A method for preparing ZSM-12 molecular sieve without template

Through a two-step hydrothermal synthesis method without template agent, ZSM-12 molecular sieve is synthesized in a polytetrafluoroethylene reactor using silicon source, aluminum source and alkali source, which solves the costly and long crystallization time of template agents in the prior art. The problem is that a low-cost and efficient preparation process and excellent product performance are achieved.

CN118343787BActive Publication Date: 2024-11-19TIANJIN PASSION ADVANCED MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410521797.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-19
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The use of expensive template agents in the existing ZSM-12 molecular sieve synthesis method increases the synthesis cost, and the crystallization time and large grain size affect the synthesis efficiency and product quality.

Method used

Using the template-free preparation method, the gel is formed by stirring silicon source, aluminum source, alkali source and water, and the pre-prepared sol seeds are added. Two-step hydrothermal synthesis is carried out in the polytetrafluoroethylene reactor, avoiding additional The use of add-on template agents simplifies the process and reduces costs.

Benefits of technology

It realizes low-cost and efficient preparation of ZSM-12 molecular sieve, shortens the crystallization time, improves the regularity and crystallinity of the grains, and reduces the synthesis cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118343787B_ABST
    Figure CN118343787B_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method for preparing ZSM-12 molecular sieve without template. The method uses silicon source, aluminum source, alkali and water as raw materials to form an initial gel, and the template-free dynamic crystallization hydrothermal synthesis of ZSM-12 molecular sieve, and the obtained molecular sieve sample is determined to be ZSM-12 molecular sieve by X-ray diffraction. The molecular sieve synthesis method provided by the present invention has a high synthesis yield, does not need to add any expensive template, and synthesizes ZSM-12 molecular sieve by two-step hydrothermal synthesis of sol seed method, the synthesis process is simple and reliable, the production cost is low, and it is easy to implement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalytic technology, and in particular to a method for preparing a ZSM-12 molecular sieve without a template. Background Art

[0002] Zeolite molecular sieves have regular and uniform pore structure, good hydrothermal stability, adjustable acidity, and unique molecular selectivity. As adsorbents, ion exchange materials, and catalysts with excellent performance, they have been widely used in environmental protection, oil refining, petrochemicals, and other fields.

[0003] ZSM-12 molecular sieve was first synthesized in 1973. Its structure type is MTW type, with one-dimensional twelve-membered ring linear non-crossed pores, pore size of 0.57nm*0.61nm, and belongs to high silicon zeolite. The pore size is between that of medium-pore and large-pore molecular sieves. This pore size shows excellent catalytic activity, selectivity and stability in reactions such as catalytic cracking, aromatic alkylation, isomerization, and shape-selective catalytic conversion of organic molecules. It can also be used for methane aromatization, methanol conversion, alkane dehydrogenation to olefins, olefin disproportionation reaction, xylene isomerization, toluene alkylation and other acid-catalyzed reactions, and has a very broad application prospect. Therefore, it is of great practical significance to develop and study the preparation method of ZSM-12 molecular sieve. At present, ZSM-12 has been widely used in reactions such as 2,6-dimethylnaphthalene synthesis, xylene isomerization, and short-chain alkane isomerization.

[0004] Currently, the template for synthesizing ZSM-12 molecular sieves is mainly tetraethylammonium ion (TEA + ), methyltriethylammonium ion (MTEA + ), benzyltrimethylammonium ion (BTMA + ) and other halogenated compounds or hydroxides of tetraalkylammonium ions. Using different templates, ZSM-12 molecular sieves with different crystal forms can be synthesized, with TEA + The ZSM-12 molecular sieve synthesized when MTEA is used as template is mostly cubic, with a grain size of about 400 μm, which belongs to the small grain level. + , BTMA + The molecular sieves synthesized using templates are mostly rice-grain shaped, with a grain size greater than 1 μm.

[0005] So far, the most commonly used method for synthesizing ZSM-12 molecular sieve is hydrothermal crystallization synthesis, which is divided into dynamic method and static method. Generally, dynamic hydrothermal crystallization has the advantages of short crystallization time, high stability and good repeatability compared with static hydrothermal crystallization. The hydrothermal synthesis method is to mix the silicon source, aluminum source and template agent with deionized water in a certain order after metering, vigorously stir them into a gel at an appropriate alkalinity, put them into a polytetrafluoroethylene-lined reactor, and crystallize them at 140-175°C for 4-8 days. After complete crystallization, the solid product is filtered, washed and dried to obtain the ZSM-12 molecular sieve raw powder.

[0006] Patent USP3832448 first reported in 1974 that microporous ZSM-12 was successfully synthesized using methyltriethylammonium bromide as a template. USP3832449 first publicly introduced the synthesis of ZSM-12 molecular sieves using tetramethylammonium or tetraethylammonium as templates. Domestic patent CN103435065A uses tetraethylammonium bromide as a template, first prepares pre-crystallized seeds by a pre-seed method, and then prepares ZSM-12 molecular sieves by adding seeds to a mixed gel. This method can significantly shorten the crystallization time, solve the problems of long crystallization time and large synthesized grain size in existing synthesis methods, and greatly improve the synthesis efficiency. Patent CN108423688A synthesized pure phase ZSM-12 molecular sieves using isopropylamine as a template. Patent CN106022805A uses the template 1,4-bis(N-methylpyrrolidine)butane halide to crystallize the small-grain ZSM-12 molecular sieve, which has high crystallinity, adjustable silicon-aluminum ratio, regular morphology and a grain size of 100-200nm.

[0007] However, the ZSM-12 molecular sieves synthesized by the above-mentioned methods all use relatively expensive template agents, which greatly increases the synthesis cost. Summary of the invention

[0008] The object of the present invention is to provide a method for preparing ZSM-12 molecular sieve without template agent, wherein silicon source, aluminum source, alkali source and water are stirred evenly to form gel, pre-prepared sol seed crystals are added, and then the molecular sieve is hydrothermally synthesized in two steps by dynamic method in a polytetrafluoroethylene-lined reactor. Among them, silicon source, aluminum source, alkali and sol seed crystals are mainly used, and no expensive template agent is required to be added. The synthesis process is simple and reliable, the synthesis cost is low, and it is easy to implement.

[0009] In order to achieve the above object, the present invention provides the following technical solutions:

[0010] The present invention provides a method for preparing ZSM-12 molecular sieve without a template, characterized in that the method comprises the following steps:

[0011] Step 1: preparing pre-crystallized sol seed crystals;

[0012] Step 2: Stir and dissolve the aluminum source, alkali source and deionized water, add the silicon source to the mixed solution, stir for a period of time, add the pre-crystallized sol seed crystals, and continue stirring to form an initial gel;

[0013] Step 3: The initial gel is then placed in a polytetrafluoroethylene reactor for crystallization at two different temperatures. After the crystallization is completed, it is filtered, washed with water, and dried to obtain a ZSM-12 molecular sieve.

[0014] The preparation method of the pre-crystallized sol seed crystal is as follows: sodium hydroxide and aluminum hydroxide are added into water, stirred, and then silica sol is slowly added dropwise, and after the addition is completed, stirring and aging are continued to obtain a mixed gel, and the pre-crystallized sol seed crystal is obtained by hydrothermal crystallization.

[0015] The preparation method of pre-crystallized sol seed crystals is specifically as follows: a. weigh 1 part of silica sol, 0.01-0.005 parts of aluminum hydroxide, 0.3-0.7 parts of sodium hydroxide and 3-8 parts of deionized water by mass fraction; wherein the content of Al2O3 in aluminum hydroxide is 65%, and the content of SiO2 in silica sol is 25%-30%; b. add the sodium hydroxide and aluminum hydroxide weighed in step a to deionized water, stir for 0.5-1h under the stirring condition of 200-300r / min, slowly dropwise add silica sol, and continue stirring and aging for 10h-15h after all the silica sol is dropped to obtain a mixed gel; c. place the mixed gel obtained in step b in a stainless steel reactor with a polytetrafluoroethylene lining, crystallize in an oven at a temperature of 140℃-160℃ for 2-6h, cool to room temperature after crystallization is completed, and take out to obtain pre-crystallized sol seed crystals.

[0016] The specific operation of step 2 is: stirring and dissolving the aluminum source, alkali and deionized water at 100° C., mixing them evenly to form a mixed solution, cooling them down, adding silica gel to the mixed solution at room temperature, continuing to stir to form a gel, and then adding 1wt.% to 40wt.% of the sol seed prepared in step 1, and continuing to stir to form an initial gel.

[0017] In step 2, the molar ratio of the aluminum source to the silicon dioxide is (0.001-1):1, preferably (0.001-0.05):1; the molar ratio of the alkali source to the silicon dioxide is (0.03-0.5):1, preferably (0.04-0.3):1. In addition, the molar ratio of water to silicon dioxide in the solution is (3-20):1, preferably (5-15):1.

[0018] In step 2, the molar ratio of the aluminum source to the silicon dioxide is (0.001-0.05):1; the molar ratio of the alkali source to the silicon dioxide is (0.04-0.3):1. In addition, the molar ratio of water to the silicon dioxide in the solution is (5-15):1.

[0019] In step 2, the alkali source is one or more of potassium hydroxide, sodium hydroxide or ammonia water; the aluminum source is one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, sodium aluminate or aluminum sol; and the silicon source is one or more of silica sol, solid silica gel, ethyl orthosilicate, white carbon black and water glass.

[0020] In step 2, the aluminum source is aluminum hydroxide or sodium aluminate, and the silicon source is silica sol or solid silica gel.

[0021] The amount of pre-crystallized sol seed added is 16 wt.% to 32 wt.%.

[0022] The crystallization in step 3 is carried out at 110° C. for 20 h to 25 h, and then at 160° C. for 20 h to 24 h.

[0023] Compared with the prior art, in the preparation method of the ZSM-12 molecular sieve provided by the present invention, an aluminum source is used as a raw material, and it is stirred and dissolved in an alkaline aqueous solution, and then a silicon source is added and stirred evenly for gelation reaction, and finally a sol seed is added, and then at a certain temperature, time and stirring rate, the gel is crystallized in a polytetrafluoroethylene reactor, and then the crystallized product is filtered, washed and dried to obtain a ZSM-12 type molecular sieve. It can be seen from the process that in the preparation method of the ZSM-12 type molecular sieve provided by the present invention, no expensive template agent is added, and the ZSM-12 type molecular sieve is synthesized by two-step hydrothermal synthesis by adding sol seeds that are easy to prepare, and the synthesis process is simple and reliable, the synthesis cost is low, and it is easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0025] Figure 1 The XRD diagram of the product in Comparative Example 1 of the present invention, wherein the abscissa is the diffraction angle and the ordinate is the absorbance;

[0026] Figure 2 This is a SEM image of the product in Comparative Example 1 of the present invention;

[0027] Figure 3 is the XRD diagram of the product in Example 1 of the present invention, wherein the abscissa is the diffraction angle and the ordinate is the absorbance;

[0028] Figure 4 is a SEM image of the product in Example 1 of the present invention;

[0029] Figure 5 is the XRD diagram of the product in Example 2 of the present invention, wherein the abscissa is the diffraction angle and the ordinate is the absorbance;

[0030] Figure 6 is a SEM image of the product in Example 2 of the present invention;

[0031] Figure 7 is the XRD diagram of the product in Example 3 of the present invention, wherein the abscissa is the diffraction angle and the ordinate is the absorbance;

[0032] Figure 8 is a SEM image of the product in Example 3 of the present invention;

[0033] Fig. 9 is the XRD diagram of the product in Example 4 of the present invention, wherein the abscissa is the diffraction angle and the ordinate is the absorbance;

[0034] Fig.10 This is a SEM image of the product in Example 4 of the present invention. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The preparation method of ZSM-12 molecular sieve provided in the embodiment of the present invention comprises:

[0037] 1. Preparation of pre-crystallized sol seed crystals: a. Weigh 1 part of silica sol, 0.01-0.005 parts of aluminum hydroxide, 0.3-0.7 parts of sodium hydroxide and 3-8 parts of deionized water by mass fraction; wherein the content of Al2O3 in aluminum hydroxide is 65%, and the content of SiO2 in silica sol is 25%-30%; b. Add the sodium hydroxide and aluminum hydroxide weighed in step a to deionized water, stir for 0.5-1h under the stirring condition of 200-300r / min, slowly add silica sol dropwise, and continue stirring and aging for 10h-15h after all the silica sol has been added dropwise to obtain a mixed gel; c. Place the mixed gel obtained in step b in a stainless steel reactor with a polytetrafluoroethylene liner, crystallize in an oven at a temperature of 140℃-160℃ for 2-6h, cool to room temperature after crystallization is completed, and take out to obtain pre-crystallized sol seed crystals.

[0038] 2. Add sodium hydroxide, aluminum hydroxide and deionized water to a 250 mL round-bottom flask, stir and dissolve at 100 ° C for 2 hours, and mix evenly to form a mixed solution; after stirring and dissolving, cool and cool, add silica gel to the mixed solution at room temperature, continue stirring for 10 minutes to form a gel, and then add 1wt.% to 40wt.% of the sol seed prepared in step 1, continue stirring to form an initial gel, and then pour the initial gel into a hydrothermal reactor for crystallization.

[0039] 3. Place the hydrothermal reactor containing the initial gel in a homogeneous reactor, react at 110°C for 20h-25h, and continue to react at 160°C for 20h-24h. After the reaction is completed and cooled, filter the reaction slurry through a sand core funnel, wash the filter cake three times with deionized water until the filtrate is neutral, and then dry the filter cake at 160°C-180°C for 2h-6h to obtain a powdered ZSM-12 molecular sieve.

[0040] Compared with the prior art, in the preparation method of the ZSM-12 molecular sieve provided by the present invention, an aluminum source is used as a raw material, and it is stirred and dissolved in an alkaline aqueous solution, and then a silicon source is added and stirred evenly for gelation reaction, and finally a sol seed is added, and then at a certain temperature, time and stirring rate, the gel is crystallized in a polytetrafluoroethylene reactor, and then the crystallized product is filtered, washed and dried to obtain a ZSM-12 type molecular sieve. It can be seen from the process that in the preparation method of the ZSM-12 type molecular sieve provided by the present invention, no expensive template agent is added, and the ZSM-12 type molecular sieve is synthesized by two-step hydrothermal synthesis by adding sol seeds that are easy to prepare, and the synthesis process is simple and reliable, the synthesis cost is low, and it is easy to implement.

[0041] The following is a detailed description of each step in the method for preparing the molecular sieve provided by the embodiment of the present invention.

[0042] In step 2, the molar ratio of the aluminum source to the silicon dioxide is (0.001-1):1, preferably (0.001-0.05):1; the molar ratio of the alkali source to the silicon dioxide is (0.03-0.5):1, preferably (0.04-0.3):1. In addition, the molar ratio of water to silicon dioxide in the solution is (3-20):1, preferably (5-15):1.

[0043] The alkali source may be one or more of potassium hydroxide, sodium hydroxide or ammonia. In this step, the aluminum source may be one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, sodium aluminate or aluminum sol, preferably aluminum hydroxide and sodium aluminate.

[0044] Adding a silicon source to the mixed solution, wherein the silicon source is selected from one or more of silica sol, solid silica gel, ethyl orthosilicate, white carbon black and water glass, preferably silica sol and solid silica gel; adding sol seed crystals to the mixed solution, wherein the amount of the sol seed crystals added is 1wt.% to 40wt.%, preferably 16wt.% to 32wt.% of the initial gel;

[0045] In step 3: after the crystallization is completed, the product is filtered, washed with water, and dried, and then tested by XRD, XRF, and SEM.

[0046] The preparation method of the molecular sieve provided by the present invention will be described in detail below through examples. In the following examples, X-ray powder diffraction phase analysis (XRD) is used, which is equipped with a PIXcel 3D detector; the test instrument for X-ray fluorescence analysis (XRF analysis): Philips MagiX fluorescence spectrometer, with a scintillation calculator and a proportional calculator to measure the intensity of the characteristic spectral lines of each element, and perform elemental composition analysis. Scanning electron microscope morphology analysis (SEM) uses a Japanese Hitachi S4800 scanning electron microscope. After the sample is dried and ground, it is glued to a conductive adhesive, and the acceleration voltage of the analysis electron microscope is 5.0kV, and the magnification is 20-800000 times.

[0047] Comparative Example 1

[0048] Take 3.10g of sodium hydroxide and add it to a 250mL round-bottom flask, then add 42.71g of TEAOH, 0.1g of aluminum hydroxide, and 57.97g of deionized water, heat and dissolve at 100°C for 2h, stir and mix evenly, then add 30g of silica gel and continue stirring for 10min to form an initial gel, wherein the molar ratio of each component is NaOH / SiO2=0.155, Al(OH)3 / SiO2=0.0015, TEAOH / SiO2=0.145, H2O / SiO2=10.

[0049] The polytetrafluoroethylene liner containing the above reaction mixture was covered, placed in a stainless steel autoclave, sealed, placed in a homogeneous reactor, and the speed was set to 20r / min. Crystallization was carried out under autogenous pressure: crystallization at 160°C for 50h, and after the crystallization was completed, the temperature was lowered to room temperature to take out the product, filtered and washed, and dried at 180°C for 2 hours to obtain a ZSM-12 molecular sieve sample. The obtained molecular sieve sample was subjected to X-ray diffraction analysis, and the XRD spectrum was shown in Figure 1 , there is a diffraction peak of ZSM-12 molecular sieve, and the crystallinity is 109.8%; the morphology of the molecular sieve was observed by SEM, and the SEM photos are shown in Figure 2 The molecular sieve is in the form of small particles with a grain size of 300-600nm. The molecular sieve is analyzed by XRD, and the SiO2 / Al2O3 molar ratio of the molecular sieve is 260.84. Figure 1The XRD pattern of the molecular sieve given shows that the output is ZSM-12 molecular sieve. Figure 2 The SEM image of the molecular sieve given shows that the grain morphology of the crystallized product is a rice-grain structure.

[0050] The following examples provide a specific synthesis method for preparing ZSM-12 molecular sieve without template (Examples 1-4)

[0051] Embodiment 1:

[0052] 1. Preparation of pre-crystallized sol seed crystals: a. Weigh 1 part of silica sol, 0.005 parts of aluminum hydroxide, 0.7 parts of sodium hydroxide and 6.5 parts of deionized water by mass fraction; wherein the content of Al2O3 in aluminum hydroxide is 65%, and the content of SiO2 in silica sol is 25%; b. Add the sodium hydroxide and aluminum hydroxide weighed in step a to deionized water, stir for 1 hour under the stirring condition of 200-300r / min, slowly add silica sol dropwise, and continue stirring and aging for 12 hours after all the silica sol has been added dropwise to obtain a mixed gel; c. Place the mixed gel obtained in step b in a stainless steel reactor with a polytetrafluoroethylene liner, crystallize in an oven at a temperature of 150°C for 2 hours, cool to room temperature after crystallization, and take out to obtain pre-crystallized sol seed crystals.

[0053] 2. Add sodium hydroxide, aluminum hydroxide and deionized water to a 250mL round-bottom flask, stir and dissolve at 100°C for 2h, and mix evenly to form a mixed solution; wherein the molar ratio of sodium hydroxide to silicon dioxide is 0.048:1, the molar ratio of aluminum hydroxide to silicon dioxide is 0.002:1, and the molar ratio of deionized water to silicon dioxide is 5.5:1. After stirring and dissolving, cool down, add silica gel to the mixed solution at room temperature, continue stirring for 10min to form an initial gel, the molar ratio of silica gel is 1, and then add 10wt.% of the sol seed prepared in step 1 of the initial gel, and then pour the mixed gel into a hydrothermal reactor for crystallization.

[0054] 3. Place the hydrothermal reactor containing the initial gel in a homogeneous reactor, react at 110°C for 24 hours, and continue to react at 160°C for 20 hours. After the reaction is completed and cooled, filter the reaction slurry through a sand core funnel. Wash the filter cake three times with deionized water until the filtrate is neutral, and then dry the filter cake at 180°C for 2 hours to obtain a powdered ZSM-12 molecular sieve. Figure 3 The XRD pattern of the molecular sieve given shows that the output is ZSM-12 molecular sieve with a crystallinity of 36.76%. Figure 4 The SEM image of the molecular sieve given shows that the crystallized material has a cubic structure.

[0055] Implementation 2

[0056] The second and third steps in Example 1 were repeated, except that the molar ratio of sodium hydroxide to silicon dioxide was 0.115:1, the molar ratio of aluminum hydroxide to silicon dioxide was 0.002:1, the molar ratio of deionized water to silicon dioxide was 10:1, and the amount of sol seed added was 16 wt.% of the initial gel.

[0057] The hydrothermal reactor containing the initial gel was placed in a homogeneous reactor, and the reaction was carried out at 110°C for 24 hours, and then at 160°C for 20 hours. After the reaction was completed and cooled, the reaction slurry was filtered through a sand core funnel, and the filter cake was washed three times with deionized water until the filtrate was neutral. The filter cake was then dried at 180°C for 2 hours to obtain a powdered ZSM-12 molecular sieve. Figure 5 The XRD pattern of the molecular sieve given shows that the output is ZSM-12 molecular sieve with a crystallinity of 85.32%. Figure 6 The SEM image of the molecular sieve shown above shows that the crystals of the crystallized product are in the shape of long strips.

[0058] Implementation 3

[0059] The second and third steps in Example 1 were repeated, except that the molar ratio of sodium hydroxide to silicon dioxide was 0.135:1, the molar ratio of aluminum hydroxide to silicon dioxide was 0.002:1, the molar ratio of deionized water to silicon dioxide was 10:1, and the amount of sol seed added was 25 wt.% of the initial gel.

[0060] The hydrothermal reactor containing the initial gel was placed in a homogeneous reactor, and the reaction was carried out at 110°C for 24 hours, and then at 160°C for 20 hours. After the reaction was completed and cooled, the reaction slurry was filtered through a sand core funnel, and the filter cake was washed three times with deionized water until the filtrate was neutral. The filter cake was then dried at 180°C for 2 hours to obtain a powdered ZSM-12 molecular sieve. Figure 7 The XRD pattern of the molecular sieve given shows that the output is ZSM-12 molecular sieve with a crystallinity of 81.5%. Figure 8 The SEM image of the molecular sieve given shows that the grain morphology of the crystallized product is a long strip structure.

[0061] Implementation 4

[0062] The second and third steps in Example 1 were repeated, except that the molar ratio of sodium hydroxide to silicon dioxide was 0.195:1, the molar ratio of aluminum hydroxide to silicon dioxide was 0.002:1, the molar ratio of deionized water to silicon dioxide was 10:1, and the amount of sol seed added was 32 wt.% of the initial gel.

[0063] The hydrothermal reactor containing the initial gel was placed in a homogeneous reactor, and the reaction was carried out at 110°C for 24 hours, and then at 160°C for 20 hours. After the reaction was completed and cooled, the reaction slurry was filtered through a sand core funnel, and the filter cake was washed three times with deionized water until the filtrate was neutral. The filter cake was then dried at 180°C for 2 hours to obtain a powdered ZSM-12 molecular sieve. Fig. 9 The XRD pattern of the molecular sieve given shows that the output is ZSM-12 molecular sieve with a crystallinity of 90.16%. Fig.10 The SEM image of the molecular sieve given shows that the grain morphology of the crystallized product is a long strip structure.

[0064] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.

[0065] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing ZSM-12 molecular sieve without template, characterized in that: Follow these steps: Step 1: preparing pre-crystallized sol seed crystals; Step 2: Stir and dissolve the aluminum source, alkali source and deionized water, add the silicon source to the mixed solution, stir for a period of time, add the pre-crystallized sol seed crystals, and continue stirring to form an initial gel; Step 3: Then the initial gel is placed in a polytetrafluoroethylene reactor for crystallization at two different temperatures. After the crystallization is completed, it is filtered, washed with water, and dried to obtain a ZSM-12 molecular sieve; Among them, the preparation method of pre-crystallized sol seed crystals is specifically as follows: a. weigh 1 part of silica sol, 0.01-0.005 parts of aluminum hydroxide, 0.3-0.7 parts of sodium hydroxide and 3-8 parts of deionized water by mass fraction; wherein the content of Al2O3 in aluminum hydroxide is 65%, and the content of SiO2 in silica sol is 25%-30%; b. add the sodium hydroxide and aluminum hydroxide weighed in step a to deionized water, stir for 0.5-1h under the stirring condition of 200-300r / min, slowly add silica sol dropwise, and continue stirring and aging for 10h-15h after all the silica sol is added dropwise to obtain a mixed gel; c. place the mixed gel obtained in step b in a stainless steel reactor with a polytetrafluoroethylene lining, crystallize in an oven at a temperature of 140℃-160℃ for 2-6h, cool to room temperature after crystallization, and take out to obtain pre-crystallized sol seed crystals.

2. The method for preparing ZSM-12 molecular sieve without template according to claim 1, characterized in that: The specific operation of step 2 is: stirring and dissolving the aluminum source, alkali and deionized water at 100°C, mixing them evenly to form a mixed solution, cooling them down, adding silica gel to the mixed solution at room temperature, continuing to stir to form a gel, and then adding 1wt.% to 40wt.% of the sol seed prepared in step 1 as the initial gel, and continuing to stir to form the initial gel.

3. The method for preparing ZSM-12 molecular sieve without template according to claim 2, characterized in that: In step 2: the molar ratio of the aluminum source to silicon dioxide is (0.001-1):1, the molar ratio of the alkali source to silicon dioxide is (0.03-0.5):1, and the molar ratio of water to silicon dioxide in the solution is (3-20):

1.

4. The method for preparing ZSM-12 molecular sieve without template according to claim 3, characterized in that: In step 2: the molar ratio of the aluminum source to silicon dioxide is (0.001-0.05):1; the molar ratio of the alkali source to silicon dioxide is (0.04-0.3):1, and the molar ratio of water to silicon dioxide in the solution is (5-15):

1.

5. The method for preparing ZSM-12 molecular sieve without template according to claim 2, characterized in that: In step 2, the alkali source is one or more of potassium hydroxide, sodium hydroxide or ammonia water; the aluminum source is one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, sodium aluminate or aluminum sol; and the silicon source is one or more of silica sol, solid silica gel, ethyl orthosilicate, white carbon black and water glass.

6. The method for preparing ZSM-12 molecular sieve without template according to claim 5, characterized in that: In step 2, the aluminum source is aluminum hydroxide or sodium aluminate, and the silicon source is silica sol or solid silica gel.

7. The method for preparing ZSM-12 molecular sieve without template according to claim 2, characterized in that: The amount of pre-crystallized sol seed crystals added is 16 wt.% to 32 wt.% of the initial gel.

8. The method for preparing ZSM-12 molecular sieve without template according to claim 1, characterized in that: The crystallization in step 3 is carried out at 110° C. for 20 h to 25 h, and then at 160° C. for 20 h to 24 h.