A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts
By treating organic silicon waste contacts by roasting and acid leaching, combined with vacuum induction furnace smelting and electromagnetic force separation, the recycling process of silicon and copper is simplified, solving the problems of complex processes and high energy consumption in the existing technology, and achieving high efficiency and environmental protection. of silicon and copper recycling.
Patent Information
- Application Number
- CN202410500214.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-04-24
AI Technical Summary
In the existing technology, the recovery and treatment process of silicon and copper in organic silicon waste contacts is complicated, which easily produces waste liquid and increases energy consumption. It also intensifies the corrosion of equipment and affects the performance of the recycled materials and the environment.
By roasting the silicone waste contact, using acid leaching for solid-liquid separation, and then smelting in a vacuum induction furnace, using electromagnetic force to separate copper and silicon, forming a mixed ingot and cutting to obtain copper-rich ingots and silicon ingots, simplifying the process flow , reduce waste generation.
It achieves efficient separation of silicon and copper, reduces process corrosion and energy consumption of equipment, simplifies the recycling process, improves recycling efficiency and purity, reduces waste generation, and is suitable for industrial promotion.
Smart Images

Figure CN118345246B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recycling and environmental protection, and relates to a method for preparing silicon-copper alloy and high-purity silicon by utilizing waste organic silicon contacts. Background Art
[0002] Organosilicon materials are widely used in aerospace, medical and health, and new energy industries due to their excellent performance in many aspects. Organosilicon monomers are important raw materials for the synthesis of organosilicon materials. The most widely used monomer is dimethylchlorosilane (M2). At present, the industrial production of M2 mainly adopts the "direct synthesis method", that is, industrial silicon powder and methyl chloride are used as raw materials, copper compounds are used as catalysts, and a methylchlorosilane mixture mainly composed of M2 is synthesized under certain temperature and pressure conditions in a fluidized bed reactor, and then M2 is separated from other by-products by distillation and other methods. In the direct synthesis process, due to factors such as the accumulation of impurities and the deactivation of catalysts, the conversion rate of silicon powder and the selectivity of the target product M2 will be significantly reduced. In order to maintain stable production, some unreacted silicon powder and deactivated catalysts must be discharged from the reactor to form industrial waste slag, which is the organosilicon waste contact body.
[0003] In the National List of Hazardous Wastes (2021), waste silicone contacts belong to waste organic solvents and waste containing organic solvents. Improper treatment can easily cause serious environmental pollution. In addition, waste silicone contacts contain about 65-75% silicon and about 10-15% copper. If the silicon and copper resources can be effectively recycled, considerable resource benefits and economic benefits can be generated.
[0004] At present, the recovery and treatment of silicon and copper in waste silicone contacts mainly focuses on the use of oxidants or other additives, and the copper is dissolved in the acid solution through processes such as oxidative acid leaching, and then the copper-containing solution and solids such as leaching residues are obtained by separation of the solid phase and the liquid phase. Finally, copper is extracted from the copper-containing solution alone, and silicon is extracted from solids such as leaching residues. For example, the patent with application number 202310000719.4 discloses a method for extracting copper from waste silicone contacts, which first obtains a copper-containing filtrate after solid-liquid separation, and then reduces the copper-containing filtrate to obtain elemental copper powder. For another example, the patent with patent number 202210762039.1 discloses a method for recovering copper and high-purity silicon powder from waste silicone contacts, which obtains a copper-containing leaching solution and leaching residues after solid-liquid separation after oxidative acid leaching, and then obtains silicon powder by neutralization through filter pressing, and obtains cathode copper by extraction, stripping and copper electrowinning. First, when more copper is dissolved into the acid solution through processes such as oxidative acid leaching, the process requirements are relatively complex, and other process equipment and additives may need to be introduced. In addition, oxidative acid leaching will deepen the corrosion of the equipment. Secondly, in the stage of extracting copper and silicon separately, the effect of solid-liquid phase separation is greatly affected by the separation conditions. The process is relatively complex and is prone to produce waste such as waste liquid, increasing the processing burden and energy consumption. At the same time, the solid-liquid phase separation process may also have a certain impact on the recyclables themselves, thereby affecting the performance of the recyclables.
[0005] Therefore, it is necessary to provide a method for preparing silicon-copper alloy and high-purity silicon using waste silicone contacts, reduce the impact of the process on equipment corrosion, simplify the process, reduce waste generation, reduce the degree of dependence of the process on separation conditions, and improve process stability, thereby achieving the purpose of reducing energy consumption, reducing costs, and effectively recovering copper and silicon in waste silicone contacts. Summary of the invention
[0006] In order to overcome the problems in the background technology, the present invention separates the silicon-copper slag from other impurities first, without allowing a large amount of copper to enter the liquid, without using other additives such as oxidants, and only needs to be completed through acid leaching, and then the silicon-copper powder is smelted. During the smelting process, the silicon component and the copper component are separated, and finally a mixed ingot is obtained. At this time, since a large amount of copper components and silicon components in the mixed ingot have been concentrated in different positions of the mixed ingot, the mixed ingot can be separated into solids by simple cutting to obtain silicon ingots and copper-rich ingots, thereby giving play to the advantages of solid-solid separation, simplifying the recycling process, reducing the amount of waste generated, and reducing the impact of the recycling process on the recyclables themselves, thereby reducing recycling energy consumption and costs, and effectively realizing the recycling of copper and silicon in waste silicone contacts, realizing resource recycling, and alleviating the environmental burden.
[0007] In order to achieve the above object, the present invention is implemented by the following technical solutions:
[0008] The preparation method comprises the following steps:
[0009] S1: In an environment of a mixed gas of oxygen and nitrogen, the waste organosilicon contacts are roasted to obtain a waste contact roasted material.
[0010] S2: prepare dilute hydrochloric acid and hydrofluoric acid and mix them to obtain a mixed solution. After heating the mixed solution to the target temperature, add the waste contact body roasting material obtained in step S1 to the mixed solution for acid leaching, wherein the solid-liquid ratio of the waste contact body roasting material to the mixed solution is 60:1~300:1, in g:L, and stir continuously during the acid leaching process to obtain an acid leaching slurry.
[0011] S3: The acid leaching slurry obtained in step S2 is filtered to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and the silicon-copper slag is vacuum dried to obtain silicon-copper powder.
[0012] S4: placing the silicon copper powder obtained in step S3 in a vacuum induction furnace, smelting at 1420-1600°C, keeping the temperature for 30-200 minutes, and then quenching the melt at a temperature of 1-20 μm·s -1 After the melt slowly migrates out of the smelting area from one end of the induction coil at a speed, it is slowly cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot. When the melt slowly migrates upward from one end of the induction coil out of the smelting area, the top of the melt leaves the smelting area first, and the temperature of the melt that leaves the smelting area first will drop to the melting point of silicon first, and the silicon in the melt will solidify into an ingot first. At this time, since the copper still exists in the form of a melt, the remaining silicon-copper alloy melt with a lower melting point will migrate downward to the smelting area under the action of electromagnetic force, and the copper melt originally located at the top of the melt will separate from the copper melt and, as the melt continues to move upward out of the smelting area, the above process is repeated at the solid-liquid interface, and the copper in the melt is continuously enriched at the end opposite to the migration direction of the melt. As a result, the melt gradually leaves the smelting area from top to bottom, the copper melt continuously migrates downward, and silicon continuously solidifies. Since the silicon content is limited, when the melt moves upward to a certain position, the silicon content in the melt in the smelting area is already less. At this time, when the melt temperature drops to the melting point of the silicon-copper alloy melt, the melt solidifies to form a copper-rich ingot. Therefore, when the direction of the mixed ingot is not rotated, the upper part of the mixed ingot is usually the silicon ingot part, and the lower part is usually the copper-rich ingot part.
[0013] S5: testing and analyzing the copper-rich ingot obtained in step S4, adjusting the relative content of silicon and copper according to the test and analysis results, and performing smelting.
[0014] S6: After the smelting is completed, the melt temperature is lowered to the target temperature for secondary heat preservation, and after the secondary heat preservation is completed, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot. The silicon-copper alloy ingot can be used as a raw material for preparing a catalyst for monomer synthesis.
[0015] Preferably, in step S1, the volume flow rate of oxygen in the mixed gas accounts for 0.05-0.20.
[0016] Preferably, in step S1, the calcination temperature is 450-700°C.
[0017] Preferably, in said step S1, the insulation time is 10 to 200 minutes.
[0018] Preferably, in step S2, the concentration of dilute hydrochloric acid is 1-5 mol·L -1 , hydrofluoric acid concentration is 0.1~2.0mol·L -1 , after the mixed solution is heated to 30~70℃, the spent contact roasting material is added for acid leaching.
[0019] Preferably, the acid leaching time is 30 to 300 minutes.
[0020] Preferably, in step S4, the cutting position is determined by the copper content in the mixed ingot, the copper content is 0.1wt% as the dividing line, the part with copper content below 0.1wt% is the silicon ingot, and the rest is the copper-rich ingot. The position where the copper content in the mixed ingot is 0.1wt% can be determined by testing the mixed ingot.
[0021] Preferably, in step S5, the relative content of silicon and copper in the copper-rich ingot is adjusted by supplementing silicon or copper, and the copper-rich ingot and the supplemented components are smelted together, and the relative content of silicon and copper in the copper-rich ingot after adjustment satisfies that the silicon content is 5.0-20.0wt% and the copper content is 80.0-95.0wt%.
[0022] Preferably, in step S5, the smelting temperature is 1150-1500° C., and the holding time is 30-200 min.
[0023] Preferably, in step S6, the secondary insulation temperature is 800-900° C., and the secondary insulation time is 60-300 min.
[0024] Beneficial effects of the present invention:
[0025] 1. The present invention separates the copper component from the silicon component through the smelting process, so that after solidification into a mixed ingot, the copper component and the silicon component are respectively concentrated in different parts of the mixed ingot, so that the copper component and the silicon component can be separated by cutting to obtain a copper-rich ingot and a silicon ingot, so that the process flow is simplified, and at the same time, the impact of the separation process on the recyclables themselves is reduced, and the waste generated in the separation and recycling process is reduced or even avoided, thereby reducing the recycling energy consumption and cost and improving the recycling efficiency.
[0026] 2. The present invention does not need to separate copper and silicon in the acid leaching stage, which is conducive to the use of additives such as oxidants, reduces the requirements for equipment corrosion resistance, and is conducive to further reducing costs and energy consumption, and is suitable for industrial promotion.
[0027] 3. The purity of silicon ingots recovered by the present invention can reach more than 99%. At the same time, the copper-rich ingots can be used as raw materials for preparing catalysts for monomer synthesis, effectively recycling waste, alleviating environmental pressure on the one hand, and realizing resource recovery and secondary utilization on the other hand. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with specific embodiments.
[0030] The chemical composition of the waste organic silicon contact body used in the embodiment of the present invention is: 65.33% silicon, 12.32% copper, 5.51% iron, 1.04% aluminum, 0.35% calcium, 0.98% zinc, 2.32% carbon, and 12.15% others.
[0031] In the examples of the present invention, chemical reagents not otherwise specified were all commercially available analytically pure for the experiments. Example 1
[0032] In this embodiment, silicon ingots and silicon-copper alloy ingots are prepared by the following steps:
[0033] (1) In a mixed gas environment of oxygen and nitrogen (where the volume flow rate of oxygen in the mixed gas accounts for 0.05), 100 g of waste silicone contacts were placed in a resistance furnace, kept warm for 10 min at 450 ° C, and roasted to obtain a waste contact roasted material;
[0034] (2) In a batch reactor, prepare 1 mol·L -1 Dilute hydrochloric acid and 0.1 mol·L -1Hydrofluoric acid is added and mixed to obtain a mixed solution, and after the mixed solution is heated to 30° C., the spent contact body roasting material is added to the mixed solution for acid leaching for 30 minutes, wherein the solid-liquid ratio of the spent contact body roasting material to the mixed solution is 60:1, in g:L, and stirring is continued during the acid leaching process to obtain an acid leaching slurry;
[0035] (3) filtering the acid leaching slurry to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and vacuum drying the silicon-copper slag to obtain silicon-copper powder;
[0036] (4) Place the silicon copper powder in a vacuum induction furnace and melt it at 1420°C. After keeping the temperature for 30 minutes, the melt is heated to 1 μm·s -1 After slowly migrating out of the smelting area from one end of the induction coil at a speed of , the mixture is slowly cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot. The total height of the mixed ingot obtained in this embodiment is 12.5 cm, and the cutting position is 10.29 cm from the top of the mixed ingot. The upper section is a high-purity silicon ingot, and the lower section is a copper-rich ingot.
[0037] (5) The copper-rich ingot was tested and analyzed. The copper content in the copper-rich ingot was 75.50 wt%. The relative content of silicon and copper was adjusted by adding 3.6 g of copper powder. The copper-rich ingot and copper powder were smelted together at 1150 °C for 30 min.
[0038] (6) After the smelting is completed, the melt temperature is lowered to 800°C for secondary heat preservation. After the secondary heat preservation for 60 minutes, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot, in which the silicon content is about 5.0wt% and the copper content is about 95.0wt%.
[0039] The components of the high-purity silicon ingot and the silicon-copper alloy ingot prepared in this example were analyzed, and the results are shown in Table 1.
[0040] Table 1
[0041] Element(%) Si Cu Fe Al Ca Zn C other Silicon Ingot 99.72 0.09 0.0013 0.0025 0.0013 0.0001 0.0311 0.1524 Alloy Ingot 4.98 94.63 0.1500 0.0059 0.0014 0.0021 0.0343 0.1963 Example 2
[0042] In this embodiment, silicon ingots and silicon-copper alloy ingots are prepared by the following steps:
[0043] (1) In a mixed gas environment of oxygen and nitrogen (where the volume flow rate of oxygen in the mixed gas accounts for 0.20), 2 tons of waste silicone contacts were placed in a resistance furnace and kept at 700°C for 200 minutes to obtain a waste contact calcined material;
[0044] (2) In a batch reactor, prepare 5 mol·L -1 Dilute hydrochloric acid and 2 mol·L -1Hydrofluoric acid is added to obtain a mixed solution, and the mixed solution is heated to 70°C, and then the spent contact body roasting material is added to the mixed solution for acid leaching for 300 minutes, wherein the solid-liquid ratio of the spent contact body roasting material to the mixed solution is 300:1, in g:L, and stirring is continued during the acid leaching process to obtain an acid leaching slurry;
[0045] (3) filtering the acid leaching slurry to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and vacuum drying the silicon-copper slag to obtain silicon-copper powder;
[0046] (4) Place the silicon copper powder in a vacuum induction furnace and melt it at 1600°C. After keeping the temperature for 200 minutes, the melt is heated at 20 μm·s -1 After slowly migrating out of the smelting area from one end of the induction coil at a speed of , the mixture is slowly cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot. The total height of the mixed ingot obtained in this embodiment is 350.0 cm, and the cutting position is 301.6 cm from the top of the mixed ingot. The upper section is a high-purity silicon ingot, and the lower section is a copper-rich ingot.
[0047] (5) The copper-rich ingot was tested and analyzed. The copper content in the copper-rich ingot was 79.36wt%. The relative content of silicon and copper was adjusted by adding 6.8kg of copper powder. The copper-rich ingot and copper powder were smelted together at 1500℃ for 200min.
[0048] (6) After the smelting is completed, the melt temperature is lowered to 900°C for secondary heat preservation. After the secondary heat preservation for 300 minutes, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot, in which the silicon content is about 20.0wt% and the copper content is about 80.0wt%.
[0049] The components of the high-purity silicon ingot and the silicon-copper alloy ingot prepared in this example were analyzed, and the results are shown in Table 2.
[0050] Table 2
[0051] Element(%) Si Cu Fe Al Ca Zn C other Silicon Ingot 99.84 0.08 0.0015 0.0016 0.0013 0.0001 0.0205 0.0550 Alloy Ingot 19.87 79.31 0.0053 0.0049 0.0014 0.0001 0.0443 0.764 Example 3
[0052] In this embodiment, silicon ingots and silicon-copper alloy ingots are prepared by the following steps:
[0053] (1) In a mixed gas environment of oxygen and nitrogen (where the volume flow rate of oxygen in the mixed gas accounts for 0.10), 100 g of waste silicone contacts were placed in a resistance furnace and calcined at 550°C for 30 min to obtain a waste contact calcined material.
[0054] (2) In a batch reactor, prepare 2 mol·L -1 Dilute hydrochloric acid and 0.1 mol·L -1Hydrofluoric acid is added and mixed to obtain a mixed solution, and the mixed solution is heated to 50°C, and then the spent contact body calcined material is added to the mixed solution for acid leaching for 90 minutes, wherein the solid-liquid ratio of the spent contact body calcined material to the mixed solution is 80:1, and the unit is g:L. Stirring is continued during the acid leaching process to obtain an acid leaching slurry.
[0055] (3) The acid leaching slurry is filtered to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and the silicon-copper slag is vacuum dried to obtain silicon-copper powder.
[0056] (4) Place the silicon copper powder in a vacuum induction furnace and melt it at 1450°C. After keeping the temperature for 30 minutes, the melt is heated at a speed of 15 μm·s -1 After slowly migrating out of the smelting area from one end of the induction coil at a speed of , the mixture is slowly cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot. The total height of the mixed ingot obtained in this embodiment is 12.8 cm, and the cutting position is 10.29 cm from the top of the mixed ingot. The upper section is a high-purity silicon ingot, and the lower section is a copper-rich ingot.
[0057] (5) The copper-rich ingot was tested and analyzed. The copper content in the copper-rich ingot was 75.83 wt%. The relative content of silicon and copper was adjusted by adding 3.6 g of copper powder. The copper-rich ingot and copper powder were smelted together at 1500°C for 60 min.
[0058] (6) After the smelting is completed, the melt temperature is lowered to 880°C for secondary heat preservation. After the secondary heat preservation for 200 minutes, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot, in which the silicon content is about 9.0wt% and the copper content is about 88.0wt%.
[0059] The components of the high-purity silicon ingot and the silicon-copper alloy ingot prepared in this example were analyzed, and the results are shown in Table 3.
[0060] Table 3
[0061] Element(%) Si Cu Fe Al Ca Zn C other Silicon Ingot 99.82 0.09 0.0013 0.0021 0.0013 0.0001 0.0311 0.0541 Alloy Ingot 9.07 87.93 0.5100 0.0059 0.0014 0.0021 0.0343 2.4463 Example 4
[0062] In this embodiment, silicon ingots and silicon-copper alloy ingots are prepared by the following steps:
[0063] (1) In a mixed gas environment of oxygen and nitrogen (where the volume flow rate of oxygen in the mixed gas accounts for 0.15), 500 g of waste silicone contacts were placed in a resistance furnace and calcined at 550°C for 70 min to obtain the waste contact calcined material.
[0064] (2) In a batch reactor, prepare 3 mol·L -1 Dilute hydrochloric acid and 1.0 mol·L -1Hydrofluoric acid is added and mixed to obtain a mixed solution, and the mixed solution is heated to 50°C, and then the spent contact body calcined material is added to the mixed solution for acid leaching for 100 minutes, wherein the solid-liquid ratio of the spent contact body calcined material to the mixed solution is 100:1, and the unit is g:L. Stirring is continued during the acid leaching process to obtain an acid leaching slurry.
[0065] (3) The acid leaching slurry is filtered to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and the silicon-copper slag is vacuum dried to obtain silicon-copper powder.
[0066] (4) Place the silicon copper powder in a vacuum induction furnace and melt it at 1500°C. After keeping the temperature for 60 minutes, the melt is heated at a speed of 15 μm·s -1 After slowly migrating out of the smelting area from one end of the induction coil at a speed of , the mixture is slowly cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot. The total height of the mixed ingot obtained in this embodiment is 20.1 cm, and the cutting position is 18.9 cm from the top of the mixed ingot. The upper section is a high-purity silicon ingot, and the lower section is a copper-rich ingot.
[0067] (5) The copper-rich ingot was tested and analyzed. The copper content in the copper-rich ingot was 77.92 wt%. The relative content of silicon and copper was adjusted by adding 25.7 g of copper powder. The copper-rich ingot and copper powder were smelted together at 1150°C for 70 min.
[0068] (6) After the smelting is completed, the melt temperature is lowered to 850°C for secondary insulation. After the secondary insulation for 200 minutes, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot, in which the silicon content is about 11.0wt% and the copper content is about 88.0wt%.
[0069] The components of the high-purity silicon ingot and the silicon-copper alloy ingot prepared in this example were analyzed, and the results are shown in Table 4.
[0070] Table 4
[0071] Element(%) Si Cu Fe Al Ca Zn C other Silicon Ingot 99.92 0.012 0.0025 0.0022 0.0013 0.0001 0.0405 0.0217 Alloy Ingot 10.86 88.23 0.0492 0.0049 0.0021 0.0001 0.0446 0.8091 Example 5
[0072] In this embodiment, silicon ingots and silicon-copper alloy ingots are prepared by the following steps:
[0073] (1) In a mixed gas environment of oxygen and nitrogen (where the volume flow rate of oxygen in the mixed gas accounts for 0.15), 2000 g of waste silicone contacts were placed in a resistance furnace and kept warm for 45 min at 600 °C to obtain a waste contact calcined material.
[0074] (2) In a batch reactor, prepare 3 mol·L -1 Dilute hydrochloric acid and 1.0 mol·L -1Hydrofluoric acid is added and mixed to obtain a mixed solution, and the mixed solution is heated to 50°C, and then the spent contact body calcined material is added to the mixed solution for acid leaching for 90 minutes, wherein the solid-liquid ratio of the spent contact body calcined material to the mixed solution is 80:1, and the unit is g:L. Stirring is continued during the acid leaching process to obtain an acid leaching slurry.
[0075] (3) The acid leaching slurry is filtered to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and the silicon-copper slag is vacuum dried to obtain silicon-copper powder.
[0076] (4) Place the silicon copper powder in a vacuum induction furnace and melt it at 1450°C. After keeping the temperature for 30 minutes, the melt is heated to 5 μm·s -1 After slowly migrating out of the smelting area from one end of the induction coil at a speed of , the mixture is slowly cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot. The total height of the mixed ingot obtained in this embodiment is 31.6 cm, and the cutting position is 27.3 cm from the top of the mixed ingot. The upper section is a high-purity silicon ingot, and the lower section is a copper-rich ingot.
[0077] (5) The copper-rich ingot was tested and analyzed. The copper content in the copper-rich ingot was 80.03 wt%. The relative content of silicon and copper was adjusted by adding 56.7 g of copper powder. The copper-rich ingot and copper powder were smelted together at 1200 °C for 100 min.
[0078] (6) After the smelting is completed, the melt temperature is lowered to 850°C for secondary heat preservation. After the secondary heat preservation for 300 minutes, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot, in which the silicon content is about 12.5wt% and the copper content is about 87.5wt%.
[0079] The components of the high-purity silicon ingot and the silicon-copper alloy ingot prepared in this example were analyzed, and the results are shown in Table 5.
[0080] Table 5
[0081] Element(%) Si Cu Fe Al Ca Zn C other Silicon Ingot 99.97 0.001 0.0003 0.0004 0.0007 0.0001 0.0121 0.0091 Alloy Ingot 12.43 87.41 0.0963 0.0035 0.0010 0.0001 0.0251 0.0340
[0082] By comparing Example 1 with Example 3, it can be seen that when the mixed ingots are of similar size, the cutting position is almost at the same position, indicating that the method of the present invention is stable in the process of preparing silicon ingots and copper-rich ingots. At the same time, before adding monomers to synthesize silicon-copper alloy ingots, the copper content of the copper-rich ingot is basically maintained at 75%~80%, and the impurity content is low, indicating that the method of the present invention is relatively stable and can effectively reduce the impurity content in the recyclate.
[0083] In summary, the method of the present invention can be used to prepare silicon ingots with higher purity in a relatively simple and convenient manner, and by adding monomers to synthesize silicon-copper alloy ingots, they can be used to prepare catalysts used in monomer synthesis, effectively realizing the recycling of waste, with significant economic and environmental benefits, and is of great significance to achieving the green and healthy development of the silicone industry.
[0084] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts. Features: The preparation method comprises the following steps: S1: roasting the waste organosilicon contact body in an oxygen and nitrogen mixed gas environment to obtain a waste contact body roasting material; S2: preparing dilute hydrochloric acid and hydrofluoric acid and mixing them to obtain a mixed solution, heating the mixed solution to a target temperature, adding the waste contact body roasting material obtained in step S1 to the mixed solution for acid leaching, wherein the solid-liquid ratio of the waste contact body roasting material to the mixed solution is 60:1-300:1, in g:L, and continuously stirring during the acid leaching process to obtain an acid leaching slurry; S3: filtering the acid leaching slurry obtained in step S2 to achieve solid-liquid separation to obtain leaching tail liquid and silicon-copper slag, and vacuum drying the silicon-copper slag to obtain silicon-copper powder; S4: placing the silicon copper powder obtained in step S3 in a vacuum induction furnace, smelting at 1420-1600°C, keeping the temperature for 30-200 minutes, and then quenching the melt at a temperature of 1-20 μm·s -1 After slowly migrating out of the smelting area from one end of the induction coil at a speed, the mixture is naturally cooled to room temperature to obtain a mixed ingot, which is then cut and separated to obtain a silicon ingot and a copper-rich ingot; S5: testing and analyzing the copper-rich ingot obtained in step S4, adjusting the relative content of silicon and copper according to the test and analysis results, and performing smelting; S6: After the smelting is completed, the melt temperature is lowered to the target temperature for secondary insulation. After the secondary insulation is completed, the temperature is slowly lowered to room temperature to obtain a silicon-copper alloy ingot.
2. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 1, Features: In step S1, the volume flow rate of oxygen in the mixed gas accounts for 0.05-0.
20.
3. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 1, Features: In the step S1, the calcination temperature is 450-700°C.
4. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 3, Features: In step S1, the insulation time is 10 to 200 minutes.
5. The method for preparing silicon-copper alloy and high-purity silicon by using waste organic silicon contacts according to claim 1, Features: In step S2, the concentration of dilute hydrochloric acid is 1-5 mol·L -1 , hydrofluoric acid concentration is 0.1~2.0 mol·L -1 , after the mixed solution is heated to 30~70℃, the spent contact roasting material is added for acid leaching.
6. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 5, Features: The acid leaching time is 30 to 300 minutes.
7. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 1, Features: In step S4, the cutting position is determined by the copper content in the mixed ingot, the copper content is 0.1wt% as the dividing line, the part with copper content below 0.1wt% is the silicon ingot, and the rest is the copper-rich ingot.
8. The method for preparing silicon-copper alloy and high-purity silicon by using waste organic silicon contacts according to claim 1, Features: In step S5, the relative content of silicon and copper in the copper-rich ingot is adjusted by supplementing silicon or copper, and the copper-rich ingot and the supplemented components are smelted together, and the relative content of silicon and copper in the copper-rich ingot after adjustment satisfies the silicon content of 5.0-20.0wt% and the copper content of 80.0-95.0wt%.
9. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 1, Features: In step S5, the smelting temperature is 1150-1500° C., and the holding time is 30-200 min.
10. A method for preparing silicon-copper alloy and high-purity silicon using waste organic silicon contacts according to claim 1, Features: In step S6, the secondary insulation temperature is 800-900° C., and the secondary insulation time is 60-300 min.
Citation Information
Cited By
Method for preparing silicon-copper alloy by using organic silicon synthesis waste contact body
CN121428613A
A method for preparing silicon-copper alloy by using organic silicon synthesis waste catalyst