of forming the first silicon germanium layer 12, the germanium layer 13, the second silicon germanium layer 14 and the silicon layer 15 can adopt a conventional solution, heating the silicon substrate above 600°C and introducing corresponding gases into the vapor deposition reaction formula to form each layer.

[0046] Step 102: inject hydrogen ions onto the donor substrate.

[0047] like Figure 3 As shown, after step 101, hydrogen gas is introduced to inject hydrogen ions above the donor original sheet.

[0048] Step 103: forming an oxide layer on the surface of the acceptor wafer.

[0049] A wafer is selected as an acceptor substrate, and the acceptor substrate will be manufactured into a germanium laser. The acceptor substrate can be a silicon substrate, a silicon carbide substrate, or a substrate of other semiconductor materials. This embodiment is described by taking a silicon substrate as an example.

[0050] like Figure 4 As shown, an oxide layer 22 is formed on the surface of the substrate 21 of the acceptor substrate by furnace tube oxidation or LPCVD. The oxide layer 22 may be a silicon dioxide layer.

[0051] The thickness of the oxide layer 22 can be set according to the product requirements of the germanium laser. In this embodiment, the thickness of the oxide layer 22 is 0.1 μm-1 μm.

[0052] Step 104: Place the donor original sheet upside down on the acceptor original sheet, so that the silicon layer in the donor original sheet contacts the oxide layer in the acceptor original sheet, and perform bonding processing using a bonding process.

[0053] After the above steps 101 to 103 are completed, Figure 5 As shown, the donor wafer is inverted on the acceptor wafer, so that the silicon layer 15 in the donor wafer contacts the oxide layer 22 in the acceptor wafer, and a bonding process is used to perform bonding, specifically, the donor wafer and the acceptor wafer are bonded by a bonding machine.

[0054] Furthermore, before bonding, the surface of the silicon layer 15 of the donor wafer and the surface of the oxide layer 22 of the acceptor wafer are respectively ground to control the surface roughness to less than 1 nm.

[0055] Step 105 , performing a splitting process on the bonded donor wafer and the acceptor wafer to separate the first silicon germanium layer from the germanium layer in the donor wafer, and the germanium layer, the second silicon germanium layer and the silicon layer in the donor wafer remain on the acceptor wafer.

[0056] After the bonding is completed, the bonded donor and acceptor original sheets are split.

[0057] One implementation method is: placing the bonded donor original sheet and acceptor original sheet in an environment of 400°C-600°C, and based on the influence of hydrogen injection and material stress, the donor original sheet and the acceptor original sheet are separated to complete the splitting.

[0058] In this embodiment, the energy of hydrogen ion implantation in step 102 is set to 10kev~100kev, and the hydrogen ion concentration is set to 1E16~1E17, so that the first silicon germanium layer 12 and the germanium layer 13 in the donor original sheet are separated, and the germanium layer 13, the second silicon germanium layer 14 and the silicon layer 15 in the donor original sheet remain on the acceptor original sheet, such as Figure 6 shown.

[0059] Step 106: forming a laser in the germanium layer on the acceptor substrate.

[0060] This embodiment provides an implementation method: a mask is used to define the second silicon germanium layer 14 and the germanium layer 13 to define a region where a laser is to be formed, and the remaining portions of the second silicon germanium layer 14 and the germanium layer 13 are removed.

[0061] For example, first, a photoresist 31 is coated on the surface of the germanium layer 13, and then a mask with a preset pattern is used to cure the photoresist 31 by ultraviolet light, and then the second silicon germanium layer 14 and the germanium layer 13 are partially removed, and the remaining portion is the area where the laser is to be formed, such as Figure 7 and Figure 8 shown.

[0062] Alternatively, a hard mask plate may be used to directly dry etch to remove portions of the second silicon germanium layer 14 and the germanium layer 13 .

[0063] Afterwards, ion implantation technology or other doping technology is used to implant dopants into the germanium layer 13 of the acceptor substrate to form an n-type region and a p-type region, respectively, thereby forming a pn junction of the light-emitting device.

[0064] A metal electrode is formed on the surface of the pn junction of the acceptor substrate using metal deposition technology to provide an electric field and current injection.

[0065] Step 107: forming an optical waveguide on the surface of the silicon layer on the acceptor substrate.

[0066] The optical waveguide may be formed using a silicon waveguide process or a silicon nitride process.

[0067] One implementation method is: Fig. 9 As shown, an optical waveguide material layer is formed on the surface of the silicon layer 15 of the acceptor substrate by using epitaxy or deposition technology. Specifically, after step 106, the optical waveguide material is coated on the surface of the silicon layer 15 not covered by the first silicon germanium layer 12 and the germanium layer 13.

[0068] Then, the structure shape of the optical waveguide is defined by photolithography and etching processes, for example, a mask is used to define the optical waveguide with the optical waveguide material layer.

[0069] Specifically, after coating the optical waveguide material, a photoresist 31 is coated on the surface of the acceptor original wafer, and after curing by ultraviolet light using a mask plate with a preset pattern, a portion of the optical waveguide material is removed by an etching process, and the remaining portion is used as the optical waveguide 23, such as Fig.10 The preset pattern can also be transferred to the photoresist by electron beam exposure.

[0070] Afterwards, dopants are injected into the optical waveguide 23 to adjust the refractive index of the optical waveguide 23 and change its optical properties.

[0071] The optical waveguide 23 is then subjected to surface treatment, such as planarization and removal of residual photoresist, to improve the surface quality and performance of the optical waveguide 23 .

[0072] The optical waveguide 23 is subjected to optical performance tests, such as transmission loss, mode distribution, etc., to verify the accuracy of the design and the compliance of the performance.

[0073] Step 108: Couple the optical waveguide to the laser.

[0074] The output light of the laser is coupled into the optical waveguide 23 through the grating structure.

[0075] Furthermore, the end face of the optical waveguide can be processed by chemical mechanical polishing technology to improve the optical coupling efficiency.

[0076] After the various parts are formed, a metal layer is deposited on the surface of the germanium laser to connect the electrodes and optical waveguides and provide circuit connections.

[0077] The technical solution provided in this embodiment sequentially forms a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer on the surface of a donor wafer; injects hydrogen ions above the donor wafer; forms an oxide layer on the surface of an acceptor wafer; turns the donor wafer upside down on the acceptor wafer so that the silicon layer in the donor wafer contacts the oxide layer in the acceptor wafer, and performs a bonding process on them; performs a splitting process on the bonded donor wafer and the acceptor wafer so that the first silicon germanium layer in the donor wafer is separated from the germanium layer, and the germanium layer, the second silicon germanium layer and the silicon layer in the donor wafer remain on the acceptor wafer; forms a laser in the germanium layer on the acceptor wafer; forms an optical waveguide on the surface of the silicon layer on the acceptor wafer; and couples the optical waveguide with the laser. This solution embeds the SOI process into the process of germanium epitaxial growth, forms germanium on the donor wafer, and then transfers the germanium material to the acceptor wafer by hydrogen injection, bonding, and splitting. This process does not require applying a high temperature of more than 600°C to the acceptor wafer, thus improving the problem of low crystal quality caused by poor thermal conductivity of silicon dioxide in traditional solutions.

[0078] In addition, the solution provided in this embodiment can significantly improve the quality and performance of the device, thereby improving the yield rate, and utilizes the stress difference between germanium and silicon germanium to make the original wafer easier to split and peel, which is beneficial to reducing the process difficulty and improving production efficiency.

[0079] In the above scheme, the first silicon germanium layer 12 is formed on the surface of the donor original wafer. Specifically, the donor original wafer can be placed in an environment with a temperature of 600°C-1200°C and a pressure of 10Pa-10000Pa, and then a gas, such as at least one of SiCl4, SiH4, SiH2(CH3)2, at least one of GeCl4, GeH4, GeH2(CH3)2, and at least one of H2, Ar, PH3, B2H6, is introduced for a preset time to form the first silicon germanium layer 12 on the surface of the donor original wafer. The preset time can be 1min-60min.

[0080] The second silicon germanium layer 14 may be formed in the same manner as the first silicon germanium layer 12 .

[0081] The germanium layer 13 is formed on the surface of the donor original sheet. Specifically, the donor original sheet with the first silicon germanium layer 12 formed thereon can be placed in an environment with a temperature of 600°C-1200°C and a pressure of 10Pa-10000Pa; a gas, such as at least one of GeCl4, GeH4, GeH2(CH3)2, and at least one of H2, Ar, PH3, and B2H6, is introduced for a preset time to form the germanium layer 13 on the surface of the donor original sheet. The duration can be 1min-360min.

[0082] The silicon layer 15 is formed on the donor wafer. Specifically, the donor wafer with the second silicon germanium layer 14 formed thereon is placed in an environment with a temperature of 600°C-1200°C and a pressure of 10Pa-10000Pa; a gas, such as at least one of SiCl4, SiH4, SiH2(CH3)2, and at least one of H2, Ar, PH3, and B2H6, is introduced therein for a preset time to form the silicon layer 15 on the surface of the donor wafer. The preset time may be 1min-360min.

[0083] Based on the above solution, this embodiment also provides a germanium laser, which is manufactured by any of the methods provided in the above content. The germanium laser has the same technical effect as the above manufacturing method.

[0084] Specifically, Fig.10 As shown, the germanium laser provided in this embodiment includes: a substrate (specifically, a substrate 21 of an acceptor substrate), an oxide layer 22 located on the substrate 21 of the acceptor substrate. From bottom to top, a silicon layer 15, a second silicon germanium layer 14, and a germanium layer 13 are sequentially located on the oxide layer 22, wherein the first silicon germanium layer 12, the germanium layer 13, the second silicon germanium layer 14, and the silicon layer 15 are sequentially formed on the substrate 11 of the donor substrate, and formed on the oxide layer 22 through a bonding process, and then the silicon layer 15, the second silicon germanium layer 14, and the germanium layer 13 are left on the oxide layer 22 through a splitting process.

[0085] A laser is formed in the germanium layer 13. An optical waveguide 23 is formed on the surface of the silicon layer 15 and is spaced apart from the side surfaces of the second silicon germanium layer 14 and the germanium layer 13. The specific scheme of the germanium laser can refer to the above content. The germanium laser provided in this embodiment has the same technical effect as the above manufacturing method.

[0086] Furthermore, hydrogen ions are implanted into the first silicon germanium layer 12, the germanium layer 13, the second silicon germanium layer 14 and the silicon layer 15 formed on the substrate 11 of the donor original wafer, and then they are formed on the oxide layer 22 by a flip-chip bonding process.

[0087] One implementation method is: for a donor original sheet, a first silicon germanium layer 12 , a germanium layer 13 , a second silicon germanium layer 14 and a silicon layer 15 are sequentially formed from bottom to top on a substrate 11 of the donor original sheet, and then hydrogen ions are implanted on the silicon layer 15 .

[0088] For the acceptor substrate, an oxide layer 22 is formed on the substrate 21 of the acceptor substrate.

[0089] The donor wafer is then flipped and bonded to the acceptor wafer, and the germanium layer 13 is separated from the first silicon germanium layer 12 by splitting, so that the germanium layer 13, the second silicon germanium layer 14 and the silicon layer 15 remain on the acceptor wafer.

[0090] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0091] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0092] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0093] Although the preferred embodiments of the present application have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications falling within the scope of the present application.

[0094] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A method for manufacturing a germanium laser, characterized in that: include: Forming a first silicon germanium layer, a germanium layer, a second silicon germanium layer and a silicon layer in sequence on the surface of the donor original wafer; Implanting hydrogen ions on top of the donor sheet; The energy of injected hydrogen ions is 10kev~100kev, and the concentration of hydrogen ions is 1E16~1E17; Forming an oxide layer on the surface of the acceptor original wafer; The donor original sheet is placed upside down on the acceptor original sheet, so that the silicon layer in the donor original sheet contacts the oxide layer in the acceptor original sheet, and a bonding process is used to perform bonding; The bonded donor wafer and acceptor wafer are subjected to a splitting process, so that the first silicon germanium layer and the germanium layer in the donor wafer are separated, and the germanium layer, the second silicon germanium layer and the silicon layer in the donor wafer remain on the acceptor wafer; A laser is formed in a germanium layer on an acceptor substrate; An optical waveguide is formed on the surface of the silicon layer on the acceptor substrate; Couple the optical waveguide to the laser.

2. The method according to claim 1, characterized in that The laser is formed in the germanium layer on the acceptor substrate, including: Dopants are injected into the germanium layer of the acceptor substrate to form n-type and p-type regions, respectively, to form a pn junction; A metal electrode is formed on the surface of the pn junction of the acceptor element.

3. The method according to claim 2, characterized in that Before implanting dopants into the germanium layer of the acceptor substrate, the method further includes: The second silicon germanium layer and the germanium layer are used to define a region where a laser is to be formed by using a mask plate, and the remaining portions of the second silicon germanium layer and the germanium layer are removed.

4. The method according to claim 3, characterized in that An optical waveguide is formed on the surface of the silicon layer on the acceptor substrate, including: forming an optical waveguide material layer on the surface of the silicon layer on the acceptor substrate; The optical waveguide material layer is defined into an optical waveguide using a mask.

5. The method according to claim 4, characterized in that After the optical waveguide is formed on the silicon layer surface of the acceptor original wafer, the method further includes: injecting dopants into the optical waveguide; Flattening the optical waveguide; Perform optical performance tests on optical waveguides.

6. The method according to claim 1, characterized in that Before bonding the donor original sheet and the acceptor original sheet, the method further includes: grinding the silicon layer surface of the donor original sheet and the oxide layer surface of the acceptor original sheet respectively.

7. The method according to claim 1, characterized in that Forming a first silicon germanium layer on the surface of the donor original wafer, comprising: Place the donor original sheet in an environment of 600℃-1200℃; At least one of SiCl4, SiH4, SiH2(CH3)2, at least one of GeCl4, GeH4, GeH2(CH3)2, and at least one of H2, Ar, PH3, B2H6 are introduced for a preset time to form a first silicon germanium layer on the surface of the donor original film.

8. The method according to claim 1, characterized in that A germanium layer is formed on the surface of the donor substrate, including: Placing the donor wafer having the first silicon germanium layer formed thereon in an environment of 600° C. to 1200° C.; At least one of GeCl4, GeH4, GeH2(CH3)2 and at least one of H2, Ar, PH3, B2H6 are introduced for a preset time to form a germanium layer on the surface of the donor original sheet.

9. A germanium laser, characterized in that: include: substrate; an oxide layer located above the substrate; A silicon layer, a second silicon germanium layer and a germanium layer are sequentially located on the oxide layer from bottom to top; The first silicon germanium layer, the germanium layer, the second silicon germanium layer and the silicon layer are sequentially formed on the substrate of the donor original wafer, and formed on the oxide layer through a bonding process, and then the silicon layer, the second silicon germanium layer and the germanium layer are left on the oxide layer through a splitting process; a laser is formed in the germanium layer; The optical waveguide is formed on the surface of the silicon layer and is spaced apart from the side surfaces of the second silicon germanium layer and the germanium layer.

10. The germanium laser according to claim 9, characterized in that: Hydrogen ions are implanted into the first silicon germanium layer, the germanium layer, the second silicon germanium layer and the silicon layer formed on the substrate of the donor original sheet, and then formed on the oxide layer through a bonding process.

Citation Information

Patent Citations

  • Micro-cavity semiconductor laser on photon cascade GaAs-OI substrate and preparation method

    CN114300938A

  • Preparation method of substrate with germanium-on-insulator silicon structure