A modified molecular sieve and preparation method thereof
Through the combination and specific treatment of modified zeolite molecular sieve and tetraim (1-imidazole) borate molecular sieve, the efficiency and stability of adsorption of carbon dioxide are improved, and the problems of insufficient carbon dioxide adsorption performance and escape in the prior art are solved, and are particularly suitable for High carbon dioxide removal scenario.
Patent Information
- Application Number
- CN202410506907.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-25
AI Technical Summary
The existing adsorption carbon dioxide molecular sieve has shortcomings in efficient adsorption and stability, especially the problem of carbon dioxide escape under high temperature and high pressure conditions is more prominent, and the adsorption performance needs to be further improved in scenarios where gas composition is high.
Using a combination of modified zeolite molecular sieve and tetra-(1-imidazole) borate molecular sieve, the pore volume and specific surface area are improved by immersion and erosion treatment, and modified molecular sieve with high adsorption properties are prepared through specific steps and conditions, including Soaked in inorganic alkali solution, ammonia erosion and amino acid solution to form modified zeolite molecular sieves supported by amino acids, and prepare tetra(1-imidazole) potassium borate molecular sieve through potassium iodide reaction to form a multi-layer structure to improve adsorption capacity.
The high-efficiency adsorption and stability of carbon dioxide are achieved, with good adsorption amounts not less than 7 mmol/g, and the stability is better during the circulating adsorption and desorption process. It is especially suitable for high carbon dioxide removal scenarios. When the gas composition requirements are high, Significantly improves the adsorption effect.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieve modification, and specifically relates to a modified molecular sieve and a preparation method thereof. Background Art
[0002] Molecular sieves are crystalline inorganic compounds composed of silicon, aluminum, oxygen and other elements, with regularly arranged pore systems and abundant active sites. According to the classification of the International Union of Pure and Applied Chemistry (IUPAC), molecular sieves can be divided into many types, such as A-type, X-type, Y-type, ZSM series, MFI series, etc., as well as emerging metal organic frameworks (MOFs).
[0003] Molecular sieves that adsorb carbon dioxide are porous materials designed specifically to capture and separate carbon dioxide (CO2) from the atmosphere or industrial emissions. With their unique pore structure, high specific surface area and excellent gas adsorption selectivity, these materials have shown great application potential in addressing global climate change, achieving carbon capture and storage (CCS) and industrial waste gas treatment.
[0004] Factors that affect adsorption performance are:
[0005] 1. Molecular sieve characteristics: Factors such as pore size and distribution, specific surface area, acid site density, and framework stability directly affect the adsorption capacity and selectivity of CO2.
[0006] 2. Operating conditions: Operating conditions such as temperature, pressure, gas composition (such as CO2 concentration, presence of other competing gases) and adsorption / desorption rate have a significant impact on adsorption performance. Generally speaking, low temperature and high pressure are conducive to increasing CO2 adsorption, but the actual process conditions and energy consumption must be taken into account.
[0007] 3. Adsorption kinetics and thermodynamics: By measuring parameters such as adsorption isotherms, adsorption rates, adsorption heats, and equilibrium constants, we can gain an in-depth understanding of the kinetic behavior and thermodynamic properties of the adsorption process, and guide the optimal design of molecular sieves.
[0008] There are various methods for preparing molecular sieves for adsorbing carbon dioxide, aiming to produce materials with suitable pore size, high specific surface area and good adsorption performance. The main methods are as follows:
[0009] 1. Hydrothermal synthesis
[0010] Hydrothermal synthesis is the most commonly used method for preparing traditional aluminosilicate molecular sieves. The process mainly includes the following steps:
[0011] Raw material preparation: Prepare silicon source (such as silica sol, sodium silicate, silicate, etc.), aluminum source (such as sodium aluminate, aluminum salt, etc.), structure directing agent (such as quaternary ammonium salt, organic amine, etc.), alkali source (such as sodium hydroxide, potassium hydroxide, etc.) and deionized water, and mix them into gel in a certain proportion.
[0012] Hydrothermal reaction: The gel is transferred to a closed autoclave and subjected to hydrothermal crystallization for a long time (several hours to several days) at a set temperature (usually between 100°C and 200°C) and pressure (normal pressure to tens of atmospheres).
[0013] Post-treatment: After crystallization is completed, cool to room temperature, take out the product for washing, drying, calcining, remove the template, and obtain the final molecular sieve powder.
[0014] 2. Dry gel transformation method
[0015] The dry gel conversion method is a simplified hydrothermal synthesis method suitable for the rapid preparation of certain specific types of molecular sieves. This method pre-synthesizes aluminosilicate dry gel and then converts it into the target molecular sieve at a lower temperature:
[0016] Preparation of dry glue: Use raw materials similar to the hydrothermal synthesis method, but quickly solidify into dry glue at a lower temperature.
[0017] Conversion reaction: Mix the dry glue with a structure-directing agent, an alkali source, etc., and carry out conversion crystallization under relatively mild conditions (the temperature is usually lower than that of the hydrothermal method).
[0018] Post-treatment: After the same steps of washing, drying, calcination, etc., the target molecular sieve is obtained.
[0019] 3. Interfacial polycondensation method
[0020] The interfacial polycondensation method is mainly used to prepare metal organic framework (MOFs) molecular sieves:
[0021] Solvothermal synthesis: Dissolve metal salts and organic ligands in an organic solvent, stir and react in a constant temperature, closed environment for a period of time to allow the metal ions and ligands to self-assemble into MOF crystals.
[0022] Centrifugal separation and drying: After the reaction is completed, the precipitate is collected by centrifugal separation and then dried under an inert atmosphere to obtain pure MOF powder.
[0023] Sol-Gel Method
[0024] The sol-gel method is suitable for preparing molecular sieves containing specific functional groups or heteroatom modifications:
[0025] Preparation of precursor solution: Dissolve the silicon source, aluminum source, structure directing agent, and modifier (such as silane, titanate, etc.) in a solvent to form a uniform sol.
[0026] Gelation and drying: After aging, the sol is transformed into gel, and then dried to remove the solvent to form a dry gel with a certain pore structure.
[0027] Heat treatment: The dry gel is subjected to high temperature heat treatment (calcination) to induce chemical reaction and sinter into dense molecular sieve material.
[0028] 5. Template-guided method
[0029] Template-directed methods are used to prepare molecular sieves with specific morphology or structure, such as nanotubes, thin films, porous ceramics, etc.:
[0030] Template preparation and coating: Use organic polymers, inorganic particles, etc. as templates to evenly coat the molecular sieve precursor liquid on the template surface or fill it in the template pores.
[0031] Curing and template removal: The precursor is cured through drying, heat treatment and other steps, and then the template is removed by chemical etching, pyrolysis and other methods to expose the specific structure of the molecular sieve.
[0032] The choice of each preparation method depends on the type of molecular sieve required, performance requirements and application scenarios. In actual operation, it is often necessary to finely control the process parameters (such as temperature, time, pH value, type and amount of template, etc.) to optimize the pore size distribution, specific surface area and adsorption performance of the molecular sieve, making it more suitable for efficient adsorption of carbon dioxide.
[0033] CN112657477 discloses a Ce-doped mesoporous molecular sieve for efficient adsorption of environmental carbon dioxide and a preparation method, comprising the following steps: step 1, preparing a mesoporous molecular sieve containing organic matter; step 2, removing the template agent by multi-stage high-temperature calcination of the mesoporous molecular sieve to form mesopores. It can efficiently and stably eliminate carbon dioxide in the ambient atmosphere, form a mesoporous molecular sieve by using a soft template agent P123, and further improve the stabilizing effect of the molecular sieve pores on the adsorption of carbon dioxide by Ce doping, thereby reducing the escape of carbon dioxide and causing secondary pollution. However, it contains special metal ions. Summary of the invention
[0034] The present invention provides a modified molecular sieve and a preparation method thereof. The prepared molecular sieve has good carbon dioxide absorption effect and is particularly suitable for scenes with high requirements for carbon dioxide removal. The carbon dioxide adsorption capacity is good and is not less than 7 mmol / g.
[0035] A modified molecular sieve comprises the following material compositions in parts by mass:
[0036] 13X molecular sieve 40~50 parts
[0037] Modified zeolite molecular sieve 10~15 parts
[0038] 0-3 parts of tetrakis(1-imidazole)borate molecular sieve.
[0039] Furthermore, the tetrakis(1-imidazole)borate is sodium tetrakis(1-imidazole)borate or potassium tetrakis(1-imidazole)borate. Sodium tetrakis(1-imidazole)borate or potassium tetrakis(1-imidazole)borate both have good adsorption performance for carbon dioxide, but potassium tetrakis(1-imidazole)borate molecular sieve has better adsorption performance for carbon dioxide and better stability during cyclic adsorption and desorption.
[0040] Furthermore, the preparation of the modified zeolite molecular sieve comprises the following steps:
[0041] S11 Soak the zeolite molecular sieve in an inorganic alkaline solution for 2-4 hours, then filter, wash with water, and dry. Soaking in the alkaline solution can expand the pores of the zeolite molecular sieve, increase the pore volume and specific surface area, and enhance the adsorption effect;
[0042] S12: passing ammonia gas into the molecular sieve obtained in step S11, and corroding the molecular sieve for 1 to 3 hours;
[0043] S13 soaking the eroded molecular sieve in an amino acid solution and then filtering;
[0044] S14: The molecular sieve soaked with amino acids obtained in step S13 is dried in vacuum at a temperature between 55 and 75° C. and activated to obtain a modified zeolite molecular sieve. Amino acids can be loaded on the molecular sieve through step S14 to further enhance its adsorption capacity.
[0045] Furthermore, in step S11, the inorganic alkaline solution is 3-5wt% sodium hydroxide solution, the soaking temperature is 120-150°C, and the pressure is 0.11-0.3Mpa. The soaking at a higher temperature and a certain pressure is better than that at room temperature and normal pressure. However, the soaking time cannot be too long, otherwise it will affect the strength of the zeolite molecular sieve.
[0046] Furthermore, in step S12, the etching temperature is between 150 and 180° C. Through high-temperature ammonia etching, the gas etching can enter the interior of the zeolite molecular sieve, and some ammonia may react with the molecular sieve to dehydrate and form -NH2 groups, thereby improving the adsorption performance of the molecular sieve.
[0047] Furthermore, in the step S13, the amino acid solution is an L-glutamic acid solution or a lysine solution, with a concentration of 3-5wt%, a soaking temperature of 35-45°C, and a soaking time of 3-5h. The amino acid is soaked, dried, and activated, and the amino acid can be loaded in part of the pore volume of the zeolite molecular sieve to enhance the adsorption performance. In particular, when a lysine solution is used, the effect is better because lysine contains two -NH2 groups and has a stronger adsorption effect. At the same time, since the amino acid contains a carboxyl group, the alkaline substances in the gas can be intercepted in the modified molecular sieve, further improving the cleanliness of the gas after adsorption, and expanding the application field of the modified molecular sieve prepared by the present invention.
[0048] Furthermore, the preparation of the potassium tetrakis(1-imidazole)borate molecular sieve comprises the following steps:
[0049] S21: adding sodium tetrakis(1-imidazole)borate to an organic solvent, and then adding potassium iodide to react;
[0050] S22: Cool the reaction solution obtained in step S21 to room temperature, filter, wash, and dry to obtain potassium tetrakis(1-imidazole)borate molecular sieve.
[0051] Furthermore, in step S21, the mass of the organic solvent is 5 times the mass of sodium tetrakis(1-imidazole)borate, the mass of potassium iodide is 0.3 times the mass of sodium tetrakis(1-imidazole)borate, the organic solvent is ethanol, the reaction temperature is 70-80°C, and the reaction time is 24-48h.
[0052] Furthermore, the above-mentioned 13X molecular sieve, modified zeolite molecular sieve, and tetrakis(1-imidazole)borate molecular sieve are stacked from bottom to top to obtain a modified molecular sieve. When the molecular sieve prepared by the present invention adsorbs carbon dioxide in the gas, the gas enters from the bottom of the molecular sieve stacking tower, and passes through the 13X molecular sieve, modified zeolite molecular sieve, and sodium tetrakis(1-imidazole)borate molecular sieve in sequence. For scenes with very high requirements for gas composition, the effect is obvious after using tetrakis(1-imidazole)borate molecular sieve. DETAILED DESCRIPTION
[0053] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1
[0054] A modified molecular sieve comprises the following material compositions in parts by mass:
[0055] 13X molecular sieve 40g
[0056] Modified zeolite molecular sieve 10g
[0057] Potassium tetrakis(1-imidazole)borate molecular sieve 1g.
[0058] The preparation of the modified zeolite molecular sieve comprises the following steps:
[0059] S11 Soak 10.5 g of zeolite molecular sieve in 4 wt% sodium hydroxide solution for 3 h at a temperature of 120-130 °C and a pressure of 0.11-0.2 MPa, then filter, wash with water, and dry;
[0060] S12: passing ammonia gas into the molecular sieve obtained in step S11, and etching for 1-3 hours at a temperature between 150 and 160° C.;
[0061] S13 soaking the corroded molecular sieve in a lysine solution with a concentration of 4 wt% at a temperature of 35-40° C. for 4 h and then filtering;
[0062] S14: The molecular sieve soaked with amino acids obtained in step S13 is dried in vacuum at a temperature between 55° C. and 75° C. to activate the molecular sieve, thereby obtaining a modified zeolite molecular sieve.
[0063] The preparation of the potassium tetrakis(1-imidazole)borate molecular sieve comprises the following steps:
[0064] S21 Add 1 g of sodium tetrakis(1-imidazole)borate to 5 g of ethanol, then add 0.3 g of potassium iodide, and react at a temperature between 70 and 80°C for 36 hours.
[0065] S22: Cool the reaction solution obtained in step S21 to room temperature, filter, wash, and dry to obtain potassium tetrakis(1-imidazole)borate molecular sieve.
[0066] The 13X molecular sieve, modified zeolite molecular sieve and potassium tetraimidazole borate molecular sieve are stacked from bottom to top to obtain a modified molecular sieve. Example 2
[0067] A modified molecular sieve comprises the following material compositions in parts by mass:
[0068] 13X molecular sieve 50g
[0069] Modified zeolite molecular sieve 15g
[0070] 2g of potassium tetrakis(1-imidazole)borate molecular sieve.
[0071] The preparation of the modified zeolite molecular sieve comprises the following steps:
[0072] S11 Soak 15.6 g of zeolite molecular sieve in 4 wt% sodium hydroxide solution for 3 h at a temperature of 130-140 °C and a pressure of 0.15-0.25 MPa, then filter, wash with water, and dry;
[0073] S12: passing ammonia gas into the molecular sieve obtained in step S11, and etching for 1-3 hours at an etching temperature between 160° C. and 170° C.;
[0074] S13 soaking the corroded molecular sieve in a lysine solution with a concentration of 5 wt% at a temperature of 35-40° C. for 4 h and then filtering;
[0075] S14: The molecular sieve soaked with amino acids obtained in step S13 is dried in vacuum at a temperature between 55° C. and 75° C. to activate the molecular sieve, thereby obtaining a modified zeolite molecular sieve.
[0076] The preparation of the potassium tetrakis(1-imidazole)borate molecular sieve comprises the following steps:
[0077] S21 Add 2 g of sodium tetrakis(1-imidazole)borate to 10 g of ethanol, then add 0.6 g of potassium iodide, and react at a temperature between 70 and 80°C for 36 hours.
[0078] S22: Cool the reaction solution obtained in step S21 to room temperature, filter, wash, and dry to obtain potassium tetrakis(1-imidazole)borate molecular sieve.
[0079] The 13X molecular sieve, modified zeolite molecular sieve and potassium tetraimidazole borate molecular sieve are stacked from bottom to top to obtain a modified molecular sieve. Example 3
[0080] A modified molecular sieve comprises the following material compositions in parts by mass:
[0081] 13X molecular sieve 40g
[0082] Modified zeolite molecular sieve 10g
[0083] Sodium tetrakis(1-imidazole)borate molecular sieve 1g.
[0084] The preparation of the modified zeolite molecular sieve comprises the following steps:
[0085] S11 Soak 10.5 g of zeolite molecular sieve in 4 wt% sodium hydroxide solution for 3 h at a temperature of 120-130 °C and a pressure of 0.11-0.2 MPa, then filter, wash with water, and dry;
[0086] S12: passing ammonia gas into the molecular sieve obtained in step S11, and etching for 1-3 hours at a temperature between 150 and 160° C.;
[0087] S13 soaking the corroded molecular sieve in a 4wt% L-glutamic acid solution at a temperature of 35-40°C for 4h and then filtering;
[0088] S14: The molecular sieve soaked with amino acids obtained in step S13 is dried in vacuum at a temperature between 55° C. and 75° C. to activate the molecular sieve, thereby obtaining a modified zeolite molecular sieve.
[0089] The 13X molecular sieve, modified zeolite molecular sieve and sodium tetraimidazole borate molecular sieve are stacked from bottom to top to obtain a modified molecular sieve. Example 4
[0090] A modified molecular sieve comprises the following material compositions in parts by mass:
[0091] 13X molecular sieve 40g
[0092] Modified zeolite molecular sieve 10g.
[0093] The preparation of the modified zeolite molecular sieve comprises the following steps:
[0094] S11 Soak 10.5 g of zeolite molecular sieve in 4 wt% sodium hydroxide solution for 3 h at a temperature of 120-130 °C and a pressure of 0.11-0.2 MPa, then filter, wash with water, and dry;
[0095] S12: passing ammonia gas into the molecular sieve obtained in step S11, and etching for 1-3 hours at a temperature between 150 and 160° C.;
[0096] S13 soaking the corroded molecular sieve in a 4wt% L-glutamic acid solution at a temperature of 35-40°C for 4h and then filtering;
[0097] S14: The molecular sieve soaked with amino acids obtained in step S13 is dried in vacuum at a temperature between 55° C. and 75° C. to activate the molecular sieve, thereby obtaining a modified zeolite molecular sieve.
[0098] The 13X molecular sieve and the modified zeolite molecular sieve are stacked from bottom to top to obtain a modified molecular sieve. Example 5
[0099] The lysine in step S13 of Example 1 was replaced with L-glutamic acid, and the rest was the same as Example 1 and will not be described in detail. Example 6
[0100] The potassium tetrakis(1-imidazole)borate in Example 1 was replaced with sodium tetrakis(1-imidazole)borate, and the rest was the same as Example 1 and will not be described in detail.
[0101] Comparative Example 1
[0102] Step S13 and step S14 in Example 3 are removed, and the rest are the same as Example 3 and will not be described in detail.
[0103] Comparative Example 2
[0104] The step S12 in Example 3 is removed, and the rest is the same as Example 3 and will not be described in detail.
[0105] Comparative Example 3
[0106] The step S11 in Example 3 is removed, and the rest is the same as Example 3 and will not be described in detail.
[0107] The modified molecular sieves prepared in the embodiments and comparative examples were subjected to performance tests. The test method was as follows: at 50°C and 0.12 MPa, a nitrogen / carbon dioxide mixture (carbon dioxide volume fraction of 10%) was passed from bottom to top into the prepared modified molecular sieves of the same mass until the concentration no longer changed. The adsorption amount was measured, and the carbon dioxide content in the mixed gas was measured after 5 min and 10 min of passing. The test results are shown in Table 1.
[0108] Table 1
[0109] Serial number Carbon dioxide adsorption, mmol / g Carbon dioxide volume fraction at 5 minutes, % Carbon dioxide volume fraction at 10 minutes, % Example 1 7.5 0.03 0.05 Example 2 7.8 0.01 0.02 Example 3 7.1 0.04 0.06 Example 4 7.0 0.20 0.31 Example 5 7.2 0.04 0.06 Example 6 7.3 0.04 0.05 Comparative Example 1 6.2 0.35 0.52 Comparative Example 2 6.5 0.28 0.41 Comparative Example 3 5.8 0.43 0.64
[0110] The test data of Examples 1 to 6 show that the modified molecular sieve prepared by the present invention has good carbon dioxide adsorption capacity, and the carbon dioxide volume fraction is low at 5min and 10min; the data of Example 4 show that the carbon dioxide adsorption capacity is slightly reduced in the absence of tetrakis(1-imidazole)borate molecular sieve, but the carbon dioxide volume fraction is significantly increased at 5min and 10min. Therefore, for scenes with high requirements for gas components after adsorption, it is recommended to adopt the technical solution of adding tetrakis(1-imidazole)borate; the data of Examples 1 and 5 show that lysine has a better technical effect; the data of Examples 1 and 6 show that potassium tetrakis(1-imidazole)borate has a better technical effect; the data of Comparative Examples 1, 2, and 3 show that steps S11, S13, and S14 can all improve the performance of the modified molecular sieve finally prepared.
[0111] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A modified molecular sieve, characterized in that: It is composed of the following substances in parts by mass: 13X molecular sieve 40~50 parts Modified zeolite molecular sieve 10~15 parts 3 parts of tetrakis(1-imidazole)borate molecular sieve; The above-mentioned 13X molecular sieve, modified zeolite molecular sieve, and tetrakis(1-imidazole)borate molecular sieve are stacked from bottom to top to obtain a modified molecular sieve; The preparation of the modified zeolite molecular sieve comprises the following steps: S11 Soak the zeolite molecular sieve in an inorganic alkali solution for 2-4 hours, then filter, wash with water, and dry; S12: passing ammonia gas into the molecular sieve obtained in step S11, and corroding the molecular sieve for 1 to 3 hours; S13 soaking the eroded molecular sieve in an amino acid solution and then filtering; S14 vacuum drying and activating the molecular sieve soaked with amino acids obtained in step S13 at a temperature between 55° C. and 75° C. to obtain a modified zeolite molecular sieve; The tetrakis(1-imidazole)borate is sodium tetrakis(1-imidazole)borate or potassium tetrakis(1-imidazole)borate; The preparation of the potassium tetrakis(1-imidazole)borate molecular sieve comprises the following steps: S21: adding sodium tetrakis(1-imidazole)borate to an organic solvent, and then adding potassium iodide to react; S22: cooling the reaction solution obtained in step S21 to room temperature, filtering, washing, and drying to obtain potassium tetrakis(1-imidazole)borate molecular sieve; In step S21, the mass of the organic solvent is 5 times that of sodium tetrakis(1-imidazole)borate, the mass of potassium iodide is 0.3 times that of sodium tetrakis(1-imidazole)borate, the organic solvent is ethanol, the reaction temperature is 70-80°C, and the reaction time is 24-48h.
2. The modified molecular sieve according to claim 1, characterized in that In step S11, the inorganic alkaline solution is 3-5 wt% sodium hydroxide solution, the soaking temperature is 120-150° C., and the pressure is 0.11-0.3 MPa.
3. The modified molecular sieve according to claim 1, characterized in that: The etching temperature in step S12 is between 150 and 180°C.
4. The modified molecular sieve according to claim 1, characterized in that In step S13, the amino acid solution is L-glutamic acid solution or lysine solution, with a concentration of 3-5wt%, a soaking temperature of 35-45°C, and a soaking time of 3-5h.