A method for upsetting a round aluminum alloy ingot with a large aspect ratio
By adding concave incisions to the cross-section of aluminum alloy round ingots, combined arrangements, pre-punching and low-speed upsetting methods, the problem of upsetting deformation and instability of aluminum alloy round ingots with a large aspect ratio is solved and better results are achieved. organization and performance, simplifying processes and reducing costs.
Patent Information
- Application Number
- CN202410789358.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-19
AI Technical Summary
It is difficult to effectively achieve upsetting of aluminum alloy round ingots with large aspect ratios using existing technology, and is prone to problems such as deformation instability and complex process flow.
By adding concave incisions to the circular cross-section of the aluminum alloy round ingot, pre-punching holes in the center of the end face after the combination and arrangement, and utilizing the mutual force restriction relationship between the arc contact surfaces during the low-speed upsetting process, an overall direction is formed. External expansion force reduces deformation dead zone and avoids bulging phenomenon.
It achieves stable upsetting of aluminum alloy round ingots with a large aspect ratio, reduces the chemical segregation and coarse structure of the ingots, improves the structure and performance, simplifies the process and reduces costs.
Smart Images

Figure CN118357403B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of aluminum alloy round ingots, in particular to an upsetting method for large aspect ratio aluminum alloy round ingots. Background Art
[0002] Upsetting is a basic plastic deformation process to improve the structure of aluminum alloy ingots. Almost all forged aluminum alloys need to be upset first to open the blank. The height-to-diameter ratio of the ingot is the most important condition for achieving upsetting. Generally, 2~2.5 is the optimal range, and the maximum does not exceed 3.5. If the value exceeds this, the ingot is prone to instability and cannot be formed. For round ingots, as the diameter increases, it is easy to produce chemical composition segregation, coarse structure and other undesirable metallurgical structures. Therefore, under the condition of meeting the height-to-diameter ratio requirements, the smaller the ingot diameter, the better.
[0003] For some large forgings, if a large-diameter ingot with a height-to-diameter ratio not exceeding 3.5 is selected for upsetting, the metallurgical quality requirements of the ingot need to be lowered. If a small-diameter ingot with higher metallurgical quality is selected for upsetting, the problem of upsetting instability with a large height-to-diameter ratio needs to be solved. This is a difficult problem currently faced by the industry.
[0004] In order to achieve upsetting with a large aspect ratio, the existing public solutions focus on adding proprietary molds, but there are problems such as high mold opening costs and complicated process flows; some solutions use the method of tilting the ingot at a certain angle, a small amount of reduction, and multiple deformations to achieve this, which has the problem of complicated process flows. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for upsetting a large aspect ratio aluminum alloy round ingot, which can achieve the upsetting of a large aspect ratio aluminum alloy round ingot, avoid deformation and instability of the aluminum alloy round ingot, and have better structure and performance.
[0006] In view of this, the present application provides a method for upsetting a round aluminum alloy ingot with a large aspect ratio, comprising the following steps:
[0007] S1) heating an aluminum alloy round ingot, wherein the round cross section of the aluminum alloy ingot has a concave cutout;
[0008] S2) arranging the aluminum alloy ingots obtained in the three steps S1) in a manner of maximizing the cross-sectional area to obtain a combined ingot;
[0009] S3) pre-punching a hole at the center of the end surface of the combined ingot;
[0010] S4) upsetting the ingot obtained in step S3);
[0011] The surface area of the concave cutout is minimized to maximize the cross-sectional area of the combined ingot;
[0012] The radius of the aluminum alloy round ingot is set to R, the width of the concave cut is R±10 mm, the depth of the concave cut is 0.134R±10 mm; the edge of the concave cut is an arc;
[0013] The diameter of the pre-punched hole is 200-300 mm, and the depth of the pre-punched hole is 50-80 mm.
[0014] Preferably, the heating temperature is 400-550° C. and the insulation time is 10-30 hours.
[0015] Preferably, the pre-punching process further includes flat anvil heating, the flat anvil heating temperature is 400-500° C., and the heat preservation time is 10-30 hours.
[0016] Preferably, during the pre-punching process, the aluminum alloy round ingot, the punch and the anvil are placed in sequence.
[0017] Preferably, the upsetting rate does not exceed 10 mm / s.
[0018] Preferably, the upsetting rate is 5-8 mm / s.
[0019] Preferably, the aspect ratio of the aluminum alloy round ingot is greater than 3.5.
[0020] Preferably, the aluminum alloy round ingot includes 7050 aluminum alloy round ingot, 2219 aluminum alloy round ingot, 7075 aluminum alloy round ingot, 7055 aluminum alloy round ingot, 7085 aluminum alloy round ingot, 2A14 aluminum alloy round ingot, 2195 aluminum alloy round ingot or 2050 aluminum alloy round ingot.
[0021] The present application provides a method for upsetting an aluminum alloy round ingot with a large aspect ratio, which comprises first heating the aluminum alloy round ingot, wherein the circular cross section of the aluminum alloy round ingot has a concave cutout, then arranging three heated aluminum alloy round ingots of the above shape in a manner to maximize the cross-sectional area to obtain a combined ingot, then pre-punching a hole at the center position of the end face of the combined ingot, and finally upsetting the obtained ingot. During the upsetting process of aluminum alloy round ingots with a large aspect ratio, the present application provides a concave cutout on the aluminum alloy round ingot, and utilizes the characteristics of the intersection of three circles. As the overlapping area of the cross sections of the round ingots increases, the total cross-sectional area of the ingots gradually decreases, and the contact area between the ingots gradually increases. When the three round ingots intersect at one point, the ingots are in the closest contact condition and have the largest total cross-sectional area, thereby realizing the connection of small-section ingots into an overall large-section ingot, reducing the aspect ratio of the ingots; at the same time, utilizing the mutual force constraint relationship between the arc contact surfaces, during the upsetting process, the force at the intersection point of a single round ingot in the horizontal direction is suppressed, thereby forming an overall outward expansion force, realizing an upsetting method similar to that of a single large-section ingot, which is not easy to separate during the upsetting process and ensures the microstructure of the upsetting ingot. Furthermore, a method of pre-punching the center hole is adopted to reduce the deformation dead zone and prevent the problem of bulging too early in the initial stage of upsetting, thereby causing deformation instability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of a concave cutout in the cross section of an aluminum alloy round ingot of the present invention;
[0023] Figure 2 This is a schematic diagram of the arrangement of aluminum alloy round ingots of the present invention;
[0024] Figure 3 This is a schematic diagram of pre-punching holes in an aluminum alloy ingot according to the present invention;
[0025] Figure 4 It is a schematic diagram of the cross section of the central punching of the aluminum alloy ingot of the present invention;
[0026] Figure 5 It is a schematic diagram of the upsetting of the aluminum alloy ingot of the present invention;
[0027] Figure 6 This is a microstructure photograph of the aluminum alloy ingot prepared in Example 1 of the present invention;
[0028] Figure 7 This is a microstructure photograph of the aluminum alloy ingot prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0029] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0030] In view of the problems in the prior art that large aspect ratio aluminum alloy round ingots are prone to instability and complex process flow during upsetting, the present application provides an upsetting method for large aspect ratio aluminum alloy round ingots, which can form the closest contact between the ingots by adopting a combination of aluminum alloy round ingots with concave cutouts, with the largest total cross-sectional area to transform the aspect ratio. At the same time, the ingots are constrained by the maximum mutual restraining force, and are not easy to separate during the upsetting process. In addition, a method of pre-punching the center hole is introduced to reduce the deformation dead zone and avoid the occurrence of deformation instability. Specifically, an embodiment of the present invention discloses a method for upsetting large aspect ratio aluminum alloy round ingots, comprising the following steps:
[0031] S1) heating an aluminum alloy round ingot, wherein the round cross section of the aluminum alloy ingot has a concave cutout;
[0032] S2) arranging the aluminum alloy ingots obtained in the three steps S1) in a manner of maximizing the cross-sectional area to obtain a combined ingot;
[0033] S3) pre-punching a hole at the center of the end surface of the combined ingot;
[0034] S4) upsetting the ingot obtained in step S3);
[0035] The concave structure minimizes the surface area to maximize the cross-sectional area of the composite ingot.
[0036] The method for upsetting an aluminum alloy round ingot provided in the present application specifically comprises the following steps in sequence: aluminum alloy round ingot processing - flat anvil heating - ingot heating - ingot transfer - pre-punching - upsetting.
[0037] In a specific embodiment, the present application firstly processes the aluminum alloy round ingot so that the circular cross section of the aluminum alloy round ingot has a concave cutout. The specific structural schematic diagram is shown in FIG. Figure 1 As shown, Figure 1Where 1 is the width of the concave cut, and 2 is the depth of the concave cut, that is, there is a concave cut on each cross section of the aluminum alloy round ingot, and the concave cut needs to satisfy the aluminum alloy round ingot and have the maximum contact area with the adjacent ingot under the premise of the minimum cutting amount. The radius of the aluminum alloy round ingot is set to R, the width of the concave cut is R±10mm, and the depth of the concave cut is 0.134R±10mm; specifically, the width of the concave cut is Rmm, R+1mm, R+2mm, R+3mm, R+4mm, R+5mm, R+6mm, R+7mm, R+8mm, R+9mm, R+10mm, R-1mm, R-2mm, R-3mm, R-4mm, R-5mm, R-6mm, R-7mm, R-8mm, R-9mm, R-10mm, and the depth of the concave cut is 0.134Rmm, 0.134R+1mm m, 0.134R+2mm, 0.134R+3mm, 0.134R+4mm, 0.134R+5mm, 0.134R+6mm, 0.134R+7mm, 0.134R+8mm, 0.134R+9mm, 0.134R+10mm, 0.13 4R-1mm, 0.134R-2mm, 0.134R-3mm, 0.134R-4mm, 0.134R-5mm, 0.134R-6mm, 0.134R-7mm, 0.134R-8mm, 0.134R-9mm, 0.134R-10mm.
[0038] The present application then heats the aluminum alloy round ingot and heats the flat anvil; the temperature of the aluminum alloy heating is 400~550℃, and the insulation time is 10~30h. Specifically, the temperature of the aluminum alloy heating is 420~510℃, and the insulation time is 12~25h. More specifically, the temperature of the aluminum alloy heating is 450~500℃, and the insulation time is 15~20h. The temperature of the flat anvil heating is 400~500℃, and the insulation time is 10~30h. Specifically, the temperature of the flat anvil heating is 420~510℃, and the insulation time is 12~25h. More specifically, the temperature of the flat anvil heating is 450~500℃, and the insulation time is 15~20h. The aluminum alloy round ingot is heated to prepare for the later pre-punching and upsetting, which is beneficial to improve the uniformity of the structure. The flat anvil is heated to avoid heat loss of the ingot.
[0039] The present application then transfers the heated aluminum alloy round ingots to the forging platform, and selects three aluminum alloy round ingots of the same specifications, and arranges them in a way that maximizes the cross-sectional area of the ingots to ensure the uniformity of the interaction forces between different ingots. Specifically, the schematic diagram of the arrangement of the aluminum alloy round ingots of the present application is as follows: Figure 2As shown, the three aluminum alloy round ingots are in close contact in the longitudinal direction, and there is no gap at the contact position, forming an intersecting contact mode with the largest cross-sectional area, thereby obtaining a combined ingot.
[0040] According to the present invention, a pre-punching hole is then performed at the center of the end face of the combined ingot. The schematic diagram of the positions of the combined ingot, the punch and the flat anvil is shown in FIG. Figure 3 The cross-sectional diagram is shown in Figure 4 As shown, Figure 3 3 is a flat anvil, 4 is a punch, and 5 is a combined ingot; the pre-punching can reduce the deformation dead zone area of the contact part between the ingot and the flat anvil, thereby preventing "bulging" from occurring too early in the initial stage of upsetting and causing deformation instability. The diameter of the pre-punching hole is 200-300mm, and the depth of the pre-punching hole is 50-80mm. Specifically, the diameter of the pre-punching hole is 220-280mm, and the depth of the pre-punching hole is 55-75mm. More specifically, the diameter of the pre-punching hole is 200mm, 210mm, 220mm, 230mm, 240mm, 250mm, 260mm, 270mm, 280mm, 290mm or 300mm, and the depth of the pre-punching hole is 50mm, 51mm, 52mm, 53mm, 54mm, 55mm, 56mm, 57mm, 58mm, 59mm, 60mm, 61mm, 62mm, 63mm, 64mm, 65mm, 66mm, 67mm, 68mm, 69mm, 70mm, 71mm, 72mm, 73mm, 74mm or 75mm. If the diameter and depth of the pre-punched hole are too small, the anti-bulging effect will be weakened; if the diameter is too large, the restraining force between the ingots will be reduced; if the depth is too large, folding will be easily generated.
[0041] In this application, the ingot is finally upset, as shown in the schematic diagram Figure 5 As shown, the upsetting rate does not exceed 10 mm / s to ensure the uniformity of the upsetting deformation; specifically, the upsetting rate is 1-10 mm / s, more specifically, the upsetting rate is 2 mm / s, 3 mm / s, 4 mm / s, 5 mm / s, 6 mm / s, 7 mm / s, 8 mm / s, 9 mm / s or 10 mm / s.
[0042] The upsetting method of the aluminum alloy round ingot with a large aspect ratio provided in the present application is suitable for aluminum alloy round ingots with an aspect ratio greater than 3.5. In a specific embodiment, the aspect ratio is specifically 4.0 to 5.0. The upsetting method is mainly for aluminum alloy round ingots with high alloy content, such as 2 series aluminum alloy or 7 series aluminum alloy. More specifically, the aluminum alloy round ingot includes 7050 aluminum alloy round ingot, 2219 aluminum alloy round ingot, 7075 aluminum alloy round ingot, 7055 aluminum alloy round ingot, 7085 aluminum alloy round ingot, 2A14 aluminum alloy round ingot, 2195 aluminum alloy round ingot or 2050 aluminum alloy round ingot.
[0043] The upsetting method for large aspect ratio aluminum alloy round ingots provided in the present application is compared with other large aspect ratio upsetting schemes: upsetting of large aspect ratio round ingots is achieved without adding additional molds, and there is no need to open a separate mold for each ingot specification, which has universality and reduces costs; multiple ingots are upset at the same time, which improves efficiency; compared with the use of large diameter ingots: the small specification ingots used in the present invention avoid the chemical composition segregation, coarse structure and other undesirable metallurgical structures that are easily produced by large diameter ingots, and have better structure and performance.
[0044] In order to further understand the present invention, the upsetting method of the aluminum alloy round ingot with a large aspect ratio provided by the present invention is described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments. Example 1
[0045] A method for upsetting a 7050 aluminum alloy round ingot with a large aspect ratio, wherein the ingot specification is Φ600*3000mm, comprises the following steps:
[0046] Step 1: Place the ingots according to Figure 1 A certain amount of metal is removed in this way, with a removal width of 300mm and a removal depth of 40mm;
[0047] Step 2: Heat the flat anvil to 450°C and keep it warm for 18 hours;
[0048] Step 3: Heat the ingot to 440°C and keep it warm for 15 hours;
[0049] Step 4: Transfer the ingots to the forging platform, select 3 ingots of the same specifications, and arrange them in a way that the ingots are in close contact and have the largest cross-sectional area, such as Figure 2 As shown, to ensure the uniformity of the interaction force between different ingots;
[0050] Step 5: Place the punch and anvil in sequence at the center of the end face of the combined ingot, such as Figure 3 As shown, pre-punching is performed, the punching diameter is 280mm, the depth is 70mm, and the cross-sectional area of the center pre-punching hole is as follows Figure 4 As shown;
[0051] Step 6: Use low speed upsetting. The upsetting diagram is as follows: Figure 5 As shown, the upsetting rate is 8 mm / s to ensure uniform deformation, and the upsetting is performed to an ingot height of 1500 mm. Example 2
[0052] A method for upsetting a 2219 aluminum alloy round ingot with a large aspect ratio, wherein the ingot specification is Φ448*2200mm, comprises the following steps:
[0053] Step 1: Place the ingots according to Figure 1A certain amount of metal is removed in this way, with a removal width of 224mm and a removal depth of 30mm;
[0054] Step 2: Heat the flat anvil to 470°C and keep it warm for 18 hours;
[0055] Step 3: Heat the ingot to 480°C and keep it warm for 12 hours;
[0056] Step 4: Transfer the ingots to the forging platform, select 3 ingots of the same specifications, and arrange them in a way that the ingots are in close contact and have the largest cross-sectional area, such as Figure 2 As shown, the uniformity of the interaction force between different ingots is ensured;
[0057] Step 5: Place the punch and anvil in sequence at the center of the end face of the combined ingot, such as Figure 3 As shown, pre-punching is performed, the punching diameter is 210mm and the depth is 60mm;
[0058] Step 6: Use low-speed upsetting with an upsetting rate of 5 mm / s to ensure uniform deformation and upsetting to an ingot height of 1100 mm. Comparative Example 1
[0059] A conventional 7050 aluminum alloy round ingot upsetting method, the ingot specification is Φ830*1600mm, comprising the following steps:
[0060] Step 1: Heat the flat anvil to 450°C and keep it warm for 18 hours;
[0061] Step 2: Heat the ingot to 440°C and keep it warm for 20 hours;
[0062] Step 3: Transfer the ingot to the forging platform;
[0063] Step 4: Upsetting rate 12mm / s, upsetting to ingot height 800mm.
[0064] The round ingots of the above embodiments did not show any instability during the forging process, thus achieving the upsetting of the round ingots with a large aspect ratio.
[0065] Compared with conventional upsetting of Φ830mm ingot ( Figure 7 ), the present invention adopts Φ600mm ingot with large aspect ratio upsetting ( Figure 6 ), the grain structure is finer, and there is no aggregation of chain-like coarse compounds, with a better microstructure.
[0066] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0067] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention shall not be limited to the embodiments shown herein, but shall be consistent with the principles and novelties disclosed herein.
[0068] The widest range of consistent characteristics.
Claims
1. A method for upsetting a round aluminum alloy ingot with a large aspect ratio, comprising the following steps: S1) heating an aluminum alloy round ingot, wherein the round cross section of the aluminum alloy ingot has a concave cutout; S2) The aluminum alloy ingots of the same specification obtained in the three steps S1) are closely contacted in the longitudinal direction and intersect at one point, with no gap at the contact part, forming an intersecting contact mode with the largest cross-sectional area, to obtain a combined ingot; S3) pre-punching a hole at the center of the end surface of the combined ingot; S4) upsetting the ingot obtained in step S3); The surface area of the concave cutout is minimized to maximize the cross-sectional area of the combined ingot; The radius of the aluminum alloy round ingot is set to R, the width of the concave cut is R±10 mm, the depth of the concave cut is 0.134R±10 mm; the edge of the concave cut is an arc; The diameter of the pre-punched hole is 200-300 mm, and the depth of the pre-punched hole is 50-80 mm.
2. The upsetting method according to claim 1, characterized in that: The heating temperature is 400-550° C., and the insulation time is 10-30 hours.
3. The upsetting method according to claim 1, characterized in that: The method further includes flat anvil heating before the pre-punching, wherein the flat anvil heating temperature is 400-500° C. and the heat preservation time is 10-30 hours.
4. The upsetting method according to claim 3, characterized in that: During the pre-punching process, the aluminum alloy round ingot, the punch and the flat anvil are placed in sequence.
5. The upsetting method according to claim 1, characterized in that: The upsetting rate does not exceed 10 mm / s.
6. The upsetting method according to claim 1 or 5, characterized in that: The upsetting rate is 5-8 mm / s.
7. The upsetting method according to any one of claims 1 to 5, characterized in that: The aluminum alloy round ingot has a height-to-diameter ratio greater than 3.
5.
8. The upsetting method according to any one of claims 1 to 5, characterized in that: The aluminum alloy round ingots include 7050 aluminum alloy round ingots, 2219 aluminum alloy round ingots, 7075 aluminum alloy round ingots, 7055 aluminum alloy round ingots, 7085 aluminum alloy round ingots, 2A14 aluminum alloy round ingots, 2195 aluminum alloy round ingots or 2050 aluminum alloy round ingots.
Citation Information
Patent Citations
Free-forging shortening method and anvil at ultralimit aspect ratio
CN101491822A
Wind power flange half die forging process
CN111992649A
Process method for upsetting steel ingot with ultra-large height-diameter ratio in limited space
CN114700453A
Upsetting method for continuous casting billet with height-diameter ratio larger than 3
CN117531943A
Upsetting method of long size stock
JP1996332544A