Spiral polycrystalline diamond composite round rod and preparation method and application thereof

By forming a spiral polycrystalline diamond composite round rod on a carbide round rod matrix, combined with carbon nanotubes, graphene and other materials, the problem of insufficient wear resistance of fiber-reinforced composite hole-making tools is solved, and efficient preparation and Improved wear resistance, suitable for drilling of fiber-reinforced composite materials.

CN118357467BActive Publication Date: 2024-10-11CY CARBIDE MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410790924.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

In the existing technology, fiber-reinforced composite hole-making tools have insufficient anti-wear properties during processing, resulting in wear and blunting of the cutting edge. Moreover, the preparation method of polycrystalline diamond composite sheets has limitations in groove processing and the welding position is close to the cutting. The blade is prone to failure due to heat.

Method used

A carbide round rod matrix is ​​used, and a transition layer and a spiral polycrystalline diamond layer are deposited on the surface of the spiral groove extending along the axial direction of the round rod. The spiral polycrystalline diamond composite round rod is formed through high-pressure and high-temperature sintering, combining carbon nanotubes, graphene, and rich Lerene is coated with materials such as diamond powder to enhance wear resistance and bonding strength, and the tool is fixed to the handle through brazing.

Benefits of technology

It achieves efficient preparation of cutting tools, reduces the impact of the brazing process on the cutting tools, improves the wear resistance, thermal stability and bonding strength of the cutting tools, is suitable for drilling processing of fiber-reinforced composite materials, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118357467B_ABST
    Figure CN118357467B_ABST
Patent Text Reader

Abstract

The present invention discloses a spiral polycrystalline diamond composite round rod and its preparation method and application. A spiral polycrystalline diamond layer is formed on the surface of the round rod by a pressing process, diamond and cemented carbide are sintered into one under high temperature and high pressure conditions, and then the sintered tool blank is welded to the handle by brazing. Since the polycrystalline diamond layer has been attached to the surface of the spiral groove in a spiral shape in advance, the position of the blade can be accurately located, and the required spiral tool blade shape can be directly and accurately processed along the spiral surface of the composite round rod, greatly reducing the difficulty of preparing the tool. The present invention is prepared using raw materials such as carbon nanotubes, graphene, and fullerene-coated diamond powder, and has the dual characteristics of diamond and reinforcing materials such as carbon nanotubes, graphene, and fullerene, so that the polycrystalline diamond composite round rod has high wear resistance, thermal stability, and bonding strength, and is particularly suitable for preparing hole-making tools.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of a cemented carbide matrix composite material, in particular to a spiral polycrystalline diamond composite round rod and a preparation method and application thereof. Background Art

[0002] With the rapid development of aviation, aerospace and military equipment, fiber-reinforced composite materials have been widely used in industrial production and daily life. However, as the performance of composite materials continues to improve, the cutting ability of materials is getting worse and worse. Long-term cutting work will aggravate the wear of the tool, thereby affecting the processing accuracy and efficiency of the tool.

[0003] At present, the hole-making tool material used for processing fiber-reinforced composite materials is mainly cemented carbide, but this type of hole-making tool has insufficient wear resistance in the process of fiber-reinforced composite hole-making, and the cutting edge is easily worn and passivated, resulting in a decrease in hole-making quality. In order to solve the problem of wear and passivation of the cutting edge of cemented carbide hole-making tools, people have used various methods to improve the wear resistance of hole-making tools, including enhancing the strength of the cemented carbide body, adding wear-resistant coatings on the cutting edge of cemented carbide hole-making tools, etc., but the improvement is limited.

[0004] There is another processing idea in the prior art, which is to change the material of the hole-making tool and use polycrystalline diamond as the cutting edge. The preparation of polycrystalline diamond hole-making tools generally involves opening a prefabricated groove on the surface of a cemented carbide substrate, and fixing the cut polycrystalline diamond composite sheet in the prefabricated groove by brazing. This type of preparation method has two major disadvantages: 1. The tool groove processing is limited, because the polycrystalline diamond composite sheet is a flat sheet, and it is difficult to process a uniform spiral edge; 2. The welding position of the polycrystalline diamond composite sheet is located on the cemented carbide substrate groove welding head very close to the cutting edge. If the processing temperature is close to the melting point of the brazing material, the heat generated during processing will cause the weld joint to fail.

[0005] Therefore, it is necessary to improve the preparation process of the hole-making tool in the prior art to reduce the impact of the brazing process on the hole-making tool. Summary of the invention

[0006] The object of the present invention is to provide a spiral polycrystalline diamond composite round rod, comprising a cemented carbide round rod substrate, at least one spiral groove surrounding the round rod substrate and extending along the axial direction of the round rod substrate, and a transition layer and a spiral polycrystalline diamond layer sequentially arranged on the surface of the spiral groove, wherein the transition layer is located between the spiral groove and the spiral polycrystalline diamond layer;

[0007] The transition layer is a transition layer deposited on the surface of the spiral groove; the spiral polycrystalline diamond layer is composed of superhard powder and a binder, which is mixed and stirred, loaded into the spiral groove after the transition layer is deposited, pre-pressed and shaped, and then sintered under high pressure of 7-9GPa and high temperature of 1400-1600℃;

[0008] The particle size of the superhard powder is not higher than 40µm, and its composition is 45-65% by mass of carbon nanotube coated diamond powder containing boron, 20-25% by mass of plated cubic boron nitride powder, 5-10% by mass of fullerene coated diamond powder containing boron, 5-10% by mass of graphene coated diamond powder containing boron and 5-10% by mass of a binder.

[0009] Furthermore, the transition layer is 6-8 μm and is deposited from one or more of niobium nitride, gallium nitride, lithium nitride, silicon nitride, titanium nitride, and chromium nitride.

[0010] Furthermore, the spiral groove is subjected to surface decobalting treatment before the transition layer is deposited, the depth of the decobalting layer is 50-60 μm, and the cobalt content of the decobalting layer is 1.8-2.2%.

[0011] Furthermore, the composition of the round rod matrix is ​​89.5-91% by mass of WC powder, 0.25-0.5% of fullerene powder, 0.5-1.0% of the total amount of fullerene powder and graphyne powder, and 8.5-9.5% of Co powder; the particle size of the WC powder is 0.8-1.2µm, the particle size of the fullerene powder and graphyne powder is 0.4-0.5µm, and the particle size of the Co powder is 0.4-0.6µm.

[0012] Furthermore, the boron content of the boron-containing diamond micropowder is 0.0005-0.012%; and the coating of the cubic boron nitride micropowder is one of a titanium-chromium alloy and a titanium-nickel alloy.

[0013] Furthermore, the binder is composed of the following raw materials in percentage by weight: Co powder 99-99.5%, Li powder 0.15-0.25%, Hf powder 0.10-0.30%, Ta powder 0.1-0.15%, Si powder 0.1-0.15%, and VC powder 0.05-0.15%.

[0014] The present invention further provides a method for preparing the spiral composite round rod, comprising the following steps:

[0015] S1. Decobalting the spiral groove surface of the round rod substrate: at least one spiral groove is formed on the round rod substrate, and the spiral groove surface of the alloy round rod substrate is etched with an acid pickling solution until the cobalt content is 1.8-2.2%, and the acid residue on the spiral groove surface is washed with deionized water to obtain a round rod substrate with decobalted spiral groove surface;

[0016] S2. Depositing a transition layer on the surface of the spiral groove: depositing a transition layer on the surface of the spiral groove after decobalting, the depth of the decobalting layer is 50-60 μm, and the cobalt content of the decobalting layer is 1.8-2.2%;

[0017] S3, spiral polycrystalline diamond layer mixing: weigh a certain amount of superhard powder and a binder, dissolve them in an isopropanol solution and stir them thoroughly in a stirring container; then transfer the stirred materials to a ball mill, add a ball milling medium and grind them repeatedly for 24-30 hours; vacuum dry them after grinding, and finally obtain a uniform spiral polycrystalline diamond layer mixed powder;

[0018] The superhard powder is one or more of carbon nanotube coated boron-containing diamond powder, plated cubic boron nitride powder, fullerene coated boron-containing diamond powder, graphene coated boron-containing diamond powder, titanium-coated diamond powder, and tungsten-coated diamond powder.

[0019] S4, spiral composite assembly: the spiral polycrystalline diamond layer mixed powder obtained in S3 is loaded into the spiral groove of the carbide round rod after the transition layer is deposited in S2, compacted and shaped, and then inserted into a high-temperature resistant metal cup to obtain a spiral composite assembly;

[0020] S5, pre-pressing the spiral composite body: placing the spiral composite body component of S4 into a pre-pressing rubber mold, and maintaining the pressure at 120-150 MPa, thereby obtaining a pre-pressed spiral composite body component;

[0021] S6, furnace purification: the pre-pressed spiral composite assembly is placed in a vacuum sintering furnace, the furnace is roughly vacuumed, and the temperature is kept at 160-200°C for 1 hour; the vacuum is continued and heated to 850-900°C, hydrogen is filled into the furnace under vacuum conditions until the pressure in the furnace reaches 110-130Mbar, and the furnace is reacted for 4-6 hours before vacuuming again;

[0022] S7, high temperature and high pressure sintering: assemble the purified spiral composite assembly with the pyrophyllite assembly block, place it in a top press, keep it at a high pressure of 7-9 GPa and a high temperature of 1400-1600°C for 20-30 minutes, stop heating and slowly reduce to normal pressure to obtain a sintered spiral polycrystalline diamond composite round rod blank;

[0023] S8, stress relief aging: Place the sintered spiral polycrystalline diamond composite round rod blank in a vacuum sintering furnace, heat it to 480-500°C under vacuum conditions and keep it warm for 7-8 hours; evacuate the vacuum again, keep it warm at 580-600°C for 3-4 hours, and naturally cool it to room temperature to obtain the required polycrystalline diamond composite round rod.

[0024] Furthermore, in step S2, the transition layer is deposited by physical vapor deposition, with niobium as the target, the round rod substrate is heated to 800° C. in a nitrogen atmosphere, and sputtering etching is performed at a power of 300 W and a frequency of 120 kHz.

[0025] The present invention forms a spiral polycrystalline diamond layer on the surface of a round rod through a pressing process, sintering diamond and cemented carbide into one under high temperature and high pressure conditions, and then brazing the sintered tool blank to the handle. Since the polycrystalline diamond layer has been pre-attached to the spiral groove surface in a spiral shape, the position of the blade can be accurately located, and the required spiral tool blade shape can be directly and accurately processed along the spiral surface of the composite round rod, which greatly reduces the difficulty of preparing the tool, and the prepared tool will not cause the polycrystalline diamond layer to fail due to brazing problems.

[0026] The present invention also specifically discloses the composition, preparation process and process parameters of the above-mentioned polycrystalline diamond composite round rod, which is prepared using raw materials such as carbon nanotubes, graphene, and fullerene-coated diamond micropowder, and has the dual characteristics of basic materials such as diamond and CBN and reinforcing materials such as carbon nanotubes, graphene, and fullerene, so that the polycrystalline diamond composite round rod has higher wear resistance, thermal stability and bonding strength. The tool prepared from the composite round rod is particularly suitable for drilling processing of fiber-reinforced composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic structural diagram of the spiral polycrystalline diamond composite round rod of the present invention;

[0028] Figure 2 It is a physical schematic diagram of the spiral polycrystalline diamond composite round rod of the present invention;

[0029] Figure 3 The schematic diagram of the cutter head is made from the spiral polycrystalline diamond composite round rod of the present invention. DETAILED DESCRIPTION

[0030] Example 1: Figure 1 and Figure 2 The spiral polycrystalline diamond composite round rod shown includes a carbide round rod substrate, at least one spiral groove surrounding the round rod substrate and extending axially along the round rod substrate, and a transition layer and a spiral polycrystalline diamond layer sequentially arranged on the surface of the spiral groove, wherein the transition layer is located between the spiral groove and the spiral polycrystalline diamond layer.

[0031] In this embodiment, a central through hole is provided on the central axis of the round rod base, and a plurality of spiral grooves are opened on the surface of the round rod base. The number of the spiral grooves can be set to two, three, four or more, and the ends thereof are evenly arranged in the circumferential direction of the head of the round rod base. The cross-sections of the spiral grooves and the spiral polycrystalline diamond layer can be set to U-shape, trapezoidal, semicircular, rectangular and other shapes according to specific needs.

[0032] The transition layer is 6-8 μm and is deposited on the surface of the spiral groove by one or more of niobium nitride, gallium nitride, lithium nitride, silicon nitride, titanium nitride, chromium nitride, etc. The transition layer can reduce the interface stress between the polycrystalline diamond layer and the cemented carbide round rod substrate, thereby improving the bonding strength between the spiral polycrystalline diamond layer and the cemented carbide.

[0033] The polycrystalline diamond layer is composed of superhard powder and a binder, which is mixed and stirred, loaded into the spiral groove after the deposition of the transition layer and pressed and shaped at high temperature to obtain a spiral composite component, which is then formed and fixed through a sintering process under high temperature and high pressure conditions.

[0034] Among them, the particle size of the superhard powder is not higher than 40µm, and its composition is one or more of carbon nanotube-coated boron-containing diamond powder, plated cubic boron nitride powder, fullerene-coated boron-containing diamond powder, graphene-coated boron-containing diamond powder, titanium-coated diamond powder, titanium-coated diamond powder, and tungsten-coated diamond powder. The formed composite round rod has the composite properties of matrix materials such as diamond and cubic boron nitride and reinforcing materials such as carbon nanotubes, graphene, and fullerene.

[0035] The present invention deposits a niobium nitride transition layer on the surface of the spiral groove of the round rod substrate, and obtains a spiral polycrystalline diamond layer by pressing and sintering superhard powder in the spiral groove, so that the position of the cutting edge can be accurately located during the subsequent processing of the tool.

[0036] Furthermore, the surface of the spiral groove is first pickled to form a decobaltized layer before the transition layer is deposited, so as to enhance the adhesion between the round rod substrate deposited with the transition layer and the polycrystalline diamond layer.

[0037] The raw material components of the superhard powder in this embodiment include 45-65% carbon nanotube-coated boron-containing diamond micropowder, 20-25% plated cubic boron nitride micropowder, 5-10% fullerene-coated boron-containing diamond micropowder, 5-10% graphene-coated boron-containing diamond micropowder and 5-10% binder; the boron content of the boron-containing diamond micropowder is 0.0005-0.012%; the coating of the plated cubic boron nitride micropowder is one of titanium-chromium alloy and titanium-nickel alloy.

[0038] The binder is composed of the following raw materials in percentage by weight: Co powder 99-99.5%, Li powder 0.15-0.25%, Hf powder 0.10-0.30%, Ta powder 0.1-0.15%, Si powder 0.1-0.15%, and VC powder 0.05-0.15%.

[0039] In this embodiment, five groups of round rod substrates made of cemented carbide are selected, and the round rod substrates are sintered by the following raw materials in weight percentage: 89.5-91% tungsten carbide powder, 0.5-1.0% total of fullerene powder and graphyne powder, and 8.5-9.5% Co powder; the selected tungsten carbide powder particle size is 0.8-1.2µm, the fullerene powder and graphyne powder particle size is 0.4-0.5µm, and the cobalt powder particle size is 0.4-0.6µm.

[0040] The mass ratios of the components of the five groups of round rod matrices are shown in the following table:

[0041]

[0042] The polycrystalline diamond composite round rods were prepared according to the following processes:

[0043] S1. Decobalting the spiral groove surface of the round rod substrate: The spiral groove surface of the alloy round rod substrate was etched with a nitric acid solution with a volume ratio of 2:5 for 40-50 minutes, and the acid residue on the spiral groove surface was rinsed with deionized water to obtain a cemented carbide substrate with decobalted spiral groove surface. The depth of the decobalted layer was measured to be 50-60μm, and the cobalt content of the decobaltized layer was 1.8-2.2%.

[0044] S2. Deposition of transition layer on the surface of spiral groove: Physical vapor deposition is used to deposit niobium carbide on the surface of spiral groove of cemented carbide round rod after decobalting. Specifically, niobium is used as target material, the round rod substrate is heated to 800°C in nitrogen atmosphere, and sputtering etching is performed under the conditions of power 300W and frequency 120kHz. Finally, a cemented carbide round rod with a transition layer deposited on the surface of spiral groove is obtained, and the thickness of the transition layer is measured to be 6-8µm.

[0045] S3. Spiral polycrystalline diamond layer mixing: weigh the raw materials of the spiral polycrystalline diamond layer according to the above ratio, dissolve them in isopropanol solution and pour them into a stirring container, stir mechanically for 20-30 minutes; then transfer the stirred materials to a ball mill, add medium and grind repeatedly. Maintain the grinding speed of 25-30r / min for 24-30h, repeatedly change the grinding direction during the grinding process to fully mix the materials in the ball mill; then transfer the mixed materials to an oven, vacuum dry them at 100-120℃ for 1.5-2h, and finally obtain a uniform spiral polycrystalline diamond layer mixed powder.

[0046] The spiral polycrystalline diamond layers of the five sets of composite round rods are made of superhard powder and binder, and the specific composition quality ratio is as follows:

[0047]

[0048] S4, spiral composite assembly: the spiral polycrystalline diamond layer mixed powder obtained in S3 is loaded into the spiral groove of the hard alloy round rod after the transition layer is deposited in S2, compacted and shaped, and then inserted into a high temperature resistant metal cup to obtain a spiral composite assembly;

[0049] S5, pre-pressing of spiral composite body: placing the spiral composite body component of S4 into a pre-pressing rubber mold, and placing the pre-pressing rubber mold into an isostatic pressing device, and maintaining the pressure at 120-150 MPa for 60-90 seconds, thereby obtaining a pre-pressed spiral composite body component;

[0050] S6. Purification in the furnace: Place the pre-pressed spiral composite assembly in a vacuum sintering furnace and roughly pump the furnace pressure to 6×10 -2 Pa, keep warm at 160-200℃ for 1h; continue to evacuate and heat to 850-900℃, fill the furnace with reducing gas hydrogen until the pressure in the furnace reaches 110-130Mbar, and evacuate again after 4-6h of reduction reaction;

[0051] S7, high temperature and high pressure sintering: assemble the purified spiral composite assembly with the pyrophyllite assembly block, place it in a six-sided top press, apply a pressure of 7-9GPa while raising the temperature to 1400℃-1600℃ and maintain it for 20-30min, then disconnect the current to stop heating, and slowly reduce the pressure to normal pressure to obtain a sintered spiral polycrystalline diamond composite round rod blank;

[0052] S8, stress relief aging: Place the sintered spiral polycrystalline diamond composite round rod blank in a vacuum sintering furnace, heat it to 480-500°C under vacuum conditions and keep it warm for 7-8 hours; evacuate the vacuum again, heat it to 580-600°C and keep it warm for 3-4 hours, and then cool it naturally to room temperature to obtain the required polycrystalline diamond composite round rod.

[0053] Example 2: The polycrystalline diamond layers of the five groups of composite round rods in this example comprise the following components in weight ratio: 25-30% of carbon nanotube-coated diamond powder containing boron, 40-60% of plated cubic boron nitride powder, 5-10% of fullerene-coated diamond powder containing boron, 5-10% of graphene-coated diamond powder containing boron and 5-10% of binder; the boron content of the boron-containing diamond powder is 0.0005-0.012%; the coating of the plated cubic boron nitride powder is one of titanium-chromium alloy and titanium-nickel alloy. Polycrystalline diamond composite round rods are prepared by the same process as in Example 1.

[0054] The specific composition quality ratio is as follows:

[0055]

[0056] Comparative Example 1: The components of the three groups of polycrystalline diamond layers are the same as those of Example 1, but no fullerene powder or graphyne powder is added to the components of the round rod substrate. The specific mass proportions of the components of the round rod substrate are as follows:

[0057]

[0058] Comparative Example 2: The components of the two groups of round rod substrates are the same as those of Example 1, but the diamond powder in the polycrystalline diamond layer does not contain boron.

[0059] The specific composition quality ratio is as follows:

[0060]

[0061] The properties of 15 groups of polycrystalline diamond composite round rods in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were tested according to the following method:

[0062] Heat resistance: Place the composite round bar sample in a vacuum welding machine and heat it to the target temperature of 600°C. Take it out and observe whether there are visible cracks or damage on the surface of the round bar. Place the round bar sample in the vacuum welding machine again and gradually increase the target temperature by 10°C until cracks are observed on the surface of the sample. Record the target temperature at this time as the heat resistance temperature of the composite round bar sample.

[0063] Impact toughness: Place each group of samples in a drop hammer impact tester and impact the samples with an energy of 40J / time, and record the energy obtained by the samples before the spiral diamond polycrystalline layer breaks and falls off;

[0064] Wear resistance test: The test is carried out in accordance with the standard "JB / T 3235-2013 Polycrystalline diamond wear ratio test method".

[0065] The performance test results of 15 groups of composite round bars are as follows:

[0066]

[0067] Then, the 15 groups of polycrystalline diamond composite round rods are prepared as follows: Figure 3 The spiral milling cutters of the same specifications shown are used to test the performance of the target hole-making tools.

[0068] Service life: Drilling test was carried out on a CNC drilling and milling machine with a carbon fiber composite plate as the workpiece. The test speed was controlled at 9000r / min and the feed speed was 30mm / min. The tool life was determined based on the exit quality, dimensional accuracy and blade wear of the processed hole. When the flank wear Vb=0.5mm was reached, the processing was stopped and the number of qualified holes that had been processed was counted.

[0069]

[0070] It can be seen from the data in the table that the composite round rods 1-13 provided by Example 1, Example 2 and Comparative Example 1 all have high heat resistance, and the heat resistance temperature of the composite round rods 1-13 all reaches above 880°C, which is unattainable by the brazing process in the prior art. In Example 2, due to the addition of more CBN micropowder components, its wear resistance is reduced compared with diamond micropowder, while the composite round rods provided by the examples have excellent indicators and can meet the processing requirements of hole-making tools in the prior art.

[0071] Compared with Example 1, Comparative Example 1 uses a conventional round rod matrix component and does not contain graphyne and fullerene. Although there is a transition layer between the polycrystalline diamond layer and the round rod matrix, the bonding effect between the polycrystalline diamond layer and the round rod matrix is ​​not ideal, which directly affects the impact toughness of the composite round rod. The impact toughness of the composite round rods 11-13 is much lower than that of the composite round rods 1-10.

[0072] In Comparative Example 2, no boron element is added to the diamond powder, which affects the heat resistance of the composite round rod. The heat resistance temperature of the composite round rods 14-15 is only 750° C., which does not reflect the difference with the prior art.

[0073] The tool 1-10 prepared from the composite round rod 1-10 processed more than 300 qualified holes before the back cutting surface was worn, which can meet the requirements of the existing technology, and the tool 1-5 even reached 350 qualified holes, indicating that the tool prepared according to the parameters of Example 1 not only has higher processing accuracy, but also has a longer service life.

[0074] Comparative Example 3: A polycrystalline diamond flat sheet is prepared with a matrix, transition layer and polycrystalline diamond layer of the same composition as the composite round rod 1, and then attached to the round rod matrix by brazing to prepare a composite round rod and a hole-making tool is prepared based on the composite round rod. The composite round rod of Comparative Example 3 was subjected to a heat resistance test. Due to the limitation of the brazing material, the round rod can only work stably under temperature conditions below 700°C. When the working temperature is between 700-800°C, cracks begin to appear at the brazing position on the surface of the composite round rod, and even fall off in severe cases. At the same time, in the process of machining the hole-making tool, it is difficult to machine an ideal spiral groove on the surface of the polycrystalline diamond layer.

[0075] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. Spiral polycrystalline diamond composite round rod, characterized by: It comprises a carbide round rod substrate, at least one spiral groove surrounding the round rod substrate and extending along the axial direction of the round rod substrate, and a transition layer and a spiral polycrystalline diamond layer sequentially arranged on the surface of the spiral groove, wherein the transition layer is located between the spiral groove and the spiral polycrystalline diamond layer; The transition layer is a transition layer deposited on the surface of the spiral groove; the spiral polycrystalline diamond layer is composed of superhard powder and a binder, which is mixed and stirred, loaded into the spiral groove after the transition layer is deposited, pre-pressed and shaped, and then sintered under high pressure of 7-9GPa and high temperature of 1400-1600℃; The particle size of the superhard powder is not higher than 40µm, and the composition thereof is 45-65% by mass of carbon nanotube-coated diamond powder containing boron, 20-25% by mass of plated cubic boron nitride powder, 5-10% by mass of fullerene-coated diamond powder containing boron, 5-10% by mass of graphene-coated diamond powder containing boron and 5-10% by mass of a binder; The binder is composed of the following raw materials in percentage by weight: Co powder 99-99.5%, Li powder 0.15-0.25%, Hf powder 0.10-0.30%, Ta powder 0.1-0.15%, Si powder 0.1-0.15%, and VC powder 0.05-0.15%.

2. The spiral polycrystalline diamond composite round rod according to claim 1, characterized in that: The transition layer is 6-8 μm thick and is deposited from one or more of niobium nitride, gallium nitride, lithium nitride, silicon nitride, titanium nitride, and chromium nitride.

3. The spiral polycrystalline diamond composite round rod according to claim 1, characterized in that: The spiral groove is subjected to surface decobalting treatment before the transition layer is deposited. The depth of the decobalting layer is 50-60 μm and the cobalt content of the decobalting layer is 1.8-2.2%.

4. The spiral polycrystalline diamond composite round rod according to claim 1, characterized in that: The composition of the round rod matrix is ​​89.5-91% by mass of WC powder, 0.5-1.0% of the total amount of fullerene powder and graphyne powder, and 8.5-9.5% of Co powder; the particle size of the WC powder is 0.8-1.2µm, the particle size of the fullerene powder and graphyne powder is 0.4-0.5µm, and the particle size of the Co powder is 0.4-0.6µm.

5. The spiral polycrystalline diamond composite round rod according to claim 1, characterized in that: The boron content of the boron-containing diamond micropowder is 0.0005-0.012%; the coating of the plated cubic boron nitride micropowder is one of a titanium-chromium alloy and a titanium-nickel alloy.

6. The method for preparing a spiral polycrystalline diamond composite round rod according to any one of claims 1 to 5, characterized in that: The steps include: S1. Decobalting the spiral groove surface of the round rod substrate: at least one spiral groove is formed on the round rod substrate, and the spiral groove surface of the alloy round rod substrate is etched with an acid pickling solution until the cobalt content is 1.8-2.2%, and the acid residue on the spiral groove surface is washed with deionized water to obtain a round rod substrate with decobalted spiral groove surface; S2. Depositing a transition layer on the surface of the spiral groove: depositing a transition layer on the surface of the spiral groove after decobalting, the depth of the decobalting layer is 50-60 μm, and the cobalt content of the decobalting layer is 1.8-2.2%; S3, spiral polycrystalline diamond layer mixing: weigh a certain amount of superhard powder and a binder, dissolve them in an isopropanol solution and stir them thoroughly in a stirring container; then transfer the stirred materials to a ball mill, add a ball milling medium and grind them repeatedly for 24-30 hours; vacuum dry them after grinding, and finally obtain a uniform spiral polycrystalline diamond layer mixed powder; The superhard powder is one or more of carbon nanotube-coated boron-containing diamond powder, plated cubic boron nitride powder, fullerene-coated boron-containing diamond powder, graphene-coated boron-containing diamond powder, titanium-coated diamond powder, and tungsten-coated diamond powder; S4, spiral composite assembly: the spiral polycrystalline diamond layer mixed powder obtained in S3 is loaded into the spiral groove of the carbide round rod after the transition layer is deposited in S2, compacted and shaped, and then inserted into a high-temperature resistant metal cup to obtain a spiral composite assembly; S5, pre-pressing the spiral composite body: placing the spiral composite body component of S4 into a pre-pressing rubber mold, and maintaining the pressure at 120-150 MPa, thereby obtaining a pre-pressed spiral composite body component; S6, furnace purification: the pre-pressed spiral composite assembly is placed in a vacuum sintering furnace, the furnace is roughly vacuumed, and the temperature is kept at 160-200°C for 1 hour; the vacuum is continued and heated to 850-900°C, hydrogen is filled into the furnace under vacuum conditions until the pressure in the furnace reaches 110-130Mbar, and the furnace is reacted for 4-6 hours before vacuuming again; S7, high temperature and high pressure sintering: assemble the purified spiral composite assembly with the pyrophyllite assembly block, place it in a top press, keep it at a high pressure of 7-9 GPa and a high temperature of 1400-1600°C for 20-30 minutes, stop heating and slowly reduce to normal pressure to obtain a sintered spiral polycrystalline diamond composite round rod blank; S8, stress relief aging: Place the sintered spiral polycrystalline diamond composite round rod blank in a vacuum sintering furnace, heat it to 480-500°C under vacuum conditions and keep it warm for 7-8 hours; evacuate the vacuum again, keep it warm at 580-600°C for 3-4 hours, and naturally cool it to room temperature to obtain the required polycrystalline diamond composite round rod.

7. The method for preparing a spiral polycrystalline diamond composite round rod according to claim 6, characterized in that: In step S2, the transition layer is deposited by physical vapor deposition, with niobium as the target material. The round rod substrate is heated to 800° C. in a nitrogen atmosphere, and sputtering etching is performed at a power of 300 W and a frequency of 120 kHz.

8. Use of the spiral polycrystalline diamond composite round rod as claimed in any one of claims 1 to 5 in the preparation of hole-making tools.